Numerical method for determining influence of reduction process on center segregation quantification
By establishing continuous casting flow, solidification heat transfer and mass transfer coupling models and heat-force coupling models, quantitatively evaluating the influence of light/heavy pressure on the center segregation of the casting billet, the high cost of pressure control under pressure in the existing technology and The problem of long cycles has achieved efficient optimization of downward process parameters and quality improvement.
Patent Information
- Application Number
- CN202411224116.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to effectively predict the quantitative impact of light/heavy pressure process on the center segregation of the casting billet through numerical simulation, and the mass transfer simulation process cannot accurately reflect the solute enrichment of the steel liquid reflux caused by underpressure extrusion, resulting in the underpressure process. Parameter regulation costs high and has a long cycle.
By establishing continuous casting flow, solidification heat transfer and mass transfer coupling models, simulating the temperature field and solute distribution of the casting billet, combining the heat-force coupling model, the change of the liquid volume and the central segregation index of the steel core in the casting billet are simulated, and the pressure is calculated. The solute content of the casting blank before and after quantitative evaluation of the effect of the pressure process on central segregation.
Quantitative evaluation of the central segregation index of the continuous casting billet under light/heavy pressure was realized by numerical simulation, simplifying the optimization process of pressurization process parameters, shortening the design and adjustment cycle, reducing costs, and providing a theoretical basis for the continuous casting process. .
Smart Images

Figure CN119089747A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel smelting, and in particular to a numerical method for determining the quantitative influence of a reduction process on central segregation. Background Art
[0002] As one of the main defects of the billet during continuous casting, center segregation is difficult to completely eliminate through subsequent homogenization heat treatment in the heating furnace and rolling, and will eventually be inherited to the rolled material, resulting in insufficient product performance. This problem has become a major factor restricting the high-quality production of continuous casting billets, especially for the production of high-quality special steel. At present, existing studies have shown that solving the center segregation defect of the billet needs to start from the source of the continuous casting solidification process of the molten steel. The main means are: low superheat casting, controlling the appropriate pulling speed, optimizing the specific water volume in the secondary cooling zone, crystallizer and end electromagnetic stirring, and light / heavy pressure reduction process. Among the many methods to reduce the center segregation of the billet, the light / heavy pressure reduction process has been widely used in the production of high-quality continuous casting billets because of its significant improvement effect on the macroscopic segregation and density of the billet. The principle is to apply a certain pressure reduction force at the end of the continuous casting billet to offset the volume shrinkage of the billet. At the same time, the extrusion effect generated by the pressure reduction prompts the molten steel with solute enriched in the liquid core to flow upstream of the billet, so that the solute elements are redistributed in the molten steel, and finally achieve the effect of improving the center segregation and increasing the density of the billet.
[0003] Although the light / heavy reduction process has a significant effect on solving the problem of center segregation of the billet, the key process parameters of the reduction technology (reduction range, reduction amount and reduction rate) need to be optimized and regulated in actual production to achieve the best implementation effect. For example, if the reduction range is too far forward, the solidified billet shell is too thin, and the billet is prone to cracks or even leakage. If the reduction range is too far back, the solidified billet shell is too thick, and the center segregation cannot be improved. To achieve the optimization of the reduction process parameters and achieve the best effect of reducing the center segregation, the center segregation index of the billet after the light / heavy reduction must be obtained as the basis for feedback regulation.
[0004] At present, the most common method in the existing literature to determine the center segregation index of the billet after being pressed down is to take a billet sample at the production site, then obtain a drill cutting sample and perform solute element detection, and finally obtain the center segregation index of the billet; this method can directly measure the center segregation of the actual billet and is more reliable, but the main problem is that the cost is high, the process is cumbersome and the cycle is long, which will lead to a significant lag in the regulation of the on-site pressing process parameters. The results of searching the existing patents involving pressing down and segregation are shown below.
