Battery pole piece for performance test and preparation method thereof
By measuring and calculating the target roller pressure thickness, the electric roller pressure is gradually increased until the pole sheet is wavy, and whether its thickness meets the target range is determined, the compaction density test during the battery pole sheet rolling process in the prior art is solved. The cumbersome problems have achieved efficient preparation of extreme sheets.
Patent Information
- Application Number
- CN202411182661.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-27
AI Technical Summary
In the prior art, during the rolling process of battery pole sheets, the compaction density test method is cumbersome and low efficiency, which affects the preparation efficiency of battery pole sheets.
By measuring the initial pole sheet thickness, calculate the target roll pressure thickness, and gradually increase the pressure in the electric roller machine until the pole sheet is wavy, then measure the pole sheet thickness after the roll pressure to determine whether it meets the target thickness range, instead of the traditional Compact density testing method, using the compaction rate of the pole sheet for quick judgment.
The rolling efficiency is improved, the method is easy to operate, stable and efficient, simplifies the preparation process of the pole sheet and improves the preparation efficiency.
Smart Images

Figure CN119092630A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of pole piece testing technology, and in particular to a battery pole piece for performance testing and a preparation method thereof. Background Art
[0002] The performance of the pole piece is an important link in battery production. