Zinc ion electrolyte ionization state detection membrane and detection method

By preparing a colloidal detection film of aluminum phosphate on the surface of zinc metal, and analyzing the ionization state of zinc ion electrolyte by electrochemical deposition potential changes, the subjectivity and limitations of electrolyte ionization state detection in the prior art are solved, and high sensitivity is achieved and highly selective ionization state detection.

CN119086668APending Publication Date: 2024-12-06QINGDAO UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411222123.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to directly and comprehensively verify the exact ionization state of solutes in electrolytes, resulting in subjective and limited explanation of electrochemical performance and lack of effective detection methods.

Method used

The ionization state in the electrolyte is detected by the difference in adsorption energy between zinc ions in different ionization states, and the change of symmetrical cells and electrochemical deposition potentials are analyzed. Ionization state of solute.

Benefits of technology

It realizes direct, objective and accurate detection of the solute ionization state in zinc ion electrolyte, with high sensitivity and high selectivity, and is suitable for the analysis of various zinc ion-based water electrolytes, reducing the error in traditional detection methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086668A_ABST
    Figure CN119086668A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of energy storage, and particularly relates to a detection membrane and a detection method capable of qualitatively analyzing the ionization degree of an electrolyte, which can directly and effectively detect the ionization state of solute in the electrolyte. The detection film spontaneously forms a film on the surface of zinc metal by using aluminum phosphate colloid, and the ionization degree of the zinc-based electrolyte is detected through the adsorption energy difference between the aluminum phosphate colloid and zinc ions in different ionization states. The qualitative detection method and the evaluation index are as follows: calculating the relative ratio of the average values of the deposition potentials of the detection film-zinc / / detection film-zinc symmetric battery and the zinc / / zinc symmetric battery in the first to 10 cycle periods, and taking the relative ratio as the evaluation index of the ionization degree of the electrolyte solute.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of energy storage, and in particular to an ionization state detection membrane and a detection method for a zinc ion electrolyte. Background Art

[0002] Electrolytes play a vital role in electrochemical reactions and directly affect the process and efficiency of energy storage. The ionization state of the solute in the electrolyte is the core indicator of the electrolyte. It directly determines the migration speed of ions in the electrolyte, the charge transfer resistance of the electrode interface, the solvation and desolvation energy of ions, and the double-layer capacitance structure of the electrode surface, thereby affecting the reaction kinetics and energy efficiency of energy storage and electroplating. Therefore, in a sense, the ionization state of the solute in the electrolyte is the core of the electrolyte properties, and the ion migration rate, charge transfer resistance, solvation and desolvation energy are all manifestations of the ionization state of the solute in the electrolyte.

[0003] In existing research, the ionization state of solutes in electrolytes is usually divided into three types: aggregated ion pairs (AGG), contacted ion pairs (CIP), and free ion pairs (SSIP). Among them, AGG refers to the formation of a relatively tight aggregate of multiple ions and solvent molecules through electrostatic interaction; CIP refers to the state in which positive and negative ions are in direct contact and attract each other through electrostatic force; SSIP means that the ions are completely dissociated and independently dispersed in the solvent. Researchers have tried to explain and illustrate the ionization state of electrolytes through molecular dynamics calculations, Raman spectroscopy, infrared spectroscopy, nuclear magnetic hydrogen spectroscopy and other methods, so as to explain their electrochemical properties. However, these methods are very subjective and limited. At present, there is no method that can directly and comprehensively verify the exact ionization state of solutes in electrolytes, which is still a difficult problem to be solved in the field of electrochemistry.