[0005] In the prior art, the patent application number is CN202311517739.5, and the patent name is "Pressure Control Method for Improving Macroscopic and Semi-macroscopic Segregation of High Carbon Low Alloy Steel". It mainly controls the pressure reduction in the continuous casting pressure reduction area by changing the solid phase ratio at the center of the billet. The solid phase ratio at the center of the pressure reduction interval is 0.09-1.0, and the total pressure reduction is 10mm. The total pressure reduction in the continuous casting pressure reduction area corresponding to the central solid phase ratio less than 0.4 is not less than 1mm and not more than 2mm; the patent suppresses the formation of macroscopic segregation and semi-macroscopic point segregation in the equiaxed crystal area by controlling the pressure reduction corresponding to different solid phase ratios of the continuous casting billet. It focuses on the control of the pressure reduction and does not involve the determination of the central segregation index of the billet after pressure reduction.
[0006] The patent application number is CN202310863839.7, and the patent name is "A method for improving the segregation of billet crankshaft steel". For the reduction area of the billet continuous casting machine with full protection casting and constant drawing speed, the maximum reduction rate is determined at a close to critical strain rate in the range of 65%-95% of the solid phase ratio of the billet and used as the reduction rate at the entrance of this area, and then gradually decreases along the direction of the billet drawing; in addition, when the drawing speed increases, the average reduction rate is reduced and the reduction is timely, so as to maximize the use of the reduction effect, avoid the reduction area being too biased towards the liquid phase area and unable to play the role of improving the central segregation, and the reduction area being biased towards the solid phase area is unfavorable to the internal quality of the billet, and finally achieves the purpose of reducing the central segregation. The patent starts with the reduction rate to adjust the reduction parameters and then improve the central segregation, and also does not involve quantitative determination of the impact of reduction on the central segregation.
[0007] The patent application number is CN201910173761.X, and the patent name is "A method for calculating the macro-segregation of thick slabs based on shell bulging and mechanical pressing". It mainly aims at the case where shell bulging occurs in the thick slab during mechanical pressing. The bulging morphology of the ingot is determined through complicated mathematical fitting, and then a macro-segregation calculation model for the thick slab is constructed on this basis and related simulation calculations are performed to study the influence of factors such as the mechanical pressing process parameters at the end of solidification of the thick slab and the asymmetric distribution of the shell bulging of the ingot on the flow and macro-segregation behavior of the enriched solute molten steel. The present invention mainly analyzes the bulging process of thick slabs under pressure, and the universality of the method is limited; the patent studies the segregation caused by bulging suction, not the upstream reflux of enriched molten steel caused by compression, and the mechanism is different; in addition, when determining the bulging morphology, the method is directly calculated and fitted by mathematical formulas based on the reduction amount of each roller. The process is complicated and has a high degree of empiricality, and fails to consider the attenuation effect of the reduction effect transmitted to the core of the ingot under different working conditions; finally, the present invention first determines the bulging morphology of the ingot shell and then performs mass transfer calculations, which is equivalent to simply changing the shape of the geometric model without considering the bulging model and then simulating it, and the suction effect is insufficient. Invention patent CN201910182561.0 provides a method for predicting segregation behavior under heavy pressure in convex roller continuous casting of large square billets. This method is basically consistent with the principle of patent CN201910173761.X, except for the research objects and conditions. It also has the disadvantages of complicated process, strong empiricism, insufficient consideration of the attenuation of pressure reduction effect, and only changing the model geometry when performing mass transfer calculations, which fails to well reflect the mechanism of reflux of solute-enriched molten steel caused by pressure reduction.
