Power device and preparation method thereof, power module, power conversion circuit and vehicle

By forming epitaxial layers, grooves and multi-layer oxide structures on the substrate of the power device, the problem of insufficient conductivity and pressure bearing capacity of the trench type device is solved, and better voltage tolerance and conductivity are achieved.

CN119092411APending Publication Date: 2024-12-06YOFC ADVANCED SEMICONDUCTOR (WUHAN) CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411193174.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Due to the different crystal phases of the trench bottom and side walls, the existing trench power devices have a thicker oxide layer on the side walls, which affects the conduction performance and have poor pressure bearing capacity.

Method used

An epitaxial layer is formed on one side of the substrate, and grooves are etched thereon, a first oxide sub-layer, a nitride sub-layer and a sacrificial layer are formed in sequence, and a first oxide layer with uniform thickness is formed by removing these layers and A thinner second oxide layer covers the bottom and side walls of the grooves to improve the device's conductivity and pressure bearing capacity.

Benefits of technology

By providing a first oxide layer with uniform thickness and a thinner second oxide layer, the on-conductivity and pressure bearing capacity of the device are improved, and a larger voltage can be borne and the switching speed can be increased.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092411A_ABST
    Figure CN119092411A_ABST
Patent Text Reader

Abstract

The invention discloses a power device and a preparation method thereof, a power module, a power conversion circuit and a vehicle. The preparation method comprises the following steps: forming an epitaxial layer on one side of a substrate; forming at least one groove in the first surface of the epitaxial layer; forming a first oxide sub-layer in the groove and on the first surface of the epitaxial layer; the first oxide sub-layer covers the bottom and the side wall of the groove and the first surface of the epitaxial layer without the groove; the nitride sub-layer covers the first oxide sub-layer; the sacrificial layer covers the nitride sub-layer at the bottom of the groove; removing the sacrificial layer, the nitride sub-layer and the first oxide sub-layer on the side wall of the groove to form a first oxide layer; the first oxide layer covers the bottom of the groove; the second oxide layer covers the first oxide layer, the side wall of the groove and the first surface of the epitaxial layer; and forming a gate on one side, away from the substrate, of the second oxide layer. According to the invention, the conduction performance and the pressure bearing capability of the device can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a power device and a preparation method thereof, a power module, a power conversion circuit and a vehicle. Background Art

[0002] Existing trench power devices form an oxide layer by high-temperature oxidation. Due to the different crystal phases between the bottom and sidewalls of the trench, a thicker oxide layer will be formed on the sidewalls of the trench than at the bottom of the groove, affecting the conduction performance of the device. At the same time, the pressure-bearing capacity of the device is poor. Summary of the invention

[0003] The present invention provides a power device and a preparation method thereof, a power module, a power conversion circuit and a vehicle, which can improve the conduction performance and pressure-bearing capacity of the device.

[0004] According to one aspect of the present invention, there is provided a method for preparing a power device, comprising:

[0005] forming an epitaxial layer on one side of the substrate; the epitaxial layer includes a first surface away from the substrate;

[0006] forming at least one groove in the first surface of the epitaxial layer;

[0007] forming a first oxide sublayer in the groove and on the first surface of the epitaxial layer; the first oxide sublayer covers the bottom and sidewalls of the groove, and the first surface of the epitaxial layer where no groove is provided;

[0008] forming a nitride sublayer on a side of the first oxide sublayer away from the substrate; the nitride sublayer covers the first oxide sublayer;

[0009] forming a sacrificial layer on a side of the nitride sub-layer away from the substrate; the sacrificial layer covers the nitride sub-layer at the bottom of the groove;

[0010] Removing the sacrificial layer, the nitride sub-layer and the first oxide sub-layer on the sidewall of the groove to form a first oxide layer; the first oxide layer covers the bottom of the groove;

[0011] forming a second oxide layer on a side of the first oxide layer away from the substrate; the second oxide layer covers the first oxide layer, the sidewall of the groove and the first surface of the epitaxial layer; the thickness of the second oxide layer is less than the thickness of the first oxide layer;

[0012] A gate is formed on a side of the second oxide layer away from the substrate.

[0013] Optionally, the thickness of the first oxide layer is 800 angstroms to 2000 angstroms;

[0014] The thickness of the second oxide layer covering the sidewall of the groove is 500 angstroms to 800 angstroms.

