Method for evaluating capacity of positive electrode material of aqueous battery and method for improving capacity of positive electrode material of aqueous battery

The electrochemical active area is measured by cyclic voltammetry and the fitting model is combined with the fitting model to quickly evaluate the positive electrode material capacity of the water system battery, and the electrochemical active area is improved by combining liquid phase ultrasonic treatment, which solves the time and time-consuming evaluation of the positive electrode material capacity of the water system battery in the prior art. Accurate problems have achieved capacity improvement and efficiency optimization.

CN119086669APending Publication Date: 2024-12-06TIANJIN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411255728.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing water-based battery positive electrode material capacity evaluation method takes a long time and is inaccurate, and the traditional method cannot truly reflect the electrochemical active area, which makes efficiency optimization difficult.

Method used

The electrochemical active area was measured by cyclic voltammetry, the cathode material capacity was quickly evaluated by fitting the model, and the electrochemical active area was increased by liquid phase ultrasonic treatment, thereby increasing the cathode material capacity.

Benefits of technology

It achieves rapid accuracy and capacity improvement in the capacity evaluation of the positive electrode material capacity of water-based batteries, which consumes less time and is suitable for different positive electrode material systems, providing new ideas for improving the capacity of water-based batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086669A_ABST
    Figure CN119086669A_ABST
Patent Text Reader

Abstract

The invention discloses a method for evaluating the capacity of a positive electrode material of an aqueous battery and a method for improving the capacity of the positive electrode material of the aqueous battery, and the method comprises the following steps: determining the electrochemical active area of a battery assembled by a positive electrode material to be detected, and substituting the electrochemical active area into a capacity-electrochemical active area fitting curve of a corresponding positive electrode material system; compared with a traditional capacity evaluation method, the method has the advantages that the consumed time is shorter, and the prediction and evaluation of the battery capacity are more accurate; according to the improvement method, the water-based battery positive electrode material with the increased electrochemical active area is obtained through liquid-phase ultrasonic treatment, so that the capacity of the water-based battery positive electrode material is improved, the method is universal for different water-based positive electrode material systems, and a new thought is provided for improving the capacity of the water-based battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of aqueous batteries, and in particular to a method for evaluating and improving the capacity of positive electrode materials of aqueous batteries. Background Art

[0002] With the change of global climate and the increasing exhaustion of traditional energy, renewable energy, with wind power and photovoltaic as the core, has developed rapidly. These forms of energy have played a huge role in reducing greenhouse gas emissions, but there is still the problem of unstable supply. In order to meet this challenge, rechargeable batteries are receiving more and more attention as an effective solution strategy. Rechargeable batteries have the advantages of being unaffected by the environment and easy to install. They can be integrated with existing energy infrastructure, further enhancing the flexibility and feasibility of their application.

[0003] Lithium-ion batteries are the most extensively studied battery system and have been widely used in mobile digital products and electric vehicles. However, the organic electrolyte of lithium-ion batteries may cause safety hazards during the charging and discharging process, such as overheating, leakage or fire. In order to solve these safety problems, safer alternative battery technologies are constantly being developed, among which aqueous batteries have attracted more and more attention due to their low cost, high safety, long life and environmental friendliness. Although aqueous batteries have many advantages, they still face some challenges, including low energy density and difficulty in optimizing efficiency. Compared with metal negative electrodes that can be used directly, the development of aqueous batteries focuses more on the improvement of positive electrode materials. Therefore, exploring aqueous battery positive electrodes with high capacity is of great significance for achieving efficient energy storage. The capacity test method of positive electrode materials currently widely used in battery research and development is to perform multiple charge and discharge cycle tests under actual working conditions until the capacity stabilizes. This results in a lot of time required to determine the actual capacity of the battery positive electrode material.

[0004] The electrochemically active area of ​​the positive electrode material of a battery refers to the actual electrochemical reaction area between the positive electrode of the battery and the electrolyte. It is a key parameter for controlling the electrochemical reaction rate in the battery and can reflect the actual capacity of the battery. The existing detection technology uses the BET method to measure the specific surface area of ​​the material. However, not all positive electrode materials inside the battery electrode are in contact with the electrolyte, which makes the specific surface area measured by the BET method larger. Therefore, the BET specific surface area cannot truly reflect the electrochemical area and the actual capacity of the battery. Therefore, drawing on the method of measuring the electrochemically active area in the field of electrocatalysis, the cyclic voltammetry method is used to measure the double-layer capacitance of the positive electrode material of the aqueous battery, thereby obtaining its electrochemically active area. The electrochemically active area obtained by this method is highly correlated with the actual capacity of the battery. Summary of the invention

[0005] In view of the difficulties in the prior art, the present invention proposes a method for evaluating the capacity of aqueous battery positive electrode materials by electrochemically active area, and a method for increasing the capacity of aqueous battery positive electrode materials by increasing the electrochemically active area. The method for evaluating the capacity of aqueous battery positive electrode materials is less time-consuming than traditional capacity evaluation methods and can accurately evaluate the capacity of the battery; the method for increasing the capacity of aqueous battery positive electrode materials is universal for different aqueous positive electrode material systems, providing a new idea for increasing the capacity of aqueous batteries.

