Surface treatment method for collector electrode with low secondary electron emission coefficient

Through the mechanical processing and surface treatment technology of graphite-doped metal materials, the secondary electron emission coefficient of the high-power millimeter wave traveling wave tube collection pole is reduced, solving the problem of limited efficiency improvement in the existing technology, and achieving efficient collection Extreme design, suitable for engineering applications.

CN119092387AActive Publication Date: 2024-12-06NANJING SANLE GROUP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411081315.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-12-06
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The secondary electron emission coefficient of the high-power millimeter wave traveling wave tube collector is too large, resulting in limited improvement in the efficiency of the entire tube. The existing surface modification technology is unstable and costly, making it difficult to apply in engineering.

Method used

Graphite-doped metal materials are used, and the collector electrode with low secondary electron emission coefficient is formed through mechanical processing, acetone ultrasonic cleaning, hydrogen calcination purification, copper plating treatment and vacuum heat treatment.

Benefits of technology

It significantly reduces the generation of secondary electrons during the traveling wave tube operation, improves the efficiency of the collector, meets the load requirements of the radar system, and improves the welding quality and vacuum degree.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092387A_ABST
    Figure CN119092387A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of collector electrode surface treatment, and provides a low secondary electron emission coefficient collector electrode surface treatment method which comprises the following steps: processing graphite doped metal into a collector electrode part in a machining manner; removing residual impurities on the surface of the machined collector electrode part by adopting an acetone ultrasonic cleaning mode; carrying out hydrogen burning purification treatment on the collector electrode part; carrying out copper plating treatment on a welding area of the graphite-doped metal material; a low-vapor-pressure gold-based alloy brazing filler metal for an electric vacuum device is adopted as a filling solder to assemble a collector; compared with a collector electrode prepared from oxygen-free copper in the prior art, the novel light material graphite doped metal is adopted, the secondary electron emission coefficient and the weight of the electrode are reduced, and through local copper plating and vacuum heat treatment on a graphite doped metal collector electrode part, the electrode has the advantages that the electrode is simple in structure and convenient to operate. The connection between the collector electrode lead and the collector electrode is realized, and the power-up requirement of each electrode of the collector is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of collector electrode surface treatment, in particular to a method for treating the surface of a collector electrode with a low secondary electron emission coefficient. Background Art

[0002] High-power millimeter-wave traveling wave tubes are indispensable core components in high-precision millimeter-wave radar systems. They have the function of microwave power amplification. The radar system has very high requirements for the efficiency of the traveling wave tube and the quality of the signal. The efficiency directly affects the load of the radar system. The collector is an important component for collecting the remaining electrons in the traveling wave tube. Therefore, improving the collector efficiency is extremely critical.

[0003] like Figure 1 As shown, under the condition that the collector structure design is determined, to obtain a high-efficiency collector, it is necessary to start from the material and process perspectives, by selecting materials with small secondary electron emission coefficients as collector electrodes, or modifying the electrode surface. However, the current problems with surface modification technology are that the process is relatively unstable and the processing cost is expensive, which is not conducive to engineering applications. Therefore, directly changing the material is the most direct and effective way to improve the recovery efficiency. Therefore, the present invention proposes a surface treatment method for a collector electrode with a low secondary electron emission coefficient, which can significantly reduce the secondary electrons generated during the operation of the traveling wave tube. Under the premise of meeting the requirements of good processing performance, low outgassing and high welding quality of thin-walled collector electrodes, the collector efficiency is improved and the weight of the entire tube is reduced, meeting the requirements of the radar system for the load of a high-power millimeter-wave traveling wave tube. Summary of the invention

[0004] The present invention provides a surface treatment method for a collector electrode with a low secondary electron emission coefficient, and studies a matching surface treatment method to meet the welding requirements of collector parts, so as to solve the problem in the background technology that the secondary emission coefficient of the collector electrode of a high-power millimeter-wave traveling wave tube made of oxygen-free copper is too large, resulting in limited improvement in the efficiency of the entire tube.