[0015] Optionally, removing the sacrificial layer, the nitride sub-layer, and the first oxide sub-layer on the sidewall of the groove to form a first oxide layer includes:

[0016] The nitride sublayer not covered by the sacrificial layer is removed to form a nitride layer; the nitride layer covers the first oxide sublayer at the bottom of the groove;

[0017] removing the sacrificial layer;

[0018] removing the first oxide sublayer not covered by the nitride layer to form a first oxide layer;

[0019] The nitride layer is removed.

[0020] Optionally, removing the nitride sublayer not covered by the sacrificial layer to form a nitride layer includes:

[0021] The nitride sub-layer not covered by the sacrificial layer is removed by silver acid to form a nitride layer.

[0022] Optionally, removing the sacrificial layer comprises:

[0023] The sacrificial layer is removed by anisotropic etching.

[0024] Optionally, removing the first oxide sublayer not covered by the nitride layer to form a first oxide layer includes:

[0025] The first oxide sub-layer not covered by the nitride layer is removed by hydrofluoric acid to form a first oxide layer.

[0026] Optionally, forming a sacrificial layer on a side of the nitride sub-layer away from the substrate comprises:

[0027] forming a sacrificial sublayer on a side of the nitride sublayer away from the substrate; the sacrificial sublayer covers the nitride sublayer;

[0028] The sacrificial sub-layer on the sidewall of the groove and the first surface is removed to form a sacrificial layer.

[0029] Optionally, forming a first oxide sublayer in the groove and on the first surface of the epitaxial layer includes:

[0030] forming a first oxide sublayer in the recess and on the first surface of the epitaxial layer by low pressure chemical vapor deposition;

[0031] Forming a nitride sub-layer on a side of the first oxide sub-layer away from the substrate, comprising:

[0032] A nitride sub-layer is formed on a side of the first oxide sub-layer away from the substrate by a low pressure chemical vapor deposition method.

[0033] Optionally, the material of the substrate includes silicon carbide or silicon;

[0034] The material of the first oxide sub-layer includes tetraethyl orthosilicate;

[0035] The material of the nitride sublayer includes silicon nitride;

[0036] The material of the sacrificial layer includes polysilicon.

[0037] According to another aspect of the present invention, there is provided a power device, which is prepared by the method for preparing a power device according to any embodiment of the present invention.

[0038] According to another aspect of the present invention, a power module is provided, comprising a substrate and a power device according to any embodiment of the present invention, wherein the substrate is used for carrying the power device.

[0039] According to another aspect of the present invention, there is provided a power conversion circuit, the power conversion circuit being used for one or more of current conversion, voltage conversion, and power factor correction;

[0040] The power conversion circuit comprises a circuit board and a power device according to any embodiment of the present invention, and the power device is electrically connected to the circuit board.

[0041] According to another aspect of the present invention, a vehicle is provided, comprising a load and the power conversion circuit described in any embodiment of the present invention, the power conversion circuit being used to convert AC power into DC power, convert AC power into AC power, convert DC power into DC power, or convert DC power into AC power and then input it into the load.

[0042] The method for preparing a power device provided by the technical solution of the embodiment of the present invention comprises: forming an epitaxial layer on one side of a substrate; the epitaxial layer comprises a first surface away from the substrate; forming at least one groove on the first surface of the epitaxial layer; forming a first oxide sublayer in the groove and on the first surface of the epitaxial layer; the first oxide sublayer covers the bottom and sidewall of the groove, and the first surface of the epitaxial layer without a groove; forming a nitride sublayer on the side of the first oxide sublayer away from the substrate; the nitride sublayer covers the first oxide sublayer; forming a sacrificial layer on the side of the nitride sublayer away from the substrate; the sacrificial layer covers the nitride sublayer at the bottom of the groove; removing the sacrificial layer, the nitride sublayer and the first oxide sublayer on the sidewall of the groove to form a first oxide layer; the first oxide layer covers the bottom of the groove; forming a second oxide layer on the side of the first oxide layer away from the substrate; the second oxide layer covers the first oxide layer, the sidewall of the groove and the first surface of the epitaxial layer; the thickness of the second oxide layer is less than the thickness of the first oxide layer; forming a gate on the side of the second oxide layer away from the substrate. In the embodiment of the present invention, the first oxide layer and the second oxide layer are thicker at the bottom of the groove, which can withstand a larger voltage and improve the performance of the device; the second oxide layer on the side wall of the groove is thinner, which can make the conductivity of the power device better, more conducive to conductivity, and can improve the switching speed of the device.