[0004] In this context, the present invention discloses and develops a detection film and a detection method for the ionization state of a zinc ion electrolyte. The method has a simple preparation method and low cost, and is particularly suitable for the detection and analysis of the ionization state of an aqueous or water-containing zinc ion-based electrolyte. Through this detection method, the ionization state of a solute in an electrolyte can be directly analyzed, avoiding the error caused by subjective speculation in traditional detection means. At the same time, the method of the present invention has high sensitivity, high selectivity and good repeatability, and is suitable for the analysis of various zinc ion-based aqueous electrolytes. Summary of the invention

[0005] The purpose of the present invention is to provide a detection membrane and a detection method that can directly and effectively detect the ionization state of solutes in an electrolyte, so as to make up for the deficiencies in the prior art. Through the detection membrane and the detection method, the ionization state of the solute in the electrolyte can be proved more objectively and accurately, thereby providing a more scientific basis for the analysis and optimization design of the electrolyte. The present invention adopts the following technical solutions:

[0006] The detection membrane of the present invention is prepared by a method in which a special colloid (including but not limited to polyvalent metal phosphates such as aluminum phosphate, calcium phosphate, magnesium phosphate, etc.) can spontaneously form a film on the surface of zinc metal. The different adsorption energies between the phosphate colloid and zinc ions in different ionization states are utilized to detect the ionization states of zinc-containing solutes (including but not limited to zinc sulfate (ZnSO4), zinc trifluoromethanesulfonate (Zn(OTf)2), lithium tetrafluoroborate (Zn(BF4)2), zinc perchlorate (Zn(ClO4)2) and other zinc salts) and their different concentrations and electrolytes formed with different solvents.

[0007] The detection method of the present invention comprises the following steps: first, a detection film is prepared on the surface of zinc foil, and the detection film-Zn (for the convenience of labeling the diagrams, it is uniformly abbreviated as APGZ), a diaphragm and an electrolyte to be tested are assembled into a symmetrical battery. Then, zinc deposition is performed by applying an external voltage, and specific functional groups in the detection film selectively adsorb ions in the electrolyte, resulting in a measurable change in the deposition potential of the metal. Finally, the ionization state of the solute in the electrolyte is evaluated by analyzing the percentage change in the deposition potential when the detection film is present or not. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 The colloids needed to make the detection membrane were found to have Tyndall effect under the laser flashlight.

[0009] Figure 2 for Figure 1 The suspension obtained by mixing the mesocolloid with anhydrous ethanol in a mass ratio of 1:3.

[0010] Figure 3 This is the surface optical photograph of the test film / zinc foil.

[0011] Figure 4 The scanning electron microscope picture of the test film.

[0012] Figure 5 This is the energy spectrometer analysis diagram of the detected film.

[0013] Figure 6 To detect the X-ray diffraction (XRD) pattern of the film.

[0014] Figure 7The symmetric cells of APGZ / / APGZ and Zn / / Zn in 1M ZnSO4 electrolyte at 0.5 mA cm -2 The current density and 1 mAh cm -2 Voltage-time curve when tested under charging capacity conditions.

[0015] Figure 8 The APGZ / / APGZ and Zn / / Zn symmetric cells in 2M ZnSO4 electrolyte at 0.5 mA cm -2 The current density and 1 mAh cm -2 Voltage-time curve when tested under charging capacity conditions.

[0016] Fig. 9 The APGZ / / APGZ and Zn / / Zn symmetric cells in 3M ZnSO4 electrolyte at 0.5 mA cm -2 The current density and 1 mAh cm -2 Voltage-time curve when tested under charging capacity conditions.

[0017] Fig.10 It is an evaluation index for zinc deposition potential and ionization state in ZnSO4 electrolytes with different concentrations.

[0018] Fig.11 The results of the APGZ / / APGZ and Zn / / Zn symmetric cells in 1 M Zn(OTf)2 electrolyte at 0.5 mA cm -2 The current density and 1 mAh cm -2 Voltage-time curve when tested under charging capacity conditions.

[0019] Fig.12 The results are shown in Figure 2 for the symmetric cells of APGZ / / APGZ and Zn / / Zn in 1M Zn(BF4)2 electrolyte at 0.5 mA cm -2 The current density and 1 mAh cm -2 Voltage-time curve when tested under charging capacity conditions.

[0020] Fig.13 The results are shown in Figure 2 for the symmetric cells of APGZ / / APGZ and Zn / / Zn in 1M Zn(ClO4)2 electrolyte at 0.5 mA cm -2 The current density and 1 mAh cm -2 Voltage-time curve when tested under charging capacity conditions.

[0021] Fig.14 It is an evaluation index for zinc deposition potential and ionization state in different electrolytes.