[0008] In summary, the following deficiencies exist in the current determination of the influence of light / heavy pressure reduction on the center segregation of the ingot: most of the research on the influence of pressure reduction on the segregation of the ingot focuses on the determination of reasonable pressure reduction parameters and the design of pressure reduction equipment; the existing determination of the quantitative influence of pressure reduction on the center segregation is basically based on sampling and testing at the production site, and there are few predictions through numerical simulation; and the results published on the influence of pressure reduction on the center segregation combined with numerical simulation are cumbersome and difficult to implement, and the mass transfer simulation process cannot well reflect the mechanism that the pressure reduction extrusion causes the reflux of solute-enriched molten steel to improve the center segregation. In view of this, the present invention proposes a numerical method for determining the quantitative influence of the pressure reduction process on the center segregation, which is original. Summary of the invention
[0009] The purpose of the present invention is to provide a numerical method for determining the quantitative influence of the reduction process on the center segregation, to obtain the quantitative change law of the center segregation of the continuous casting billet before and after the application of light / heavy reduction, thereby providing an important basis for the evaluation of the reduction effect, and clarifying the effect of the light / heavy reduction process on the internal quality improvement of the billet during the continuous casting process, and is suitable for the light / heavy reduction process in the continuous casting process of slabs, square billets and round billets.
[0010] To achieve the above object, the present invention is implemented through the following technical solutions:
[0011] A numerical method for determining the quantitative influence of the pressing process on the center segregation, through the continuous casting flow, solidification heat transfer and mass transfer coupling, namely model I, the temperature field, solute distribution and center segregation index of the ingot are simulated, and the temperature field is used as the heat load, and the ingot is pressed down by thermal-mechanical coupling, namely model II, and the volume change of the core molten steel is simulated; based on the solute distribution and the volume change of the core molten steel, the solute content of the ingot at the end of pressing is calculated, and then the solute content of the ingot at the end of pressing is used as the inlet boundary, and the local flow, solidification heat transfer and mass transfer coupling are carried out, namely model III, and the center segregation index when the ingot is completely solidified and the segregation change before and after pressing are simulated.
[0012] Solid fraction f s As the solid-liquid two-phase interface, the volume of the core molten steel before pressing is obtained based on the calculation results of model I, and the volume of the core of the ingot after pressing is obtained using the results of model II. Finally, the change in the volume of the core molten steel is determined, and the formula is as follows:
[0013] ΔV=V0-V1①
[0014] In formula ①, V0 represents the volume of the core molten steel before pressing, V1 represents the volume of the core of the ingot after pressing, and ΔV represents the change in the volume of the core molten steel.
[0015] Based on the solute distribution in model I, the average solute content on the cross section of the ingot before pressing and the average solute volume content in the entire pressing interval are obtained, and then the solute content of the ingot at the end of pressing is obtained by using the volume change of the core molten steel. The formula is as follows:
[0016] W1=W0-ΔV×W average ②
[0017] In formula ②, W0 represents the average solute content on the cross section of the ingot before pressing, and W average It represents the average solute volume content in the entire reduction interval, ΔV represents the volume change of the core molten steel, and W1 represents the solute content of the ingot at the end of reduction.
[0018] Taking the average solute content at the end of pressing as the initial condition, local simulation of continuous casting flow, solidification heat transfer and mass transfer coupling was carried out to obtain the central segregation index when the billet was completely solidified. The quantitative effect of the pressing process on the central segregation of the billet is as follows:
[0019] ΔS=S0-S1 ③
[0020] In formula ③, S1 represents the central segregation index when the ingot is completely solidified, ΔS represents the segregation change before and after pressing, and S0 represents the central segregation index.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. By combining the multi-field coupling mathematical model of flow, solidification heat transfer and mass transfer with the thermal-mechanical coupling finite element mathematical model, the numerical simulation calculation of the center segregation index of the continuous casting billet after light / heavy reduction is realized, which is helpful to quantitatively evaluate the improvement effect of the reduction process on the center segregation, thereby providing technical support for the optimization of the reduction process parameters;
[0023] 2) Based on the center segregation index calculated by simulation, the improvement effect of the reduction process on the quality of the continuous casting billet can be quantitatively evaluated. Compared with the traditional method of determining the influence of the reduction process on the center segregation through industrial experiments, the scheme in the present invention is more convenient and can provide a theoretical basis for the design of the reduction scheme and the regulation of the reduction parameters in the continuous casting process;
[0024] 3) The quantitative influence of light / heavy reduction on center segregation is determined by numerical simulation, which can provide theoretical and technical guidance for the optimization of reduction process parameters. The adoption of the present invention can not only significantly shorten the reduction process design and adjustment cycle, but also reduce industrial tests, thereby saving costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a flow chart for determining the effect of the pressing process on center segregation.
