Method for non-destructively measuring bonding strength of wafer
A non-destructive method for measuring wafer bond strength using pressure and tension to create cracks, combined with water mist and infrared/ultrasonic detection, addresses the destructive nature of existing methods, enhancing accuracy and reducing waste.
Patent Information
- Application Number
- CN202411091455.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Current methods for measuring wafer bond strength in low-temperature direct bonding are destructive, leading to high wafer scrap rates and accuracy issues due to the use of blades, which cause damage and introduce measurement errors from inconsistent blade insertion parameters.
A non-destructive method involving pressure and tension application to create a crack in the bonded wafers, followed by water mist penetration and measurement using infrared or ultrasonic detection to calculate bond strength without damaging the wafers.
Accurately measures bond strength without destroying the wafers, reducing scrap rates and measurement errors, thus being cost-effective and precise.
Smart Images

Figure CN119092421A_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of wafer detection methods, and in particular to a method for non-destructively measuring wafer bonding strength. Background technology:
[0002] Low-temperature wafer direct bonding technology is the most popular bonding method in recent years, but it is also very difficult. This is because it is the bonding method with the highest requirements for silicon wafer surface morphology and surface treatment process. Poor silicon wafer surface morphology or surface treatment will cause irreparable defects in the bonded wafer pair. The process of wafer direct bonding has gone through the process from early high-temperature wafer bonding to the currently widely studied and promoted low-temperature wafer bonding process, mainly to overcome the impact of high temperature on devices, so people began to focus on the research of low-temperature wafer bonding. The main research currently includes hydrophilic bonding and hydrophobic bonding. The essence of low-temperature direct bonding is to improve the surface energy by surface treatment of the silicon surface, and then bond two or more silicon wafers together through water molecule bridging (hydrophilic bonding) or HF molecule bridging (hydrophobic bonding) and intermolecular forces.
[0003] In low-temperature wafer direct bonding technology, bond strength is one of the most important measurement characteristics, and it is an important indicator related to the quality of bonding. If the bond strength is low, the two bonded wafers are likely to crack during processing, leading to failure. Slight changes in manufacturing process parameters (especially the surface pretreatment steps and bonding conditions of the wafers) will directly affect the strength performance of the bonding interface. Therefore, insufficient bond strength reflects that there is a problem in some link of the bonding process; high bond strength proves that the two wafers are in close contact, and the impact of cracks and voids on the bonding interface is minimal. Devices made using bonding technology are also less likely to fail due to damage from environmental factors such as temperature and humidity.
[0004] At present, commercial bond strength measurement methods all use destructive measurement methods, including crack propagation diffusion method, straight pull method, micro wedge groove test method, static oil pressure test method and four-point bending test method, among which crack propagation diffusion method is the most commonly used. For example, see the Chinese invention patent application with patent number: 201811368336.8, which discloses "a method for measuring bond strength and a bonded wafer using the measurement method". This technical solution is to use the crack propagation diffusion method, commonly known as the blade insertion method. This is the most traditional and common method for measuring bond strength. It separates the two wafers by inserting a thin blade at the bonding interface. The crack length finally obtained by this technical solution is a representation of the bond strength. However, in this method, the thin blade will cause serious damage to the wafer, which is a destructive measurement method. The bonding energy is related to the crack length, blade thickness, wafer thickness and blade insertion speed, and the thin blade will cause serious damage to the wafer, resulting in the scrapping of the wafer, so it is very disadvantageous in terms of accuracy and cost.
[0005] In summary, in low-temperature wafer direct bonding technology, bond strength is one of the most important measurement characteristics, and it is an important indicator related to the quality of bonding. However, the current commercial bond strength measurement methods all use destructive measurement methods, resulting in a high wafer scrap rate. In view of this, the inventors combine the deficiencies of the prior art and propose the following technical solutions. Summary of the invention:
[0006] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and propose a method for non-destructively measuring the bonding strength of a wafer.