[0022] Fig.15 The APGZ / / APGZ and Zn / / Zn symmetric cells in 1M ZnSO4 / (H2O)1(DMSO)1 electrolyte were tested at 0.5 mA cm -2 The current density and 1 mAh cm -2 Voltage-time curve when tested under charging capacity conditions.

[0023] Fig.16 The APGZ / / APGZ and Zn / / Zn symmetric cells in 1M ZnSO4 / (H2O)3(DMSO)1 electrolyte were tested at 0.5 mA cm -2 The current density and 1 mAh cm -2 Voltage-time curve when tested under charging capacity conditions.

[0024] Fig.17 For 1M ZnSO4 / (H2O) 10 In (DMSO)1 electrolyte, the symmetric cells of APGZ / / APGZ and Zn / / Zn were tested at 0.5 mA cm -2 The current density and 1 mAh cm -2 Voltage-time curve when tested under charging capacity conditions.

[0025] Fig.18 It is an evaluation index of zinc deposition potential and ionization state of 1M ZnSO4 in electrolytes with different proportions of H2O and DMSO as solvents. DETAILED DESCRIPTION

[0026] In zinc-based rechargeable electrochemical energy storage devices, charged zinc ions (electrochemically active ions) are removed from one electrode and transferred to another electrode. The chemical composition of the electrode surface has an important influence on the adsorption and deposition process of zinc ions. Zinc ions in different ionization states in the electrolyte have different charge transfer efficiencies at the electrode / electrolyte interface, which in turn affects energy storage and conversion efficiency. By modifying the electrode surface with phosphate, the strong adsorption properties of phosphate for metal ions are utilized to achieve the purpose of reducing the deposition potential. This method is extremely sensitive to the type, concentration and solvent type of zinc salts and has a strong resolution.

[0027] The present invention provides a method for spontaneously forming a detection film of phosphate on the surface of zinc foil. The method has a simple preparation method, low cost and is suitable for large-area preparation. The binding force of the phosphate film on the surface of the zinc foil is related to the valence state of its metal ions. The higher the valence state, the better the binding force of the detection film. Preferably, the phosphate detection film is aluminum phosphate colloid.

[0028] The aluminum phosphate detection film on the surface of the zinc foil of the present invention is realized by the following technical scheme:

[0029] Preparation step 1: Weigh a certain amount of orthophosphoric acid (H3PO4, 85%), add deionized water to dilute to 60%, and set aside.

[0030] Preparation step 2: Weigh a certain amount of Al(OH)3 powder and add it to the phosphoric acid solution in preparation step 1, where the molar ratio of Al(OH)3 to H3PO4 is 1:3, and stir at 100°C for 3h to obtain a colloid ( Figure 1 ).

[0031] Preparation step 3: Take the colloid obtained in step 1 and anhydrous ethanol in a mass ratio of 1:3 and mix and shake to obtain a modified suspension A ( Figure 2 ).

[0032] Preparation step 4: Cut a 4 cm × 10 cm zinc foil, clean the surface with anhydrous ethanol, and evenly scrape the modified suspension A on the surface of the zinc foil with a 100 μm scraper ( Figure 3 ).

[0033] Preparation step five: keep the zinc foil uniformly coated with the modification liquid A in step four at a constant temperature of 110° C. for 2 hours to obtain a detection film / zinc foil, and take it out for use.

[0034] The obtained detection film was characterized by scanning electron microscope and analyzed by energy dispersive spectrometer to obtain the surface morphology and element distribution of the detection film (see Figure 4 and Figure 5 ).

[0035] The XRD results of the above-obtained detection film showed that the detection film had an amorphous structure (see Figure 6 ).

[0036] The present invention provides a method for detecting the degree of ionization of zinc ions in a zinc-based electrolyte using the detection membrane. The method is as follows:

[0037] Test step 1: Use a cutting machine to cut the obtained APGZ into pieces with a surface area of ​​1.13cm 2 of round pieces.