[0026] Figure 2 It is a schematic diagram of the core of the continuous casting billet.
[0027] Figure 3 It is a schematic diagram of the three-dimensional morphology of the molten steel in the core of the ingot. DETAILED DESCRIPTION
[0028] The present invention is described in detail below in conjunction with the accompanying drawings, but it should be noted that the implementation of the present invention is not limited to the following embodiments.
[0029] A numerical method for determining the quantitative effect of the reduction process on the center segregation of the billet during the continuous casting of slabs, square billets and round billets. Based on this method, the change of the center segregation index of the continuous casting billet after applying the light / heavy reduction process can be obtained, and the improvement effect of the reduction process on the billet quality can be evaluated, thereby optimizing the relevant reduction process parameters. The main contents of the invention are:
[0030] 1) For the continuous casting process of slabs, square billets and round billets, including the crystallizer zone, secondary cooling zone and air cooling zone, a flow, solidification heat transfer and mass transfer coupling mathematical model I is constructed. Model I adopts Gong Feng, Shen Jun, Liu Lin and Fu Hengzhi, who published "Combined numerical simulation of flow, heat transfer and mass transfer in directional solidification process - I mathematical model" Progress in Natural Science, Vol. 16, No. 8, August 2006, and other methods can also be used. Based on this simulation, the temperature field and solute element distribution information of the continuous casting billet are obtained, and the central segregation index S0 is calculated; the interval under light / heavy pressure during the continuous casting process is selected to establish a thermal-mechanical coupling finite element model II. Model II adopts Jing Dejun and Cai Kaike, who published "Finite element simulation of thermal-mechanical coupling state in continuous casting crystallizer" Acta Metallurgica Sinica, Vol. 36, No. 4, April 2000, and other methods can also be used. Then the above models are combined. The temperature field obtained in model Ⅰ is loaded as a thermal load into model Ⅱ for thermal-mechanical coupling simulation, and the change in the volume of the molten steel in the core of the ingot before and after the reduction is obtained ΔV; based on this, combined with the solute distribution obtained in model Ⅰ, the solute content W1 on the cross section of the ingot at the end of the reduction can be calculated; W1 is loaded as the inlet boundary into the local mathematical model Ⅲ for the coupling of flow, solidification heat transfer and mass transfer. Model Ⅲ adopts Gong Feng, Shen Jun, Liu Lin, and Fu Hengzhi to publish "Combined numerical simulation of flow, heat transfer and mass transfer in directional solidification process-Ⅰ mathematical model" Progress in Natural Science, Vol. 16, No. 8, August 2006, and other methods can also be used to simulate the distribution of solute elements in the ingot after complete solidification, and calculate the center segregation index S1 of the ingot after reduction, and then subtract it from S0 to clarify the quantitative effect of the reduction process on the center segregation ΔS, see Figure 1 .
[0031] 2) Determination of the volume change of the core steel liquid ΔV, see Figure 2 , with the solid phase rate fs as the solid-liquid two-phase interface; Figure 2 (a) is the core of the continuous casting billet when no pressure is applied. Its three-dimensional morphology can be determined based on the calculation results in model I, such as Figure 3 As shown, based on this, the volume of molten steel V0 is obtained by mathematical integration; Figure 2 (b) is the core of the continuous casting billet after light / heavy reduction. The three-dimensional morphology of the core can be obtained by analyzing the deformation results of the reduction model, and then its volume V1 is obtained by integration using a similar method; finally, the volume change of the core molten steel after the light / heavy reduction process ΔV=V0-V1 can be obtained.