[0006] In order to solve the problems of the prior art, the present invention adopts the following technical solutions:

[0007] The present invention provides a method for evaluating and improving the capacity of an aqueous battery positive electrode material.

[0008] In a first aspect, the present invention provides a method for evaluating the capacity of a battery with an aqueous cathode material, wherein the capacity of the cathode material of the battery is evaluated by the electrochemical active area of ​​the battery, comprising the following steps:

[0009] A method for evaluating the capacity of an aqueous battery positive electrode material, the method comprising the following steps:

[0010] Step (101), selecting a battery with the same positive electrode material system as a reference battery, and measuring the capacity and electrochemical active area value of the positive electrode material of the reference battery;

[0011] Step (102), numerically fitting the capacity and electrochemical active area of ​​the reference battery positive electrode material to obtain a capacity-electrochemical active area fitting model;

[0012] Step (103), determining the electrochemical active area value of the positive electrode material of the sample battery to be tested; wherein:

[0013] The method for obtaining the electrochemically active area in step (101) and step (103) comprises performing a cyclic voltammetry test on the battery at a series of scan rates v, calculating the difference Δi between two currents corresponding to the median voltage of the cyclic voltammetry curve at different scan rates; plotting a graph with Δi and v as the horizontal and vertical coordinates, respectively, and performing a linear fit, and obtaining the electrochemically active area value according to the slope of the fitted straight line;

[0014] Step (104), substituting the electrochemically active area value of the sample battery positive electrode material into the capacity-electrochemically active area fitting model of the corresponding material system, and calculating the capacity evaluation result of the sample battery positive electrode material.

[0015] Furthermore, the positive electrode material loading amount in the positive electrode sheet of the reference battery and the sample battery is the same, which is 0.8-1.2 mg / cm 2 .

[0016] Furthermore, the number of cycles of the cyclic voltammetry test at the same scan rate is 3-5 times, and the scan rate range is 0.2-1.0 mV s –1 , the voltage cycle range is 0.1-0.2V.

[0017] The method for evaluating the capacity of an aqueous battery provided by the present invention has the advantage that a capacity-electrochemically active area fitting curve of the corresponding material system can be obtained in advance based on a reference battery of the same positive electrode material system, and then the electrochemically active area of ​​the battery to be tested is brought into the above-mentioned capacity-electrochemically active area fitting curve to obtain the capacity of the positive electrode material of the sample battery. The method for evaluating the capacity of an aqueous battery provided by the present invention is less time-consuming than traditional capacity evaluation methods and is more accurate in predicting and evaluating battery capacity.

[0018] In a second aspect, the present invention provides a method for increasing the capacity of an aqueous battery positive electrode material, characterized in that the electrochemical active area of ​​the battery positive electrode material is increased by liquid phase ultrasonic treatment, comprising the following steps: step (201), grinding the positive electrode material to obtain a corresponding positive electrode material powder;

[0019] Step (202), placing the cathode material powder in a solvent and subjecting it to liquid-phase ultrasonic treatment to obtain a cathode material dispersion;

[0020] Step (203), centrifuging and washing the positive electrode material dispersion to obtain a precipitate;

[0021] Step (204), drying the precipitate to obtain a positive electrode material having an electrochemically active area value.

[0022] Furthermore, the grinding process described in step (201) takes 10-20 minutes.

[0023] Furthermore, the solvent in step (202) is one or more of water, ethanol, N-methylpyrrolidone (NMP), isopropanol, and N,N-dimethylformamide; and the concentration of the positive electrode material dispersion is 0.05-0.12 g / mL.

[0024] Furthermore, the liquid phase ultrasonic treatment in step (203) is carried out under the following conditions: the circulating water temperature is 0-4°C, the ultrasonic time is 4-8 hours, and the ultrasonic power is 70-120W.