[0038] Test step 2: Inject 125μL of the electrolyte to be tested onto the diaphragm, and assemble the APGZ disc, glass fiber filter paper diaphragm and detection membrane / zinc foil disc into a CP2032 symmetrical battery. Use the Wuhan Blue Electric CT2001A system to perform constant current charge and discharge tests, and compare with the pure zinc electrode sheet assembled into a CP2032 symmetrical battery. The total amount of zinc involved in the electrochemical reaction should generally be less than 10% of the total mass of the zinc foil. The current density and time of electrochemical deposition are designed according to the mass of the zinc foil used, and the general current density is 0.5~5mA cm -2 The unidirectional electrochemical deposition time is generally 30 minutes to 2 hours.

[0039] Test step three: Calculate the relative ratio of the average values ​​of the deposition potentials of the Zn / / Zn symmetric battery and the APGZ / / APGZ symmetric battery in the 1st to 10th cycles, and use this as an evaluation index for the ionization state of the electrolyte solute.

[0040] The present invention is further described in detail below through specific examples and comparative examples, but it should be understood that these examples are only used for more detailed description and should not be understood as limiting the present invention in any form.

[0041] Example 1 - Different concentrations

[0042] The electrolyte to be tested in test step 2 is 1M ZnSO4: at 0.5mA cm -2 and 1mAh cm -2 Under the test conditions, the average deposition potential of the Zn / / Zn symmetric battery in the 1st to 10th cycle is 0.044V, while the average deposition potential of the APGZ / / APGZ symmetric battery is 0.03V. It can be seen that the detection membrane is conducive to the reduction of the deposition potential, which is derived from the strong adsorption of zinc ions by the surface phosphate functional groups. Through simple calculations, the deposition potential of the Zn / / Zn symmetric battery is 1.47 higher than the deposition potential of the APGZ / / APGZ symmetric battery. The larger the value, the higher the degree of ionization. This is recorded as the evaluation index of the ionization state of 1M ZnSO4 (see Figure 7 ).

[0043] Example 2 - Different concentrations

[0044] The electrolyte to be tested in test step 2 is 2M ZnSO4, and the determination method is the same as in Example 1. It can be concluded that the evaluation index of the ionization state of 2M ZnSO4 is 1.14 (see Figure 8 ).

[0045] Example 3 - Different concentrations

[0046] The electrolyte to be tested in test step 2 is 3M ZnSO4, and the determination method is the same as in Example 1. It can be concluded that the evaluation index of the ionization state of 3M ZnSO4 is 1.11 (see Fig. 9 ).

[0047] From this series of data, it can be seen that the detection membrane can clearly distinguish the ionization state of zinc sulfate at different concentrations. The lower the concentration, the greater the degree of zinc sulfate ionization (see Fig.10 ). In order to reduce the possible errors introduced during the experimental operation, the obtained data are the results of three sets of experiments repeated under the same conditions.

[0048] Example 4—Same concentration, different solutes

[0049] The electrolyte to be tested in Test Step 2 is 1 M Zn(OTf)2, and the measurement method is the same as that in Example 1. The evaluation index of the ionization state of 1 M Zn(OTf)2 is 1.28 (see Fig.11 ).

[0050] Example 5 - Same concentration, different solutes

[0051] The electrolyte to be tested in Test Step 2 is 1 M Zn(BF4)2, and the measurement method is the same as that in Example 1. The evaluation index of the ionization state of 1 M Zn(BF4)2 is 1.33 (see Fig.12 ).

[0052] Example 6 - Same concentration, different solutes

[0053] The electrolyte to be tested in Test Step 2 is 1 M Zn(ClO4)2, and the measurement method is the same as that in Example 1. The evaluation index of the ionization state of 1 M Zn(ClO4)2 is 1.03 (see Fig.13 ).

[0054] Through horizontal comparison, we can see that the ionization state in water is Zn(ClO4)2 < Zn(OTf)2 < Zn(BF4)2 < ZnSO4 (see Fig.14 ). To reduce the possible errors introduced during the experimental operation, all the obtained data are the results of repeating the experiment three times under the same conditions.

[0055] Example 7 - Same concentration, change in solvent composition ratio: 1 M ZnSO4, the solvent is a mixed solution of H2O and dimethyl sulfoxide (DMSO)

[0056] The electrolyte to be tested in Test Step 2 is 1 M ZnSO4, a mixed solution of the solvent H2O and DMSO, where the volume ratio of H2O to DMSO is 1:1, which is abbreviated as 1 M ZnSO4 / (H2O)1(DMSO)1 for convenience. The measurement method is the same as that in Example 1. The evaluation index of the ionization state of 1 M ZnSO4 / (H2O)1(DMSO)1 is 0.56 (see Fig.15 ).