[0007] In order to solve the above technical problems, the present invention adopts the following technical scheme: the method for non-destructively measuring the bonding strength of wafers comprises the following steps: step 1: placing two wafers that have been bonded on a work platform, wherein the first wafer located at the bottom is fixed on the surface of the work platform; step 2: applying pressure and tension to the second wafer located at the top at different regions thereof at the same time; step 3: a crack is generated between the second wafer and the first wafer under the pressure and tension; step 4: after the crack is formed, spraying water mist or other liquid into the crack to allow the water mist to penetrate into the crack; step 5: measuring the size of the crack, and calculating the bonding strength of the wafer according to the following formula: γ = 3Et 3 y 2 / 32L 4 .
[0008] Furthermore, in the above technical solution, the first wafer is fixed to the surface of the working platform by vacuum adsorption, that is, pores are distributed on the surface of the working platform, and the first wafer is adsorbed on the surface of the working platform by forming a vacuum or negative pressure at the pores.
[0009] Furthermore, in the above technical solution, the first wafer is fixed to the surface of the working platform by mechanical embedding, that is, a positioning groove is formed on the surface of the working platform, and the first wafer is embedded in the positioning groove.
[0010] Furthermore, in the above technical solution, the tension acting position F1 on the second wafer is close to the edge, the pressure acting position F2 on the second wafer is far away from the tension acting position F1, and the distance between them is greater than the length L of the crack.
[0011] Furthermore, in the above technical solution, in step 5, the size of the crack is measured by infrared detection or ultrasonic detection.
[0012] Furthermore, in the above technical scheme, another technical problem to be solved by the present invention is to propose a device for non-destructively measuring the bonding strength of wafers according to the above technical scheme, and the device includes: a working platform, which is used to place two wafers that have been bonded, and the working platform has a vacuum adsorption or mechanical positioning device to fix the first wafer located below to the surface of the working platform; a pressure mechanism, which is located on the working platform, and the two wafers on the working platform are pressed downward by the pressure mechanism; a tension mechanism, which is located on the working platform, and the tension mechanism acts on the second wafer located above to form an upward tension on it; a spray mechanism, which is located on the side of the working platform; a detection device, which is an infrared detector or an ultrasonic detector.
[0013] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0014] Firstly, the present invention refers to the existing blade insertion method, but does not need to use a blade, thereby avoiding destructive measurement caused by blade insertion and avoiding the cost problem caused by wafer scrapping.
[0015] Secondly, after adopting the measuring method of the present invention, the measuring error caused by the inconsistent factors such as the inserting speed and angle of the blade in the existing inserting method can be avoided.
[0016] In summary, the non-destructive bonding strength measurement method provided by the present invention can accurately measure the bonding strength without destroying the wafer, so it is very advantageous in terms of accuracy and cost. Description of the drawings:
[0017] Figure 1 It is a working principle diagram of the present invention;
[0018] Figure 2 It is a schematic diagram of the first embodiment of the device in the present invention;
[0019] Figure 3 It is a schematic diagram of the second embodiment of the device in the present invention. Specific implementation method:
[0020] The present invention is further described below in conjunction with specific embodiments and drawings.
[0021] See Figure 1 As shown, this is a working principle diagram of the method for non-destructively measuring wafer bonding strength used in the invention. The method comprises the following steps:
[0022] Step 1: Place the bonded wafer 2 on the work platform 1, wherein the first wafer 21 located below is fixed on the surface of the work platform 1. In this step 1, the first wafer 21 can be fixed on the work platform 1 by vacuum adsorption. This method will not damage the first wafer 21 and ensures the integrity of the first wafer 21 to the greatest extent possible.
[0023] Step 2: Apply pressure and tension to different areas of the second wafer 22 located above. By applying pressure to form a pressing force, a pressing fulcrum relative to the pulling force is formed to press the second wafer 22 onto the first wafer 21, so that the bonded wafer 2 will not be directly separated from the work platform under the action of the pulling force. The applied pressure should not cause compression damage to the wafer, and the wafer can be pressed down.