[0005] The technical solution of the present invention is as follows:

[0006] A method for treating the surface of a collector electrode with a low secondary electron emission coefficient comprises the following steps:

[0007] S1: Processing graphite-doped metal into collector electrode parts by mechanical processing;

[0008] S2: Use acetone ultrasonic cleaning to remove the debris or particles remaining on the surface of the collector electrode parts after processing;

[0009] S3: Maintain the collector electrode parts at 700°C for 10 minutes to perform hydrogen burning purification treatment;

[0010] S4: copper plating is performed on the welding area of ​​the graphite-doped metal material, and then the welding area is kept at 900°C-950°C in a vacuum furnace for 20 minutes;

[0011] S5: Use electric vacuum devices and use low vapor pressure gold-based alloy solder as filler solder to assemble the collector, and weld it into the collector component in a vacuum furnace.

[0012] Preferably, the graphite in the graphite-doped metal in S1 accounts for 80%-90%.

[0013] Preferably, the machining methods in S1 include turning, washing, grinding and electric spark machining.

[0014] Preferably, alcohol is used as the coolant during the machining in S1.

[0015] Preferably, the vacuum degree in the vacuum furnace in S4 and S5 shall not be less than 10 -4 Pa.

[0016] Preferably, the copper layer in S4 has a thickness of 7-8 μm.

[0017] Preferably, the gold-based alloy solder in S5 includes Au-Cu and Au-Ni.

[0018] Preferably, the Au-Cu welding temperature is 910-930° C., the Au-Ni welding temperature is 950-1000° C., and the heating rate is 10° C. / min.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention adopts a lightweight new material graphite doped with metal, and compared with the collector electrode prepared by oxygen-free copper in the past, the secondary electron emission coefficient and weight of the electrode itself are reduced, and alcohol is used as a coolant; through processes such as lathe processing and acetone ultrasonic cleaning, while meeting the processing accuracy of the collector electrode, the serious degassing problem of the material in the later stage caused by improper processing technology is effectively solved, which is helpful to improve the vacuum degree in the traveling wave tube and improve the consistency of electrical parameters such as spiral current.

[0021] 2. The present invention improves the bonding strength between the copper-plated layer and the graphite-doped metal matrix, improves the wetting performance of the solder on the graphite-doped metal surface, realizes the connection between the collector electrode lead and the collector electrode, and meets the power-on requirements of each collector electrode by locally plating copper on the graphite-doped metal collector electrode parts and performing vacuum heat treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a structural diagram of the collector of the present invention;

[0023] Figure 2 This is a physical picture of the graphite-doped metal collector electrode of the present invention;

[0024] Figure 3 This is a physical picture of the graphite-doped metal collector electrode of the present invention;

[0025] Figure 4 Detailed description of the invention The present invention is a flow chart of the surface treatment method. DETAILED DESCRIPTION

[0026] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0027] Embodiment 1:

[0028] A method for treating the surface of a collector electrode with a low secondary electron emission coefficient comprises the following steps:

[0029] S1: Graphite-doped metal with a graphite content of 80% is processed into the required collector electrode parts by turning, washing, grinding, and electrospark machining. In order to meet the vacuum hygiene requirements of the traveling wave tube, the collector electrode parts are processed by mechanical processing using alcohol as the coolant to avoid problems such as collector electrode degassing caused by the inability to completely remove the coolant residue;

[0030] S2: Use acetone ultrasonic cleaning to remove the debris or particles remaining on the surface of the collector electrode parts after processing, so as to avoid the formation of excess materials after assembling the whole tube, which may cause the traveling wave tube to ignite.

[0031] S3: In order to remove the copper oxide on the surface of the parts during processing, the collector electrode parts are placed in a sealed container, high-purity hydrogen is introduced into the container and heated, and maintained at 700°C for 10 minutes; the processed collector electrode is as follows Figure 2 As shown;

[0032] S4: In order to meet the requirements of different voltages for each electrode, it is necessary to weld external leads to the collector electrode. In order to achieve reliable welding of graphite-doped metal, a copper plate is used as the cathode and the welding area of ​​graphite-doped metal is used as the anode. At a potential of 0.5V and 1.5-2.5A / cm 2 Under the current density, copper ions are reduced from the electrolyte by electrolysis reaction and deposited on the graphite surface to a copper layer thickness of 7 μm. Then, the vacuum degree shall not be less than 10 -4 The Pa vacuum furnace is used for 20 minutes of heat preservation at 900℃-950℃, which not only improves the bonding strength between the copper layer and the graphite-doped metal matrix, but also effectively removes the residual gas molecules inside the material.

[0033] S5: Use low vapor pressure gold-based alloy solder (Au-Cu or Au-Ni) as filler solder to fix the predetermined position on the collector of the electric vacuum device, and then put it into a vacuum furnace and keep it at a temperature not less than 10 -4 Pa vacuum, and keep the temperature at 910-930℃ or 950-1000℃, while increasing the temperature at a heating rate of 10℃ / min, and keep the temperature constant when the gold-based alloy solder melts, so that the gold-based alloy solder and the collector component are fully combined; the collector electrode assembly brazed with gold-based solder wire is as follows Figure 3 shown.

[0034] Embodiment 2:

[0035] S1: The graphite-doped metal with a graphite content of 85% is processed into the required collector electrode parts by turning, washing, grinding, and electrospark machining. In order to meet the vacuum hygiene requirements of the traveling wave tube, the collector electrode parts are processed by mechanical processing using alcohol as the coolant to avoid problems such as collector electrode degassing caused by the inability to completely remove the coolant residue;

[0036] S2: Use acetone ultrasonic cleaning to remove the debris or particles remaining on the surface of the collector electrode parts after processing, so as to avoid the formation of excess materials after assembling the whole tube, which may cause problems such as sparking of the traveling wave tube;

[0037] S3: In order to remove the copper oxide on the surface of the parts during processing, the collector electrode parts are placed in a sealed container, high-purity hydrogen is introduced into the container and heated, and maintained at 700°C for 10 minutes; the processed collector electrode is as follows Figure 2 As shown;

[0038] S4: In order to meet the requirements of different voltages for each electrode, it is necessary to weld external leads to the collector electrode. In order to achieve reliable welding of graphite-doped metal, a copper plate is used as the cathode and the welding area of ​​graphite-doped metal is used as the anode. At a potential of 0.5V and 1.5-2.5A / cm 2 Under the current density, copper ions are reduced from the electrolyte by electrolysis reaction and deposited on the graphite surface to a copper layer thickness of 7.5 μm. Then, the vacuum degree shall not be less than 10 -4 The Pa vacuum furnace is used for 20 minutes of heat preservation at 900℃-950℃, which not only improves the bonding strength between the copper layer and the graphite-doped metal matrix, but also effectively removes the residual gas molecules inside the material.

[0039] S5: Use low vapor pressure gold-based alloy solder (Au-Cu or Au-Ni) as filler solder to fix the predetermined position on the collector of the electric vacuum device, and then put it into a vacuum furnace and keep it at a temperature not less than 10 -4Pa vacuum, and keep the temperature at 910-930℃ or 950-1000℃, while increasing the temperature at a heating rate of 10℃ / min, and keep the temperature constant when the gold-based alloy solder melts, so that the gold-based alloy solder and the collector component are fully combined; the collector electrode assembly brazed with gold-based solder wire is as follows Figure 3 shown.

[0040] Embodiment three:

[0041] A method for treating the surface of a collector electrode with a low secondary electron emission coefficient comprises the following steps:

[0042] S1: The graphite-doped metal with a graphite content of 90% is processed into the required collector electrode parts by turning, washing, grinding, and electrospark machining. In order to meet the vacuum hygiene requirements of the traveling wave tube, the collector electrode parts are processed by mechanical processing using alcohol as the coolant to avoid problems such as collector electrode degassing caused by the inability to completely remove the coolant residue;

[0043] S2: Use acetone ultrasonic cleaning to remove the debris or particles remaining on the surface of the collector electrode parts after processing, so as to avoid the formation of excess materials after assembling the whole tube, which may cause problems such as sparking of the traveling wave tube;

[0044] S3: In order to remove the copper oxide on the surface of the parts during processing, the collector electrode parts are placed in a sealed container, high-purity hydrogen is introduced into the container and heated, and maintained at 700°C for 10 minutes; the processed collector electrode is as follows Figure 2 As shown;

[0045] S4: In order to meet the requirements of different voltages for each electrode, it is necessary to weld external leads to the collector electrode. In order to achieve reliable welding of graphite-doped metal, a copper plate is used as the cathode and the welding area of ​​graphite-doped metal is used as the anode. At a potential of 0.5V and 1.5-2.5A / cm 2 Under the current density, copper ions are reduced from the electrolyte by electrolysis reaction and deposited on the graphite surface to a copper layer thickness of 8 μm. Then, the vacuum degree shall not be less than 10 -4 The Pa vacuum furnace is used for 20 minutes of heat preservation at 900℃-950℃, which not only improves the bonding strength between the copper layer and the graphite-doped metal matrix, but also effectively removes the residual gas molecules inside the material.