[0043] It should be understood that the contents described in this section are not intended to identify the key or important features of the embodiments of the present invention, nor are they intended to limit the scope of the present invention. Other features of the present invention will become easily understood through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0045] Figure 1 It is a flow chart of a method for preparing a power device provided by an embodiment of the present invention.

[0046] Figure 2-Figure 11 It is a schematic diagram of an intermediate structure of a power device provided by an embodiment of the present invention.

[0047] Fig.12 yes Figure 1 A detailed flow chart included in S160. DETAILED DESCRIPTION

[0048] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0049] It should be noted that the terms "first", "second", etc. in the present invention are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product, or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products, or devices.

[0050] The embodiment of the present invention provides a method for preparing a power device. Figure 1 is a flow chart of a method for preparing a power device provided by an embodiment of the present invention; Figure 2-Figure 11 is a schematic diagram of an intermediate structure of a power device provided by an embodiment of the present invention, with reference to Figure 1 , the preparation method comprises:

[0051] S110, forming an epitaxial layer on one side of the substrate; the epitaxial layer includes a first surface away from the substrate.

[0052] The power device may be a silicon carbide trench metal oxide semiconductor field effect transistor (MOSFET). The substrate may be a silicon substrate or a silicon carbide substrate. Figure 2 If the device is an N-type device, the substrate 10 is an N+ substrate, such as an N+ silicon carbide substrate; the epitaxial layer 20 is an N-epitaxial layer, such as an N-silicon carbide epitaxial layer; if the device is a P-type device, the substrate 10 is a P+ substrate, and the epitaxial layer 20 is a P-epitaxial layer. The epitaxial layer 20 is formed on one side of the substrate 10 by epitaxial growth.

[0053] S120 , forming at least one groove on the first surface of the epitaxial layer.

[0054] Among them, reference Figure 2 At least one groove 30 is etched on the first surface of the epitaxial layer 20 by a conventional etching process.

[0055] S130, forming a first oxide sublayer in the groove and on the first surface of the epitaxial layer; the first oxide sublayer covers the bottom and sidewalls of the groove, and the first surface of the epitaxial layer where no groove is set.

[0056] The first oxide sublayer may be prepared by a low pressure chemical vapor deposition process or a thermal oxidation process. Exemplarily, the material of the first oxide sublayer may be silicon dioxide formed by decomposition of tetraethyl orthosilicate (TEOS); Exemplarily, refer to Figure 3 If the first oxide sublayer 41 is prepared by a thermal oxidation process, since the crystal phases of the epitaxial layer 20 at the bottom of the groove 30 and the first surface of the epitaxial layer 20 are the same, but are different from the crystal phases of the epitaxial layer 20 at the sidewall of the groove 30, the growth rate of the first oxide sublayer 41 at the sidewall of the groove 30 is greater than the growth rate of the first oxide sublayer 41 at the bottom of the groove 30. Therefore, the thickness of the first oxide sublayer 41 grown on the sidewall of the groove 30 along the first direction X is greater than the thickness of the first oxide sublayer 41 at the bottom of the groove 30 along the second direction Y, and the first direction X is perpendicular to the second direction Y. If the first oxide sublayer 41 is prepared by a low-pressure chemical vapor deposition process, the thickness of the first oxide sublayer 41 at each position is consistent.

[0057] S140, forming a nitride sublayer on a side of the first oxide sublayer away from the substrate; the nitride sublayer covers the first oxide sublayer.

[0058] Among them, reference Figure 3 A nitride sublayer 51 can be formed on the side of the first oxide sublayer 41 away from the substrate 10 by low-pressure chemical vapor deposition. The nitride sublayer 51 can be silicon nitride. The nitride sublayer 51 can be used to protect the surface of the first oxide sublayer 41 to prevent the surface of the first oxide sublayer 41 from being damaged and affecting the performance of the device.

[0059] S150, forming a sacrificial layer on a side of the nitride sub-layer away from the substrate; the sacrificial layer covers the nitride sub-layer at the bottom of the groove.