[0032] 3) Determination of the solute content W1 in the liquid separation zone of the cross section of the ingot at the end of pressing, see Figure 2(b) Based on the solute distribution information in Model I, we can know the average content of solute elements in the liquid phase on the cross section of the continuous casting billet before the start of reduction, W0, and the volume average content of solute elements in the liquid phase during the entire reduction interval, Waverage. On this basis, combined with the volume change ΔV obtained in content 2), we can obtain the average content of solute elements in the liquid phase on the cross section at the end of reduction, W1 = W0-ΔV×Waverage.
[0033] 4) Determination of the quantitative effect of the reduction process on the center segregation index ΔS. A local mathematical model III for the coupling of flow, solidification heat transfer and mass transfer is established for the continuous casting billet after the reduction, and W1 determined in content 3) is used as the initial condition of the solute element distribution for simulation. After the billet is completely solidified, the solute distribution information and the center segregation index S1 of the continuous casting billet after the light / heavy reduction process can be obtained, and finally the quantitative effect of the reduction process on the center segregation of the billet ΔS=S0-S1 is obtained.
[0034] The following examples are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following examples. The methods used in the following examples are conventional methods unless otherwise specified.
[0035] [Example 1]
[0036] A numerical method for determining the quantitative effect of the reduction process on center segregation, see Figure 1 , the specific implementation steps are as follows:
[0037] 1) With reference to the actual continuous casting machine structure of slabs, square billets, round billets, etc., a continuous casting flow, solidification heat transfer and mass transfer coupling mathematical model I including the crystallizer zone, secondary cooling zone and air cooling zone was established, and then the steel grade composition and content, thermophysical parameters and related boundary conditions were determined; on this basis, the temperature field and solute element distribution information of the continuous casting billet were simulated and calculated, and the central segregation index S0 without reduction was obtained according to the solute element distribution.
[0038] 2) Select the actual continuous casting machine to apply pressure to the interval to build the continuous casting billet thermal-mechanical coupling finite element model II, see Figure 2 (b) The temperature field of the relevant area obtained in step 1) is loaded into model II as a thermal load, and a thermal-mechanical coupling simulation is performed after determining the high-temperature mechanical properties of the steel grade and applying relevant constraints to obtain the core deformation of the continuous casting billet.
[0039] 3) Solid phase rate f s (value range is 0.7~1) as the solid-liquid two-phase interface, and then determine according to the temperature field in step 1) Figure 2 (a) The core steel liquid area of the ingot, and extract Figure 3The three-dimensional morphology of the core molten steel is obtained, and then its volume V0 when no pressure is applied is calculated; based on the deformation of the continuous casting billet calculated in step 2), a similar method is used to calculate the volume V1 of the core molten steel area of the casting billet after pressure is applied; finally, the two are subtracted to obtain the volume reduction of the central liquid phase area of the continuous casting billet due to pressure ΔV=V0-V1.
[0040] 4) Based on the solute element distribution information in model I, the average solute element content W0 in the liquid phase of the ingot cross section at the beginning of reduction and the volume average solute element content W in the entire reduction interval can be obtained. average ,See Figure 2 (b); Combined with the core molten steel volume reduction ΔV obtained in step 3), the average solute element content in the molten steel area of the cross section of the ingot at the end of the pressing can be obtained: W1 = W0-ΔV×W average .
[0041] 5) A local mathematical model III of flow, solidification heat transfer and mass transfer coupling is constructed for the ingot after the pressing is completed, and the W1 obtained in step 4) is used as the initial distribution condition of the solute element to continue the simulation calculation until the continuous casting ingot is completely solidified, and finally the distribution information of the solute elements after the pressing is applied is obtained, based on which the center segregation index S1 of the ingot after the pressing is obtained.