[0046] S5: Use low vapor pressure gold-based alloy solder (Au-Cu or Au-Ni) as filler solder to fix the predetermined position on the collector of the electric vacuum device, and then put it into a vacuum furnace and keep it at a temperature not less than 10 -4Pa vacuum, and keep the temperature at 910-930℃ or 950-1000℃, while increasing the temperature at a heating rate of 10℃ / min, and keep the temperature constant when the gold-based alloy solder melts, so that the gold-based alloy solder and the collector component are fully combined; the collector electrode assembly brazed with gold-based solder wire is as follows Figure 3 shown.

[0047] Comparative Example 1:

[0048] S1: Processing of multi-level common pressed graphite substrates as required;

[0049] S2: Use ordinary pressed graphite material to process a masking fixture to block the area where the pyrolytic graphite coating does not need to be deposited;

[0050] S3: Install the shielding fixture on each graphite substrate and deposit a pyrolytic graphite coating with a coating thickness of 10-50 μm;

[0051] S4: metallizing the graphite composite electrode obtained in step S3: shielding the area on the electrode where the pyrolytic graphite coating is deposited with a stainless steel shielding fixture, and performing vacuum ion titanium plating treatment, wherein the thickness of the titanium layer is controlled to be 5-15 μm;

[0052] S5: Metallization of the welding surface of the insulating porcelain parts: Use the conventional high-temperature molybdenum-manganese method for metallization process, and then nickel-plated and hydrogen-burned on the surface;

[0053] S6: welding;

[0054] S7: After assembling multiple graphite composite electrode units obtained in S6 in axial order, they are sleeved with oxygen-free copper or monel sleeves and put into a furnace for welding; after solidification, they are naturally cooled to obtain a finished product.

[0055] By conducting secondary emission coefficient measurement experiments on Examples 1 and 2 and Comparative Examples 1 and 2:

[0056] S1: Preparation

[0057] Place the sample to be tested between the collecting plates, ensure that the sample surface is clean and free of contamination, and adjust the electron gun to emit a stable high-energy electron beam;

[0058] S2: Measure the incident electron beam current

[0059] Without placing the sample to be tested, let the electron beam pass through the collecting plate and enter the Faraday cup. Use an ammeter to measure the current formed by the electron beam entering the Faraday cup, which is recorded as I injection current.

[0060] S3: Measuring background current

[0061] The collecting plate is short-circuited, and a voltage of 50V is applied between the sample to be tested and the collecting plate to prevent the secondary electrons from escaping the sample to be tested. At this time, the current between the sample to be tested and the collecting plate is measured. This current is mainly composed of background current (such as instrument noise, leakage current, etc.), which is recorded as I1. Ignoring the slight changes in the background current, it can be considered that I1≈I BG (background current);

[0062] S4: Measuring secondary electron current

[0063] Keep the collecting plate short-circuited, but apply a voltage of 20V between the first collecting plate and the sample to be tested. At this time, the secondary electrons emitted by the sample to be tested are collected by the collecting plate to form a secondary electron current. Use an ammeter to measure the current between the first collecting plate and the sample to be tested, recorded as I2, which includes the background current, the current formed by the incident electron beam penetrating the sample (if any), and the secondary electron current;

[0064] Calculate the secondary electron current ISE according to the formula I2 = IBG + Iothers + ISE (where ISE is the secondary electron current). Note that due to the measurement of the I injection current and I1, the size of I others (other electron currents) can be estimated;

[0065] S5: Calculate the secondary emission coefficient

[0066] The secondary emission coefficient δ is usually defined as the number of secondary electrons excited per unit incident electron, but in actual measurements, it is often expressed as a current ratio;

[0067] Based on the secondary electron current ISE and the incident electron beam current Iinjection current, the secondary emission coefficient δ=ISE / Iinjection current can be calculated.

[0068] When the injection current I is 5.62×10 -8 A, the experimental data are measured, as shown in Table 1.