[0024] The pressure and tension are respectively applied to different regions of the second wafer 22, wherein in order to facilitate the generation of cracks, the tension application position F1 on the second wafer 22 should be close to the edge of the second wafer 22. At the same time, the pressure application position F2 on the second wafer 22 is far away from the tension application position F1, and usually the pressure application position F2 and the tension application position F1 are respectively located on opposite sides of the second wafer.
[0025] Step 3: As the tension increases, the pressure position F2 at one end of the second wafer 22 is suppressed by the pressure, and the tension position F1 at the other end is deformed under the tension, and within the elastic deformation range, a crack 20 is generated between the second wafer 22 and the first wafer 21. The distance between the pressure position F2 and the tension position F1 is greater than the length L of the crack, that is, the crack 20 cannot overlap with the pressure position F2, otherwise it will affect the crack length and cause the measurement result to be invalid. If the crack overlaps with the pressure position F2, it can be improved by reducing the pulling height of the tension or adjusting the pressure position F2.
[0026] Step 4: After the crack 20 is formed, spray water mist or other liquid into the crack 20 to allow the water mist to penetrate into the crack 20. Spraying water mist or other liquid substances into the crack is to facilitate the subsequent measurement of the size of the crack. Because the crack length will be obtained later using an infrared camera or an ultrasonic microscope, and different materials have different reflection and penetration behaviors under infrared light or ultrasonic waves, so the crack length can be observed in the image.
[0027] Step 5: Measure the size of the crack 20 by infrared detection or ultrasonic detection, and calculate the wafer bonding strength according to the following formula:
[0028] γ=3Et 3 y 2 / 32L 4 ,in,
[0029] γ is the wafer bonding strength;
[0030] E is the Young’s modulus of a single wafer;
[0031] t is the thickness of a single wafer;
[0032] y is the height by which the second wafer is stretched;
[0033] L is the length of the crack;
[0034] The length L of the crack is the distance from the center of the tension acting position F1 to the deepest part of the crack, and the height y of the second wafer stretched is the pulling height at the center of the tension acting position F1.
[0035] The present invention refers to the existing blade insertion method, but does not need to use a blade, thereby avoiding destructive measurement caused by blade insertion and avoiding the cost problem caused by wafer scrapping. At the same time, after adopting the measurement method of the present invention, the measurement error caused by inconsistent factors such as the blade insertion speed and angle in the existing blade insertion method can be avoided.
[0036] After the wafer 2 of the present invention has completed the bonding strength measurement, it can be reused after the bonding process is released and the surface is cleaned, thus avoiding waste.
[0037] According to the above-mentioned measuring method of the present invention, corresponding measuring equipment can be designed. Figure 2 As shown, the device includes: a working platform 1, a pressure mechanism 3, a tension mechanism 4, a spray mechanism 5 and a detection device 6.
[0038] The work platform 1 is used to place two wafers 2 that have been bonded, and the work platform 1 has a vacuum adsorption device to fix the first wafer 21 located below to the surface of the work platform 1. Figure 2As shown, the vacuum adsorption device is realized by distributing air holes 11 on the surface of the working platform 1. The air holes 11 are connected to an external vacuum air pump. The first wafer is adsorbed on the surface of the working platform by forming a vacuum or negative pressure at the air holes 11.
[0039] This vacuum adsorption method will not cause damage or destruction to the wafer. Of course, other mechanical methods can also be used, such as the attached Figure 3 As shown, this is a schematic diagram of the second embodiment of the present invention. In the second embodiment, the first wafer is fixed to the surface of the work platform 1 by mechanical clamping, that is, a positioning groove 12 is formed on the surface of the work platform 1, and the second wafer 21 is clamped in the positioning groove 12. Of course, the first wafer can also be fixed by mechanical clamping. The present invention prefers the fixing method of vacuum adsorption.
[0040] The pressure mechanism is located on the working platform 1 , and can be a cylinder or a hydraulic cylinder, or a connecting rod mechanism, and is installed above the working platform. The pressure mechanism 3 is used to press the wafer 2 on the working platform 1 .