[0025] Beneficial Effects

[0026] Compared with the traditional technical solution, the beneficial effect brought by the present invention is: the method for increasing the capacity of the positive electrode material of an aqueous battery provided by the present invention has the advantage of using a simple liquid phase ultrasonic treatment to reduce the particle size of the positive electrode material of the aqueous battery and thereby increase its electrochemical active area, thereby ultimately increasing its capacity. The method for increasing the capacity of the positive electrode material of an aqueous battery is universal for different aqueous positive electrode material systems, and provides a new idea for increasing the capacity of aqueous batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a flow chart of the method for evaluating the capacity of an aqueous battery described in Example 1.

[0028] Figure 2 This is the capacity-electrochemical active area fitting curve described in Example 1.

[0029] Figure 3 This is the cyclic voltammetry test curve of the sample battery described in Example 1, and the inset is the fitting curve of the current difference and the scan rate.

[0030] Figure 4 This is the cycle capacity curve of the sample battery described in Example 1.

[0031] Figure 5 This is a flow chart of the method for increasing the capacity of the positive electrode material of an aqueous battery as described in Example 2.

[0032] Figure 6 This is a scanning electron microscope (SEM) image of the hydrated vanadium oxide described in Example 2.

[0033] Figure 7 This is a scanning electron microscope (SEM) image of the hydrated vanadium oxide material treated by liquid phase ultrasound as described in Example 2.

[0034] Figure 8 The cycle capacity curves are those of an aqueous battery assembled with the hydrated vanadium oxide positive electrode material described in Example 2 and an aqueous battery assembled with the hydrated vanadium oxide positive electrode material treated by liquid phase ultrasound. DETAILED DESCRIPTION

[0035] The following is combined with Figure 1-8 The present invention is described as follows:

[0036] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the following will be described in detail in conjunction with specific embodiments and their accompanying drawings. It should be noted that the embodiments described herein are only used to explain the present application, and are not used to limit the present application.

[0037] Example 1

[0038] According to an embodiment of the present invention, an embodiment of a method for evaluating the capacity of an aqueous battery positive electrode material is provided. Figure 1 is a flow chart of a method for evaluating the capacity of an aqueous battery according to an embodiment of the present invention. Figure 1 As shown, the evaluation method includes the following steps:

[0039] Nine batteries belonging to the same positive electrode material system were prepared as reference batteries (R1-R9), and the reference batteries were subjected to multiple constant current charge and discharge cycles until the battery capacity tended to be stable, thereby obtaining their capacities C1-C9.

[0040] At 0.2, 0.4, 0.6, 0.8 and 1.0mV s –1 The battery (R1-R n ) were subjected to cyclic voltammetry tests and the test was repeated 5 times at each scan rate with a voltage cycle range of 0.1-0.2 V. The difference (Δi) between the two currents corresponding to the median voltage of the cyclic voltammetry curves at different scan rates was calculated, and the ν-Δi curve was linearly fitted. The electrochemical active areas S1-S9 were obtained according to the slope of the fitting straight line.

[0041] The capacity C1-C obtained in step 101 n The electrochemical active area S1-S obtained in step 1-2 n By numerical fitting, the mathematical expression of the aqueous battery capacity-electrochemical active area fitting curve is obtained, such as Figure 2 As shown, its expression is: C = 437.7S + 66.1;

[0042] According to the above steps, the water sample battery R is obtained. * The electrochemical active area S * 0.808mF cm –2 The cyclic voltammetry test curve of the above sample battery and the fitting curve of current difference and scan rate are shown in Figure 3 As shown. * Substitute the obtained mathematical expression of the fitting curve to obtain the capacity evaluation result C of the sample battery. * =419.8 mAh g –1 .

[0043] Furthermore, the sample battery R * Perform multiple constant current charge and discharge cycles until the battery capacity stabilizes and measure R * The actual capacity is 415mAh g –1 ,The relative error with the evaluated capacity is 1.14%, which shows that the prediction and evaluation of battery capacity by this scheme are highly accurate.

[0044] Example 2

[0045] like Figure 5 According to another aspect of the present invention, there is also provided an embodiment of a method for increasing the capacity of an aqueous battery positive electrode material, comprising the following steps:

[0046] Grind the hydrated vanadium oxide positive electrode material V1 for 15 minutes to obtain the corresponding powder;

[0047] The obtained powder was placed in N-methylpyrrolidone (NMP) for liquid phase ultrasonic treatment to obtain a positive electrode material dispersion with a concentration of 0.08 g / mL. The liquid phase ultrasonic treatment conditions were a circulating water temperature of 2°C, an ultrasonic time of 6 hours, and an ultrasonic power of 100W.

[0048] The obtained positive electrode material dispersion was centrifuged at 8000 rpm and washed with anhydrous ethanol to obtain a precipitate.

[0049] The obtained precipitate was vacuum dried at 70°C for 12 h to obtain a hydrated vanadium oxide positive electrode material V2 with an increased electrochemical active area.