[0060] Among them, reference Figure 4 and Figure 5 , a sacrificial sublayer 61 may be first deposited by a deposition process to fill the groove 30 and cover the surface of the nitride sublayer 51 away from the substrate 10, and then the sacrificial sublayer 61 on the surface of the nitride sublayer 51 away from the substrate 10 and part of the sacrificial sublayer 61 in the groove 30 may be removed by an etching process, and a sacrificial layer 60 may be formed on the side of the nitride sublayer 51 away from the substrate 10. The material of the sacrificial layer 60 may be a polysilicon material. Since the nitride sublayer 51 in contact with the sacrificial layer 60 may be damaged when etching the sacrificial layer 60, the nitride sublayer 51 may protect the surface of the first oxide sublayer 41. The sacrificial layer 60 covers the nitride sublayer 51 at the bottom of the groove 30, and the nitride sublayer 51 at the bottom of the groove 30 includes the corner of the groove.

[0061] S160, removing the sacrificial layer, the nitride sub-layer and the first oxide sub-layer on the sidewall of the groove to form a first oxide layer; the first oxide layer covers the bottom of the groove.

[0062] The first oxide layer and the first oxide sublayer are made of the same material; Figure 6-Figure 9 , the sacrificial layer 60, the nitride sublayer 51 and the first oxide sublayer 41 on the sidewall of the groove 20 are removed to form a first oxide layer 40, which covers the bottom of the groove 30, and the bottom of the groove 30 includes the corner of the groove. Removing the sacrificial layer 60 and the nitride sublayer 51 can protect the surface where the first oxide layer is formed from being damaged, thereby avoiding affecting the device performance.

[0063] S170, forming a second oxide layer on a side of the first oxide layer away from the substrate; the second oxide layer covers the first oxide layer, the sidewall of the groove and the first surface of the epitaxial layer; the thickness of the second oxide layer is less than the thickness of the first oxide layer.

[0064] Among them, reference Fig.10 The second oxide layer 70 is formed on the side of the first oxide layer 40 away from the substrate 10 by a high temperature oxidation process. The second oxide layer 70 grows faster on the sidewall of the groove 30 and hardly grows on the first oxide layer 40 at the bottom of the groove 30, which can be ignored. Fig.10 The second oxide layer 70 grown at the bottom of the groove 30 is not shown. By controlling the process time, the thickness of the second oxide layer 70 can be made smaller than the thickness of the first oxide layer 40, and finally the thickness of the second oxide layer 70 on the side wall of the groove 30 is made smaller than the thickness of the first oxide layer 40 on the bottom of the groove 30. The bottom of the groove 30 includes the corner of the groove 30. Since the electric field at the corner of the groove 30 is easily concentrated, resulting in a large electric field and easy breakdown, a thicker first oxide layer 40 is provided at the bottom of the groove 30, which can withstand a larger voltage, improve the performance of the device, and solve the problem of electric field concentration at the bottom of the groove 30. The second oxide layer 70 on the side wall of the groove 30 is thinner, which can make the power device have better conductivity and be more conducive to conductivity.

[0065] S180 , forming a gate on a side of the second oxide layer away from the substrate.

[0066] Among them, reference Fig.11 A gate 80 is formed on a side of the second oxide layer 70 away from the substrate 10 ; the gate 80 may be a polysilicon layer.

[0067] The method for preparing a power device provided by the technical solution of the embodiment of the present invention comprises: forming an epitaxial layer on one side of a substrate; the epitaxial layer comprises a first surface away from the substrate; forming at least one groove on the first surface of the epitaxial layer; forming a first oxide sublayer in the groove and on the first surface of the epitaxial layer; the first oxide sublayer covers the bottom and sidewall of the groove, and the first surface of the epitaxial layer without a groove; forming a nitride sublayer on the side of the first oxide sublayer away from the substrate; the nitride sublayer covers the first oxide sublayer; forming a sacrificial layer on the side of the nitride sublayer away from the substrate; the sacrificial layer covers the nitride sublayer at the bottom of the groove; removing the sacrificial layer, the nitride sublayer and the first oxide sublayer on the sidewall of the groove to form a first oxide layer; the first oxide layer covers the bottom of the groove; forming a second oxide layer on the side of the first oxide layer away from the substrate; the second oxide layer covers the first oxide layer, the sidewall of the groove and the first surface of the epitaxial layer; the thickness of the second oxide layer is less than the thickness of the first oxide layer; forming a gate on the side of the second oxide layer away from the substrate. In the embodiment of the present invention, the first oxide layer and the second oxide layer are thicker at the bottom of the groove, which can withstand a larger voltage and improve the performance of the device; the second oxide layer on the side wall of the groove is thinner, which can make the conductivity of the power device better, more conducive to conductivity, and can improve the switching speed of the device.