[0041] The pulling mechanism 4 is also located on the working platform 1. The pulling mechanism can be a cylinder or a hydraulic cylinder mechanism. The pulling mechanism 4 acts on the second wafer located above to form an upward pulling force on it. The connection between the pulling mechanism 4 and the second wafer can also be a vacuum adsorption method, that is, a vacuum suction head is set at the end of the pulling mechanism 4, and the second wafer is pulled by vacuum adsorption. Of course, the connection between the pulling mechanism 4 and the second wafer 22 can also be achieved by adhesive bonding.
[0042] The spray mechanism 5 is located on the side of the working platform 1 and is used to spray water mist or other liquids into the cracks.
[0043] The detection device 6 is an infrared detector or an ultrasonic detector. It can be directly set above the workbench and moved by a mechanical arm, or it can be set separately from the workbench as an independent component. When testing, the wafer is taken out from the work platform 1 and placed in the detection device 6 for testing.
[0044] Of course, the above description is only a specific embodiment of the present invention and is not intended to limit the scope of implementation of the present invention. All equivalent changes or modifications made according to the structure, characteristics and principles described in the patent application scope of the present invention should be included in the patent application scope of the present invention.
Claims
1. A method for non-destructively measuring wafer bonding strength, characterized in that: The method comprises the following steps: Step 1: Place the two bonded wafers on a work platform, wherein the first wafer at the bottom is fixed on the surface of the work platform; Step 2: Applying pressure and tension to different regions of the second wafer at the same time; Step 3: A crack is generated between the second wafer and the first wafer under the pressing effect of pressure and the tensile force; Step 4: After the cracks are formed, spray water mist or liquid into the cracks to allow the water mist to penetrate into the cracks; Step 5: Measure the size of the crack and calculate the wafer bonding strength according to the following formula: γ=3Et 3 y 2 / 32L 4 ,in, γ is the wafer bonding strength; E is the Young’s modulus of a single wafer; t is the thickness of a single wafer; y is the height by which the second wafer is stretched; L is the length of the crack.
2. The method for non-destructively measuring wafer bonding strength according to claim 1, characterized in that: The first wafer is fixed on the surface of the work platform by vacuum adsorption, that is, air holes are distributed on the surface of the work platform, and the first wafer is adsorbed on the surface of the work platform by forming a vacuum or negative pressure at the air holes.
3. The method for non-destructively measuring wafer bonding strength according to claim 1, characterized in that: The first wafer is fixed to the surface of the working platform by mechanical embedding, that is, a positioning groove is formed on the surface of the working platform, and the first wafer is embedded in the positioning groove.
4. The method for non-destructively measuring wafer bonding strength according to claim 1, characterized in that: The tension acting position F1 on the second wafer is close to the edge, and the pressure acting position F2 on the second wafer is far away from the tension acting position F1 , and the distance between the two is greater than the length L of the crack.
5. The method for non-destructively measuring wafer bonding strength according to claim 1, characterized in that: In step 5, the size of the crack is measured by infrared detection or ultrasonic detection.
6. The method for non-destructively measuring wafer bonding strength according to any one of claims 1 to 5, characterized in that: The device for implementing the method includes: A working platform, which is used to place the two wafers that have been bonded, and the working platform has a vacuum adsorption or mechanical positioning device to fix the first wafer located below on the surface of the working platform; A pressure mechanism, which is located on the working platform and presses down the two wafers on the working platform; A tension mechanism, wherein the pressure mechanism is located on the working platform, and the tension mechanism acts on the second wafer located above to form an upward pulling force thereon; A spray mechanism, which is located on the side of the working platform; The detection device is an infrared detector or an ultrasonic detector.
Citation Information
Patent Citations
Method for measuring bonding strength and bonding wafer using the same
CN109524321A
Method of measuring an adhesive force of interlayer adhesive layer in tensile mode and apparatus
CN105938806A
Methods for processing a first substrate bonded to a second substrate
CN108353507A
Method and apparatus for testing interface bonding strength of layered composite material
CN108387445A
Testing method of wafer interface bonding energy
CN110231285A
Cited By
Wafer surface adhesion work statistical distribution characterization method based on force-distance curve
CN122545847A