[0057] Example 9 - Same concentration, change in solvent composition ratio: 1 M ZnSO4, the solvent is a mixed solution of H2O and DMSO

[0058] The electrolyte to be tested in test step 2 is a mixed solution of 1M ZnSO4, solvent H2O and DMSO, wherein the volume ratio of H2O to DMSO is 3:1, which is abbreviated as 1MZnSO4 / (H2O)3(DMSO)1 for convenience. The determination method is the same as that in Example 1. It can be concluded that the evaluation index of the ionization state of 1MZnSO4 / (H2O)3(DMSO)1 is 1.04 (see Fig.16 ).

[0059] Example 10—Same concentration, solvent composition ratio changed: 1M ZnSO4, solvent is a mixed solution of H2O and DMSO

[0060] The electrolyte to be tested in test step 2 is a mixed solution of 1M ZnSO4, solvent H2O and DMSO, where the volume ratio of H2O to DMSO is 10:1, which is abbreviated as 1MZnSO4 / (H2O) for convenience. 10 (DMSO) 1. The determination method is the same as in Example 1. It can be obtained that 1MZnSO4 / (H2O) 10 The evaluation index of the ionization state of (DMSO)1 is 1.13 (see Fig.17 ).

[0061] By horizontal comparison, we can see that the ionization state in water is 1M ZnSO4 / (H2O)1(DMSO)1<1M ZnSO4 / (H2O)3(DMSO)1<1M ZnSO4 / (H2O) 10 (DMSO) 1<1M ZnSO4 / H2O (see Fig.18 ). In order to reduce the possible errors introduced during the experimental operation, the obtained data are the results of three sets of experiments repeated under the same conditions.

[0062] The proportion and composition of the solution are not limited to the above embodiments. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.

Claims

1. A membrane for detecting the ionization state of a zinc ion electrolyte, characterized in that: The modified liquid is directly scraped onto the surface of the zinc foil. This process does not require other adhesives. The test film has good adhesion to the zinc foil substrate and has good uniformity.

2. The modification liquid according to claim 1, characterized in that: The phosphate colloid and the dispersed phase solvent are mixed in a mass ratio of 1:

3. The dispersed phase solvent is one of organic solvents with low surface tension such as ethanol, methanol, and ethylene glycol dimethyl ether (DME).

3. The phosphate colloid according to claim 2, characterized in that: One of the water-insoluble multivalent metal phosphates such as aluminum phosphate (AlPO4), calcium phosphate (Ca3(PO4)2), and magnesium phosphate (Mg3(PO4)2).

4. The method for preparing the phosphate colloid according to claim 3 is as follows: weigh a certain amount of metal hydroxide Me(OH) x (Al(OH)3, Ca(OH)2, Mg(OH)3), added to 60% phosphoric acid solution, Me(OH) x The molar ratio of H3PO4 was 1:x, and the mixture was stirred at 100°C for 3 h to obtain phosphate colloid.

5. A method for detecting the degree of ionization of a zinc ion electrolyte using the detection membrane according to claim 1, characterized in that: The detection method is as follows: (1) Use a cutting machine to cut the obtained test film / zinc foil into pieces with a surface area of ​​1.13 cm 2 of round pieces. (2) 125 μL of the electrolyte to be tested was injected onto the diaphragm, and the test membrane-zinc circular sheet, glass fiber filter paper diaphragm and test membrane-zinc circular sheet were assembled into a CP2032 symmetrical battery. The constant current charge and discharge test was carried out using the Wuhan Blue Electric CT2001A system, and compared with the CP2032 symmetrical battery assembled with a pure zinc electrode sheet. (3) Calculate the relative ratio of the average values ​​of the deposition potentials of the zinc / / zinc symmetric battery and the detection membrane-zinc / / detection membrane-zinc symmetric battery in the 1st to 10th cycles, and use this as an evaluation index for the degree of ionization of the electrolyte solute.