[0068] Optionally, the thickness of the first oxide layer is 800 angstroms to 2000 angstroms; the thickness of the second oxide layer covering the sidewall of the groove is 500 angstroms to 800 angstroms.

[0069] Among them, the thickness of the first oxide layer and the second oxide layer formed can be adjusted by controlling the process conditions. For example, the thickness of the first oxide layer and the second oxide layer can be controlled by adjusting the length of the process operation time. The thickness of the first oxide layer is 800 angstroms-2000 angstroms; the thickness of the second oxide layer covering the side wall of the groove is 500 angstroms-800 angstroms, which can achieve a thicker thickness of the first oxide layer and the second oxide layer at the bottom of the groove, which can withstand a larger voltage and improve the performance of the device; and the second oxide layer on the side wall of the groove can be made thinner, which can make the conductivity of the power device better, more conducive to conductivity, and improve the switching speed of the device.

[0070] Optional, Fig.12 yes Figure 1 A detailed flow chart included in S160, refer to Fig.12 S160, removing the sacrificial layer, the nitride sub-layer and the first oxide sub-layer on the sidewall of the groove to form a first oxide layer, including:

[0071] S161 , removing the nitride sub-layer not covered by the sacrificial layer to form a nitride layer; the nitride layer covers the first oxide sub-layer at the bottom of the groove.

[0072] Among them, reference Figure 5-Figure 6 The nitride sublayer 51 not covered by the sacrificial layer 60 is removed by silver acid to form a nitride layer 50, and the nitride layer 50 covers the first oxide sublayer 51 at the bottom of the groove 30; since the nitride layer 50 at the bottom of the groove 30 is covered by the sacrificial layer 60, the nitride layer 50 covered by the sacrificial layer 60 can be retained.

[0073] S162, removing the sacrificial layer.

[0074] Among them, the sacrificial layer can be removed by anisotropic etching. Figure 7 It is the structure after removing the sacrificial layer.

[0075] S163, removing the first oxide sublayer not covered by the nitride layer to form a first oxide layer.

[0076] Among them, reference Figure 7 and Figure 8 , the first oxide sublayer 41 not covered by the nitride layer 50 can be removed by hydrofluoric acid to form the first oxide layer 40. Since the first oxide layer 40 at the bottom of the groove 30 is covered by the nitride layer 50, the first oxide layer 40 covered by the nitride layer 50 can be retained, and at this time the surface of the first oxide layer 40 is not damaged, and the performance of the device can be guaranteed.

[0077] S164, removing the nitride layer.

[0078] Among them, reference Fig. 9 , the nitride layer can be removed by silver acid.

[0079] Optionally, S161, removing the nitride sublayer not covered by the sacrificial layer to form a nitride layer, includes: removing the nitride sublayer not covered by the sacrificial layer by using silver acid to form a nitride layer.

[0080] Among them, the nitride sublayer not covered by the sacrificial layer is removed by silver acid to form a nitride layer. The process is simple and the cost is low. It will not affect the first oxide layer at the bottom of the groove, so the surface of the first oxide layer can be protected to ensure the performance of the power device.

[0081] Optionally, S162, removing the sacrificial layer, includes: removing the sacrificial layer by anisotropic etching.

[0082] Among them, removing the sacrificial layer by anisotropic etching has high production efficiency and low cost.

[0083] Optionally, S163, removing the first oxide sublayer not covered by the nitride layer to form a first oxide layer, includes: removing the first oxide sublayer not covered by the nitride layer by using hydrofluoric acid to form the first oxide layer.

[0084] Among them, the first oxide sublayer not covered by the nitride layer is removed by hydrofluoric acid to form the first oxide layer, which has a simple process and low cost. Since the nitride layer covers the first oxide layer at the bottom of the groove, the surface of the first oxide layer can be protected to ensure the performance of the power device.

[0085] Optionally, S150, forming a sacrificial layer on a side of the nitride sub-layer away from the substrate, includes:

[0086] S151, forming a sacrificial sub-layer on a side of the nitride sub-layer away from the substrate; the sacrificial sub-layer covers the nitride sub-layer.

[0087] Among them, reference Figure 4 A sacrificial sub-layer 51 is formed on a side of the nitride sub-layer 41 away from the substrate 10 , and the sacrificial sub-layer 51 may be deposited by a deposition process.

[0088] S152 , removing the sacrificial sublayer on the groove sidewall and the first surface to form a sacrificial layer.

[0089] Among them, reference Figure 5 , removing the sacrificial sublayer on the groove sidewall and the first surface by dry etching to form a sacrificial layer; illustratively, the dry etching includes anisotropic etching, etc.

[0090] Optionally, S130, forming a first oxide sublayer in the groove and on the first surface of the epitaxial layer, includes: forming the first oxide sublayer in the groove and on the first surface of the epitaxial layer by low pressure chemical vapor deposition.

[0091] Optionally, S140, forming a nitride sublayer on a side of the first oxide sublayer away from the substrate, includes: forming the nitride sublayer on a side of the first oxide sublayer away from the substrate by low pressure chemical vapor deposition.

[0092] Among them, the low-pressure chemical vapor deposition process can make the first oxide sublayer and the nitride sublayer have higher uniformity and fewer defects, thereby improving the performance of the power device.

[0093] Optionally, the material of the substrate includes silicon carbide or silicon; the material of the first oxide sublayer includes tetraethyl orthosilicate; the material of the nitride sublayer includes silicon nitride; and the material of the sacrificial layer includes polysilicon.

[0094] The materials of the substrate and the epitaxial layer include silicon carbide or silicon; the material of the first oxide sublayer includes tetraethyl orthosilicate; the material of the nitride sublayer includes silicon nitride; and the material of the sacrificial layer includes polysilicon. The process preparation of these materials is mature and the operation is simple.

[0095] An embodiment of the present invention provides a power device based on the above embodiment, which is prepared by using the method for preparing a power device described in any embodiment of the present invention.

[0096] The power device provided by the technical solution of the embodiment of the present invention and the method for preparing the power device described in any embodiment of the present invention have the same beneficial effects.

[0097] An embodiment of the present invention further provides a power module based on the above embodiment, comprising a substrate and the power device described in any embodiment of the present invention, wherein the substrate is used to carry the power device.

[0098] The power module provided by the technical solution of the embodiment of the present invention has the same beneficial effects as the power device described in any embodiment of the present invention.

[0099] An embodiment of the present invention further provides a power conversion circuit based on the above embodiments, and the power conversion circuit is used for one or more of current conversion, voltage conversion, and power factor correction; the power conversion circuit includes a circuit board and the power device described in any embodiment of the present invention, and the power device is electrically connected to the circuit board.

[0100] The power conversion circuit provided by the technical solution of the embodiment of the present invention has the same beneficial effects as the power device described in any embodiment of the present invention.

[0101] An embodiment of the present invention further provides a vehicle based on the above embodiments, including a load and the power conversion circuit described in any embodiment of the present invention, the power conversion circuit is used to convert AC power into DC power, convert AC power into AC power, convert DC power into DC power, or convert DC power into AC power and then input it into the load.

[0102] The vehicle provided by the technical solution of the embodiment of the present invention and the power device described in any embodiment of the present invention have the same beneficial effects.

[0103] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps described in the present invention can be executed in parallel, sequentially or in different orders, as long as the desired results of the technical solution of the present invention can be achieved, and this document does not limit this.