[0042] 6) Combining the central segregation indexes S0 and S1 of the ingot obtained without and with light / heavy reduction in step 1) and step 5), the quantitative influence of the reduction process on the central segregation ΔS=S0-S1 is obtained; on this basis, the improvement effect of light / heavy reduction on the quality of the continuous casting ingot can be evaluated, thereby carrying out the regulation of the reduction process parameters.
[0043] The present invention is applicable to the light / heavy reduction process of continuous casting of slabs, square billets, round billets and other cross-sectional shapes and sizes, and can quantitatively obtain the influence of the reduction process on the center segregation of the continuous casting billet. In order to obtain the best implementation effect, the following recommendations are made:
[0044] A) Accurately collect relevant parameters
[0045] Geometric parameters:
[0046] Crystallizer length, secondary cooling zone division and length of each zone, air cooling section length, crystallizer cooling water volume, water spray volume in each secondary cooling zone, cooling water temperature.
[0047] Process parameters:
[0048] Continuous casting casting speed V, casting temperature T0.
[0049] Material parameters:
[0050] Steel composition and content, density ρ, specific heat capacity C p , heat transfer coefficient λ, latent heat L f , solid-liquid phase TS With T L , solute element distribution coefficient k, solute diffusion coefficient D, liquation line slope G m , elastic modulus E, Poisson's ratio, expansion coefficient and yield stress-plastic strain.
[0051] B) Based on the continuous casting flow, solidification heat transfer and mass transfer coupling mathematical model, simulation calculation is performed to obtain the temperature field and solute element distribution information of the ingot. Finite volume method is used for numerical simulation. To ensure the feasibility of numerical simulation, the following assumptions are made:
[0052] a) The continuous casting process is regarded as a steady-state process, and the casting speed and superheat remain unchanged;
[0053] b) Ignore the effects of mold vibration, protective slag, taper, and air gap on macrosegregation; ignore the effects of billet curvature;
[0054] c) Simplify the heat transfer process in each zone of secondary cooling, the cooling intensity of the billet in the same cooling zone is considered to be the same, and the comprehensive heat transfer coefficient is used to describe the heat transfer process on the billet surface;
[0055] d) Compared with the latent heat of solidification of steel, the heat released by solid phase transformation is very limited and its influence can be ignored;
[0056] e) Assume local thermodynamic equilibrium during continuous casting solidification.
[0057] The flow and solidification heat and mass transfer model is described by the continuity equation, NS momentum equation, energy equation, Realize k-ε two-equation turbulence model, mass transfer equation and enthalpy-porous model.
[0058] C) Continuous casting slab thermal-mechanical coupling finite element model
[0059] A continuous casting billet thermal-mechanical coupling finite element model is constructed in the pressing interval, and the three-dimensional temperature distribution of the billet obtained in operation B) is loaded into the model as a thermal load for thermal-mechanical coupling simulation. The model makes the following assumptions:
[0060] a) The material is isotropic and uniform, and the mechanical properties are nonlinear;
[0061] b) The Prandtl-Reuss flow increment theory is used to describe the relationship between stress and strain increments in the billet under the plastic yield state;
[0062] c) Use the Von Mises yield criterion to describe the yield of the ingot;
[0063] d) The material satisfies the small deformation theory;
[0064] e) The casting follows the isotropic hardening theory;
[0065] f) Ignore the extension of the ingot in the width direction.
[0066] At the same time, the static pressure of the metal liquid is set on the solid-liquid interface, and the direction is perpendicular to the solid-liquid interface and outward. Finally, the deformation displacement of the continuous casting billet is calculated.