[0050] The positive electrode materials with improved electrochemical active area were assembled into aqueous zinc-ion batteries, and the capacity of the aqueous zinc-ion batteries was improved from 415 mAh g –1 Upgraded to 440mAh g –1 .

[0051] Figure 7 This is the SEM image of the hydrated vanadium oxide positive electrode material V1. Figure 8 This is a SEM image of the positive electrode material V2 treated with liquid phase ultrasound. V1 presents a sea urchin-like nanosphere morphology with a diameter of about 10μm, composed of a large number of nanobelts with a width of about 100nm. V2 presents a sheet structure composed of short nanobelts, where the nanobelts are about 100nm wide and 200-500nm long, which matches well with the nanobelts after V1 is broken. This shows that after liquid phase ultrasound treatment, the particle size of the hydrated vanadium oxide positive electrode material is reduced and its electrochemical active area is improved.

[0052] Figure 8 The cycle capacity curves of hydrated vanadium oxide battery and hydrated vanadium oxide battery treated with liquid phase ultrasound. This shows that the capacity of aqueous zinc ion battery with hydrated vanadium oxide as positive electrode material has been improved by liquid phase ultrasound treatment, from 415mAh g –1 Upgraded to 440mAh g –1 .

[0053] Although the present invention has been described above, the present invention is not limited to the above-mentioned specific embodiments. The above-mentioned specific embodiments are merely illustrative and not restrictive. Under the guidance of the present invention, ordinary technicians in this field can make many modifications without departing from the purpose of the present invention, which are all within the protection of the present invention.

Claims

1. A method for evaluating the capacity of an aqueous battery positive electrode material, characterized in that: The method comprises the following steps: Step (101), selecting a battery with the same positive electrode material system as a reference battery, and measuring the capacity and electrochemical active area value of the positive electrode material of the reference battery; Step (102), numerically fitting the capacity and electrochemical active area of ​​the reference battery positive electrode material to obtain a capacity-electrochemical active area fitting model; Step (103), determining the electrochemical active area value of the positive electrode material of the sample battery to be tested; wherein: The method for obtaining the electrochemically active area in step (101) and step (103) comprises performing a cyclic voltammetry test on the battery at a series of scan rates v, calculating the difference Δi between two currents corresponding to the median voltage of the cyclic voltammetry curve at different scan rates; plotting a graph with Δi and v as the horizontal and vertical coordinates, respectively, and performing a linear fit, and obtaining the electrochemically active area value according to the slope of the fitted straight line; Step (104), substituting the electrochemically active area value of the sample battery positive electrode material into the capacity-electrochemically active area fitting model of the corresponding material system, and calculating the capacity evaluation result of the sample battery positive electrode material.

2. The method for evaluating the capacity of an aqueous battery positive electrode material according to claim 1, characterized in that: The positive electrode material loading amount in the positive electrode sheet of the reference battery and the sample battery is the same, which is 0.8-1.2 mg / cm 2 .

3. The method for evaluating the capacity of an aqueous battery positive electrode material according to claim 1, characterized in that: The number of cycles in the cyclic voltammetry test at the same scan rate is 3-5 times, and the scan rate range is 0.2-1.0mV s –1 , the voltage cycle range is 0.1-0.2V.

4. A method for increasing the capacity of an aqueous battery positive electrode material, characterized in that: The method comprises the following steps: Step (201), grinding the positive electrode material to obtain corresponding positive electrode material powder; Step (202), placing the cathode material powder in a solvent and subjecting it to liquid-phase ultrasonic treatment to obtain a cathode material dispersion; Step (203), centrifuging and washing the positive electrode material dispersion to obtain a precipitate; Step (204), drying the precipitate to obtain a positive electrode material having an electrochemically active area value.

5. The method for increasing the capacity of the positive electrode material of an aqueous battery according to claim 4, characterized in that: The grinding process described in step (201) takes 10-20 minutes.

6. The method for increasing the capacity of the positive electrode material of an aqueous battery according to claim 4, characterized in that: The solvent in step (202) is one or more of water, ethanol, N-methylpyrrolidone (NMP), isopropanol, and N,N-dimethylformamide; the concentration of the positive electrode material dispersion is 0.05-0.12 g / mL.

7. The method for increasing the capacity of the positive electrode material of an aqueous battery according to claim 4, characterized in that: The liquid phase ultrasonic treatment in step (203) is carried out under the following conditions: the circulating water temperature is 0-4°C, the ultrasonic time is 4-8 hours, and the ultrasonic power is 70-120W.

Citation Information

Cited By

  • Method for determining specific surface area of NFPP material based on cyclic voltammetry and application thereof

    CN120507262A