[0069] Table 1: Secondary emission coefficient measurement experimental data

[0070] Embodiment 1 Embodiment 2 Embodiment 3 Comparative Example 1 Secondary emission coefficient 0.62 0.67 0.75 1.32

[0071] It can be seen from Table 1 that the secondary emission coefficient of the collector electrode made by doping graphite with metal has been significantly reduced, and the 80%-90% graphite ratio and the 7-8μm copper layer thickness have reduced the secondary emission coefficient to a certain extent.

[0072] Embodiment 1, Embodiment 2, and Embodiment 3 are compared with Comparative Example 1. The graphite-doped metal collector electrode parts are partially copper-plated and vacuum-heat-treated to improve the bonding strength between the copper-plated layer and the graphite-doped metal substrate, improve the wettability of the solder on the graphite-doped metal surface, realize the connection between the collector electrode lead and the collector electrode, and meet the requirements for electrification of each collector electrode. By adopting a lightweight new material, graphite-doped metal, the secondary emission coefficient and weight of the collector electrode itself are significantly reduced. The collector electrode parts are machined and formed by a mechanical processing method using alcohol as a coolant, thereby avoiding problems such as degassing of the collector electrode caused by the inability to completely remove the residual coolant. In addition, an acetone ultrasonic cleaning method is used to remove the debris or particles remaining on the surface of the collector electrode parts after processing, thereby avoiding problems such as sparking of the traveling wave tube due to the formation of excess materials after assembling the entire tube. While meeting the processing accuracy of the collector electrode, the serious degassing problem of the material caused by improper processing technology in the later stage is effectively solved, which is helpful to improve the vacuum degree in the traveling wave tube and improve the consistency of electrical parameters such as spiral current.

[0073] The embodiments of the present invention are provided for the purpose of illustration and description. Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations of the present invention. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A method for surface treatment of collector electrode with low secondary electron emission coefficient, characterized in that: The following steps are involved: S1: Processing graphite-doped metal into collector electrode parts by mechanical processing; S2: Use acetone ultrasonic cleaning to remove the debris or particles remaining on the surface of the collector electrode parts after processing; S3: Maintain the collector electrode parts at 700°C for 10 minutes to perform hydrogen burning purification treatment; S4: copper plating is performed on the welding area of ​​the graphite-doped metal material, and then the welding area is kept at 900°C-950°C in a vacuum furnace for 20 minutes; S5: Use electric vacuum devices and use low vapor pressure gold-based alloy solder as filler solder to assemble the collector, and weld it into the collector component in a vacuum furnace.

2. The method for surface treatment of collector electrode with low secondary electron emission coefficient according to claim 1, characterized in that: The graphite in the graphite-doped metal in S1 accounts for 80%-90%.

3. The method for surface treatment of collector electrode with low secondary electron emission coefficient according to claim 1, characterized in that: The machining methods in S1 include turning, milling, grinding and electric spark machining.

4. The method for surface treatment of collector electrode with low secondary electron emission coefficient according to claim 1, characterized in that: In the S1, alcohol is used as a coolant during machining.

5. The method for surface treatment of collector electrode with low secondary electron emission coefficient according to claim 1, characterized in that: The vacuum degree in the vacuum furnace of S4 and S5 shall not be less than 10 -4 Pa.

6. The method for surface treatment of collector electrode with low secondary electron emission coefficient according to claim 1, characterized in that: The copper layer thickness in the S4 is 7-8 μm.

7. The method for surface treatment of collector electrode with low secondary electron emission coefficient according to claim 1, characterized in that: The gold-based alloy solder in S5 includes Au-Cu and Au-Ni.

8. The method for surface treatment of collector electrode with low secondary electron emission coefficient according to claim 8, characterized in that: The Au-Cu welding temperature is 910-930° C., the Au-Ni welding temperature is 950-1000° C., and the heating rate is 10° C. / min.

Citation Information

Patent Citations

  • Double-layer electrode for multi-level depressed collector and preparation process thereof

    CN101752168A

  • Graphite composite multistage depressed collector and manufacturing method thereof

    CN102074438A

  • Metallization process and welding method for pyrolytic graphite

    CN102234764A

  • Surface treatment method before brazing space traveling-wave tube collector and radiator

    CN103143801A

  • Method for processing surface of Cu electrode of multistage depressed collector through graphene

    CN104465267A