[0067] The present invention combines the multi-field coupling mathematical model of flow, solidification heat transfer and mass transfer with the thermal-mechanical coupling finite element mathematical model to realize the numerical simulation calculation of the center segregation index of the continuous casting billet after light / heavy reduction, which is helpful to quantitatively evaluate the improvement effect of the reduction process on the center segregation, thereby providing technical support for the optimization of the reduction process parameters; based on the center segregation index of the simulation calculation, the improvement effect of the reduction process on the quality of the continuous casting billet can be quantitatively evaluated. Compared with the traditional method of determining the influence of the reduction process on the center segregation through industrial experiments, the scheme in the present invention is more convenient and can provide a theoretical basis for the design of the reduction scheme and the regulation of the reduction parameters in the continuous casting process; the quantitative influence of light / heavy reduction on the center segregation is determined by numerical simulation, which can provide theoretical and technical guidance for the optimization of the reduction process parameters. The use of the present invention can not only significantly shorten the reduction process design and adjustment cycle, but also reduce industrial experiments, thereby saving costs.
Claims
1. A numerical method to determine the quantitative effect of the reduction process on center segregation, It is characterized in that Model I is the coupling of continuous casting flow, solidification heat transfer and mass transfer, which is used to simulate the temperature field, solute distribution and central segregation index of the ingot. The temperature field is used as the heat load, and the thermal-mechanical coupling of the ingot is used to simulate the volume change of the core molten steel. The solute content of the ingot at the end of pressing is calculated based on the solute distribution and the volume change of the core molten steel. Then, the solute content of the ingot at the end of pressing is used as the inlet boundary, and local flow, solidification heat transfer and mass transfer coupling are used to simulate the central segregation index when the ingot is completely solidified and the segregation change before and after pressing.
2. A numerical method for determining the quantitative effect of the reduction process on the center segregation according to claim 1, It is characterized in that Solid fraction f s As the solid-liquid two-phase interface, the volume of the core molten steel before pressing is obtained based on the calculation results of model I, and the volume of the core of the ingot after pressing is obtained using the results of model II. Finally, the change in the volume of the core molten steel is determined, and the formula is as follows: ΔV=V 0 -V 1 ① In formula ①, V 0 Indicates the volume of the core steel liquid when not pressed down, V 1 It represents the volume of the core of the ingot after pressing down, and ΔV represents the volume change of the core molten steel.
3. A numerical method for determining the quantitative effect of the reduction process on the center segregation according to claim 1, It is characterized in that Based on the solute distribution in model I, the average solute content on the cross section of the ingot before pressing and the average solute volume content in the entire pressing interval are obtained, and then the solute content of the ingot at the end of pressing is obtained by using the change in the volume of the core molten steel. The formula is as follows: IN 1 =In 0 -ΔV×W average ② In formula ②, W 0 It represents the average solute content on the cross section of the ingot before pressing down, W average represents the average solute volume content in the entire reduction interval, ΔV represents the volume change of the core steel liquid, and W 1 Indicates the solute content of the billet at the end of pressing.
4. A numerical method for determining the quantitative effect of the reduction process on the center segregation according to claim 1, It is characterized in that Taking the average solute content at the end of pressing as the initial condition, local simulation of continuous casting flow, solidification heat transfer and mass transfer coupling was carried out to obtain the central segregation index when the billet was completely solidified. The quantitative effect of the pressing process on the central segregation of the billet is as follows: ΔS=S 0 -S 1 ③ In formula ③, S 1 It indicates the center segregation index when the ingot is completely solidified, ΔS indicates the change of segregation before and after pressing, S 0 Represents the central segregation index.
Citation Information
Patent Citations
A segregation behavior prediction method for a bloom convex roller under continuous casting heavy pressure
CN109711113A
Thick plate blank macrosegregation calculation method based on blank shell bulging and mechanical pressing
CN109783994A
Pressing method for improving segregation of square billet crankshaft steel
CN116809883A
A method for improving the macro and semi-macro segregation of high carbon low alloy steel by press reduction control
CN117226059B