[0104] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a power device, It is characterized in that include: forming an epitaxial layer on one side of the substrate; The epitaxial layer includes a first surface away from the substrate; forming at least one groove on the first surface of the epitaxial layer; forming a first oxide sublayer in the groove and on the first surface of the epitaxial layer; the first oxide sublayer covers the bottom and sidewalls of the groove, and the first surface of the epitaxial layer where the groove is not provided; Forming a nitride sublayer on a side of the first oxide sublayer away from the substrate; the nitride sublayer covers the first oxide sublayer; forming a sacrificial layer on a side of the nitride sub-layer away from the substrate; the sacrificial layer covers the nitride sub-layer at the bottom of the groove; removing the sacrificial layer, the nitride sub-layer and the first oxide sub-layer on the sidewall of the groove to form a first oxide layer; The first oxide layer covers the bottom of the groove; forming a second oxide layer on a side of the first oxide layer away from the substrate; The second oxide layer covers the first oxide layer, the sidewall of the groove and the first surface of the epitaxial layer; The thickness of the second oxide layer is less than the thickness of the first oxide layer; A gate is formed on a side of the second oxide layer away from the substrate.

2. The preparation method according to claim 1, It is characterized in that The thickness of the first oxide layer is 800 angstroms to 2000 angstroms; The thickness of the second oxide layer covering the sidewall of the groove is 500 angstroms to 800 angstroms.

3. The preparation method according to claim 1, It is characterized in that Removing the sacrificial layer, the nitride sub-layer, and the first oxide sub-layer on the sidewall of the groove to form a first oxide layer, comprising: The nitride sublayer not covered by the sacrificial layer is removed to form a nitride layer; the nitride layer covers the first oxide sublayer at the bottom of the groove; removing the sacrificial layer; removing the first oxide sublayer not covered by the nitride layer to form a first oxide layer; The nitride layer is removed.

4. The preparation method according to claim 3, It is characterized in that Removing the nitride sublayer not covered by the sacrificial layer to form a nitride layer, comprising: The nitride sub-layer not covered by the sacrificial layer is removed by silver acid to form a nitride layer.

5. The preparation method according to claim 3, It is characterized in that Removing the sacrificial layer comprises: The sacrificial layer is removed by anisotropic etching.

6. The preparation method according to claim 3, It is characterized in that Removing the first oxide sublayer not covered by the nitride layer to form a first oxide layer, comprising: The first oxide sub-layer not covered by the nitride layer is removed by hydrofluoric acid to form a first oxide layer.

7. The preparation method according to claim 1, It is characterized in that Forming a sacrificial layer on a side of the nitride sub-layer away from the substrate, comprising: Forming a sacrificial sublayer on a side of the nitride sublayer away from the substrate; the sacrificial sublayer covers the nitride sublayer; The sacrificial sublayer on the sidewall of the groove and the first surface is removed to form a sacrificial layer.

8. The preparation method according to claim 1, It is characterized in that Forming a first oxide sublayer in the groove and on the first surface of the epitaxial layer, comprising: forming a first oxide sublayer in the groove and on the first surface of the epitaxial layer by low pressure chemical vapor deposition; Forming a nitride sublayer on a side of the first oxide sublayer away from the substrate, comprising: A nitride sub-layer is formed on a side of the first oxide sub-layer away from the substrate by a low pressure chemical vapor deposition method.

9. The preparation method according to claim 1, It is characterized in that The material of the substrate includes silicon carbide or silicon; The material of the first oxide sublayer includes tetraethyl orthosilicate; The material of the nitride sublayer includes silicon nitride; The material of the sacrificial layer includes polysilicon.

10. A power device, It is characterized in that The power device is prepared by the method for preparing the power device according to any one of claims 1 to 9.

11. A power module, It is characterized in that The invention comprises a substrate and at least one power device according to claim 10, wherein the substrate is used for supporting the power device.

12. A power conversion circuit, It is characterized in that The power conversion circuit is used for one or more of current conversion, voltage conversion, and power factor correction; The power conversion circuit comprises a circuit board and at least one power device as claimed in claim 10, wherein the power device is electrically connected to the circuit board.

13. A vehicle, It is characterized in that It includes a load and a power conversion circuit as described in claim 12, wherein the power conversion circuit is used to convert AC power into DC power, convert AC power into AC power, convert DC power into DC power, or convert DC power into AC power and then input it into the load.

Citation Information

Patent Citations

  • Manufacturing method for trench gate power transistor

    CN105789053A

  • Trench MOSFET and technological method thereof

    CN108258053A

  • Manufacturing method of semiconductor device

    CN112802752A

  • Forming method of MOS device

    CN113675078A

  • Semiconductor device, power module, power conversion circuit, vehicle and manufacturing method of semiconductor device

    CN118299425A