Electrolytic capacitor anode aluminum foil and preparation method thereof

By using deionized water to clean, dry, pretreat and electrochemical corrosion steps in the preparation process of aluminum foil capacitor anode, combined with microfiltration membrane or ultrafiltration membrane to form uniform corrosion holes, the corrosion holes of aluminum foil capacitors in the prior art are solved. The problems of inhomogeneity and risk of aluminum powder shedding improve the performance and safety of the capacitor.

CN119092304APending Publication Date: 2024-12-06HENAN YUANZHONG EQUIP MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411468750.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing aluminum foil capacitor anode is difficult to ensure the uniformity of the corrosion holes during the acid treatment process, and the risk of aluminum powder falling off is high, which affects the performance and safety of the capacitor.

Method used

Using deionized water to clean, dry, pretreat, coating and electrochemical corrosion steps, uniform corrosion holes are formed through microfiltration membrane, ultrafiltration membrane or nanofiltration membrane to ensure the uniform distribution of corrosion holes on the surface of aluminum foil and electrically Clean before chemical corrosion to remove oil.

Benefits of technology

The uniform distribution of the corrosion holes on the surface of the aluminum foil is achieved, the specific capacitance and stability of the capacitor are improved, the risk of aluminum powder falling off is reduced, and the safety and performance of the capacitor are enhanced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a preparation method of an anode aluminum foil of an electrolytic capacitor. The preparation method comprises the following steps: sequentially carrying out deionized water cleaning, drying, pretreatment, deionized water cleaning, film coating, electrochemical corrosion and film coating removal on a high-voltage corrosion foil with the purity of 99.99%, wherein the conductivity of the deionized water is less than 0.056 uS / cm, and the drying temperature is 50-70 DEG C; the covering film adopts one or more of a microfiltration membrane, an ultrafiltration membrane and a nanofiltration membrane. In the preparation process of the electrolytic capacitor anode aluminum foil, film coating is firstly carried out and then electrochemical corrosion is carried out, so that uniform corrosion holes are formed in the surface of the aluminum foil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aluminum foil production, and in particular to an anode aluminum foil for an electrolytic capacitor and a preparation method thereof. Background Art

[0002] The anode or positive plate of an electrolytic capacitor is made of metal and forms an insulating oxide layer through anodic oxidation, which acts as the dielectric of the capacitor. A solid, liquid or gel electrolyte covers the surface of this oxide layer and serves as the cathode or negative plate of the capacitor. Due to its asymmetric structure, electrolytic capacitors are polarized components, with polarity markings on the device housing, and must always be operated at a higher voltage on the anode than on the cathode, otherwise the dielectric will be damaged and even the capacitor will be damaged, and in severe cases, dangerous situations such as explosion or fire may occur.

[0003] Electrolytic capacitors are widely used for decoupling or noise filtering in power supply and DC link circuits, in variable frequency drives, to couple signals between amplifier stages, and to store energy in flash lamps. Polarized electrolytic capacitors are usually used for power supply filtering, decoupling, signal coupling, time constant setting, and DC isolation in power supply circuits or intermediate frequency and low frequency circuits. Non-polar (bipolar) electrolytic capacitors are usually used in audio frequency divider circuits, TV S correction circuits, and single-phase motor starting circuits.

[0004] In order to meet the needs of electrolytic capacitors, researchers have developed a variety of aluminum foil preparation methods, such as: a sintered aluminum foil capacitor foil and its preparation method disclosed in Chinese patent CN118610004A, a method for manufacturing an electrolytic capacitor anode aluminum foil disclosed in Chinese patent CN101110298A, and a method for manufacturing an electrolytic capacitor anode aluminum foil disclosed in Chinese patent CN101110298A. In the preparation process of electrolytic capacitor aluminum foil, it is often necessary to use acids to treat the surface of the aluminum foil to form etch holes to increase the specific surface area. However, it is difficult to ensure the uniformity of the formation of etch holes by acid treatment of the aluminum foil. Chinese patent CN118610004A coats aluminum powder slurry on the surface of the aluminum foil and then sinters it to form a three-dimensional structure similar to etch holes on the surface of the aluminum foil. However, the risk of aluminum powder falling off is relatively high.

[0005] In order to solve the above problems, people have been seeking an ideal technical solution. Summary of the invention

[0006] The object of the present invention is to provide an electrolytic capacitor anode aluminum foil and a preparation method thereof in view of the deficiencies in the prior art.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is: A method for preparing an anode aluminum foil of an electrolytic capacitor comprises the steps of sequentially performing deionized water cleaning, drying, pretreatment, ionized water cleaning, coating, electrochemical corrosion, and coating removal on a high-voltage corrosion foil with a purity of 99.99%; wherein the conductivity of the deionized water is less than 0.056 uS / cm, and the drying temperature is 50-70°C; and the coating adopts one or more of a microfiltration membrane, an ultrafiltration membrane, and a nanofiltration membrane.

[0008] In the pretreatment step, the high-voltage corrosion foil is immersed in an acid solution with a concentration of 2-10 wt%, and electrochemical corrosion is performed after 30-90 s; wherein the acid solution is one of hydrochloric acid solution, phosphoric acid solution, nitric acid solution, sulfuric acid solution, oxalic acid solution, and hydrofluoric acid solution, or a combination of at least two thereof.

[0009] The electrochemical corrosion step includes pore corrosion, in which the concentration of hydrochloric acid in the pore corrosion solution is 1-3 mol / L, the current density is 0.3-0.7A / cm2, the pore corrosion time is 1-3 min, and the pore corrosion temperature is 70-90°C.

[0010] The electrochemical corrosion step includes hole expansion corrosion, in which the concentration of hydrochloric acid is 1-3 mol / L, the concentration of sulfuric acid is 0.2-1 mol / L, and the current density is 0.1-0.3 A / cm 2 The hole expansion corrosion time is 1-2 min, and the hole expansion corrosion temperature is 40-70℃.

[0011] The amount of corrosive liquid used for pore corrosion is 200-350 kg / m 2 During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid and then the power is turned on.

[0012] The amount of corrosion liquid used for hole expansion corrosion is 150-300 kg / m 2 During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid and then the power is turned on.

[0013] An electrolytic capacitor anode aluminum foil is obtained by the preparation method.

[0014] The present invention has outstanding substantive features and significant progress compared to the prior art. Specifically, the present invention provides an electrolytic capacitor anode aluminum foil. During the preparation process, the aluminum foil is first coated and then electrochemically corroded, so that uniform etch holes are formed on the surface of the aluminum foil. The coating adopts a microfiltration membrane, an ultrafiltration membrane or a nanofiltration membrane, and the distribution of the etch holes is more uniform through the micropores on the coating. In addition, before the electrochemical corrosion, the aluminum foil is also cleaned and pre-treated to remove oil stains on the surface of the aluminum foil. DETAILED DESCRIPTION

[0015] The technical solution of the present invention is further described in detail below through specific implementation methods. Example

[0016] This embodiment provides an electrolytic capacitor anode aluminum foil, which is prepared by the following steps: The steps of deionized water washing, drying, pretreatment, ionized water washing, film coating, electrochemical corrosion, film removal, and deionized water washing are sequentially performed on the high-voltage corrosion foil with a purity of 99.99%; wherein the conductivity of the deionized water is less than 0.056uS / cm, and the drying temperature is 50-70°C; the film coating adopts one or more of microfiltration membrane, ultrafiltration membrane, and nanofiltration membrane. It should be noted that the film coating refers to covering the surface of the aluminum foil with a microfiltration membrane, an ultrafiltration membrane, or a nanofiltration membrane, and completely fitting the aluminum foil, and then electrochemically corroding. During the electrochemical corrosion process, the electrolyte contacts the surface of the aluminum foil after passing through the microfiltration membrane, the ultrafiltration membrane, or the nanofiltration membrane, and does not directly drip on the surface of the aluminum foil to contact the aluminum foil. After removing the film and washing, the steps of aluminum foil formation and post-treatment are performed to complete the preparation of the aluminum foil. The aluminum foil formation and post-treatment adopt the existing technology (for example: the manufacturing method of electrolytic capacitor anode aluminum foil disclosed in Chinese patent CN101110298A), which will not be repeated.

[0017] In the pretreatment step, the high-voltage corrosion foil is immersed in an acid solution with a concentration of 2-10 wt%, and electrochemical corrosion is performed after 30-90 s; wherein the acid solution is one of hydrochloric acid solution, phosphoric acid solution, nitric acid solution, sulfuric acid solution, oxalic acid solution, and hydrofluoric acid solution, or a combination of at least two thereof.

[0018] The electrochemical corrosion step includes pore corrosion, in which the concentration of hydrochloric acid in the pore corrosion solution is 1-3 mol / L, the current density is 0.3-0.7A / cm2, the pore corrosion time is 1-3 min, and the pore corrosion temperature is 70-90°C; the amount of pore corrosion solution is 200-350 kg / m 2 During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid and then the power is turned on.

[0019] The electrochemical corrosion step includes hole expansion corrosion, in which the concentration of hydrochloric acid is 1-3 mol / L, the concentration of sulfuric acid is 0.2-1 mol / L, and the current density is 0.1-0.3 A / cm 2 The hole expansion corrosion time is 1-2 min, the hole expansion corrosion temperature is 40-70℃; the amount of corrosion liquid for hole expansion corrosion is 150-300kg / m 2 During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid and then the power is turned on.

[0020] Example 1 This embodiment provides an electrolytic capacitor anode aluminum foil, which is prepared by the following steps: The steps of deionized water cleaning, drying, pretreatment, deionized water cleaning, coating, electrochemical corrosion, coating removal and deionized water cleaning are sequentially performed on a high-voltage corrosion foil with a purity of 99.99% to obtain a corrosion aluminum foil; wherein the conductivity of the deionized water is less than 0.056 uS / cm, and the drying temperature is 50-70°C; the coating adopts an ultrafiltration membrane with a pore size of 0.01 micron, and the ultrafiltration membrane can be made of acid-resistant materials, such as: polyolefin.

[0021] In the pretreatment step, the high-voltage corrosion foil is immersed in an acid solution with a concentration of 6 wt %, and then electrochemically corroded after immersion for 80 seconds; wherein the acid solution is an aqueous solution of 6 wt % sulfuric acid and 6 wt % nitric acid.

[0022] The electrochemical corrosion process includes pore corrosion, in which the concentration of hydrochloric acid in the pore corrosion solution is 2 mol / L, the current density is 0.5 A / cm2, the pore corrosion time is 1.5 min, and the pore corrosion temperature is 80°C; the amount of pore corrosion solution is 220 kg / m 2 During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid, and then the power is turned on, and the corrosion liquid is sprayed with a nozzle.

[0023] The electrochemical corrosion process includes hole expansion corrosion, in which the concentration of hydrochloric acid is 2.5 mol / L, the concentration of sulfuric acid is 0.6 mol / L, and the current density is 0.25 A / cm 2 The hole expansion corrosion time is 1 min, the hole expansion corrosion temperature is 50℃, and the amount of corrosion liquid for hole expansion corrosion is 280 kg / m 2 During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid, and then the power is turned on, and the corrosion liquid is sprayed with a nozzle.

[0024] After testing, the specific capacitance of the corroded aluminum foil is 2.42×10 -4 F / cm 2 . Comparative Example The present embodiment provides an electrolytic capacitor anode aluminum foil, which is prepared by the following steps: sequentially subjecting a high-voltage corrosion foil with a purity of 99.99% to the steps of deionized water cleaning, drying, pretreatment, ionized water cleaning, and electrochemical corrosion to obtain the corrosion aluminum foil; wherein the conductivity of the deionized water is less than 0.056 uS / cm, and the drying temperature is 50-70°C.

[0025] In the pretreatment step, the high-voltage corrosion foil is immersed in an acid solution with a concentration of 6 wt %, and then electrochemically corroded after immersion for 80 seconds; wherein the acid solution is an aqueous solution of 6 wt % sulfuric acid and 6 wt % nitric acid.

[0026] The electrochemical corrosion process includes pore corrosion, in which the concentration of hydrochloric acid in the pore corrosion solution is 2 mol / L, the current density is 0.5 A / cm2, the pore corrosion time is 1.5 min, and the pore corrosion temperature is 80°C; the amount of pore corrosion solution is 220 kg / m 2 .

[0027] The electrochemical corrosion process includes hole expansion corrosion, in which the concentration of hydrochloric acid is 2.5 mol / L, the concentration of sulfuric acid is 0.6 mol / L, and the current density is 0.25 A / cm 2 The hole expansion corrosion time is 1 min, the hole expansion corrosion temperature is 50℃, and the amount of corrosion liquid for hole expansion corrosion is 280 kg / m 2 .

[0028] After testing, the specific capacitance of the corroded aluminum foil is 1.62×10 -4 F / cm 2 . Example 2 This embodiment provides an electrolytic capacitor anode aluminum foil, which is prepared by the following steps: The steps of deionized water cleaning, drying, pretreatment, deionized water cleaning, coating, electrochemical corrosion, coating removal and deionized water cleaning are sequentially performed on a high-voltage corrosion foil with a purity of 99.99% to obtain a corrosion aluminum foil; wherein the conductivity of the deionized water is less than 0.056 uS / cm, the drying temperature is 50-70°C; and the coating adopts an ultrafiltration membrane with a pore size of 0.02 microns.

[0029] In the pretreatment step, the high voltage corrosion foil is immersed in an acid solution with a concentration of 6 wt %, and then electrochemically etched after immersion for 90 s; wherein the acid solution is an aqueous solution of 6 wt % sulfuric acid and 6 wt % nitric acid.

[0030] The electrochemical corrosion steps include pore corrosion, in which the concentration of hydrochloric acid in the pore corrosion solution is 2 mol / L, the current density is 0.5 A / cm2, the pore corrosion time is 1.5 min, and the pore corrosion temperature is 70 °C; the amount of pore corrosion solution is 200 kg / m 2 During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid and then the power is turned on.

[0031] The electrochemical corrosion process includes hole expansion corrosion, in which the concentration of hydrochloric acid is 2.5 mol / L, the concentration of sulfuric acid is 0.8 mol / L, and the current density is 0.25 A / cm 2 The hole expansion corrosion time is 1.5 min, the hole expansion corrosion temperature is 60℃, and the amount of corrosion liquid for hole expansion corrosion is 300 kg / m 2During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid and then the power is turned on.

[0032] After testing, the specific capacitance of the corroded aluminum foil is 2.35×10 -4 F / cm 2 . Example 3 This embodiment provides an electrolytic capacitor anode aluminum foil, which is prepared by the following steps: The steps of deionized water cleaning, drying, pretreatment, deionized water cleaning, coating, electrochemical corrosion, coating removal and deionized water cleaning are sequentially performed on a high-voltage corrosion foil with a purity of 99.99% to obtain a corrosion aluminum foil; wherein the conductivity of the deionized water is less than 0.056 uS / cm, the drying temperature is 50-70°C; and the coating adopts an ultrafiltration membrane with a pore size of 0.008 microns.

[0033] In the pretreatment step, the high-voltage corrosion foil is immersed in an acid solution with a concentration of 10 wt%, and electrochemical corrosion is performed after 50 s; wherein the acid solution is an aqueous solution of 10 wt% sulfuric acid and 10 wt% nitric acid.

[0034] The electrochemical corrosion steps include pore corrosion, in which the concentration of hydrochloric acid in the pore corrosion solution is 2 mol / L, the current density is 0.6 A / cm2, the pore corrosion time is 80 s, and the pore corrosion temperature is 80°C; the amount of pore corrosion solution is 250 kg / m 2 During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid and then the power is turned on.

[0035] The electrochemical corrosion step includes hole expansion corrosion. In the hole expansion corrosion solution, the concentration of hydrochloric acid is 2.5 mol / L, the concentration of sulfuric acid is 0.5 mol / L, and the current density is 0.25 A / cm 2 The hole expansion corrosion time is 2 min, the hole expansion corrosion temperature is 50℃, and the amount of corrosion liquid for hole expansion corrosion is 250 kg / m 2 During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid and then the power is turned on.

[0036] After testing, the specific capacitance of the corroded aluminum foil is 2.18×10 -4 F / cm 2 . Performance Testing The corroded aluminum foil obtained in Example 1 and the comparative example was subjected to an alternating current impedance (EIS) test using an RST5200 electrochemical workstation. The electrolyte solution used in the test was a potassium sulfate solution with a concentration of 0.5 mol / L, and the experimental temperature was room temperature. The alternating current impedance spectrum can be finally obtained through the alternating current impedance test, and the specific capacitance can be calculated based on the curve. The experiment adopted an open circuit potential, the test time was 10 min, the initial frequency of the tested frequency was 100 KHz, the termination frequency was 10 mHz, and the scanning speed was 20 m / s. During the test, the corroded aluminum foil was sealed with 704 silicone rubber, and the area in direct contact with the solution after sealing was 1 cm 2 .

[0037] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.

Claims

1. A method for preparing an anode aluminum foil for an electrolytic capacitor, comprising the steps of sequentially washing a high-voltage corrosion foil with a purity of 99.99% with deionized water, drying, pre-treatment, washing with ionized water, coating, electrochemical corrosion, and removing the coating; wherein: The conductivity of deionized water is less than 0.056 uS / cm, and the drying temperature is 50-70°C; the coating adopts one or more of microfiltration membrane, ultrafiltration membrane and nanofiltration membrane.

2. The preparation method according to claim 1, characterized in that: In the pretreatment step, the high-voltage corrosion foil is immersed in an acid solution with a concentration of 2-10wt% for 30-150s, and then coated for electrochemical corrosion; wherein the acid solution is one of hydrochloric acid solution, phosphoric acid solution, nitric acid solution, sulfuric acid solution, oxalic acid solution, and hydrofluoric acid solution, or a combination of at least two thereof.

3. The preparation method according to claim 2, characterized in that: The electrochemical corrosion process includes pore corrosion, in which the concentration of hydrochloric acid in the pore corrosion solution is 1-3 mol / L and the current density is 0.3-0.7A / cm 2 The pore corrosion time is 1-3 min, and the pore corrosion temperature is 70-90℃.

4. The preparation method according to claim 3, characterized in that: The electrochemical corrosion step includes hole expansion corrosion, in which the concentration of hydrochloric acid is 1-3 mol / L, the concentration of sulfuric acid is 0.2-1 mol / L, and the current density is 0.1-0.3 A / cm 2 The hole expansion corrosion time is 1-2 min, and the hole expansion corrosion temperature is 40-70℃.

5. The preparation method according to claim 4, characterized in that: The amount of corrosive liquid used for pore corrosion is 200-350kg / m 2 During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid and then the power is turned on.

6. The preparation method according to claim 5, characterized in that: The amount of corrosion liquid for hole expansion corrosion is 150-300kg / m 2 During the hole expansion corrosion process, the coating is first moistened with the corrosion liquid and then the power is turned on.

7. An electrolytic capacitor anode aluminum foil, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 6.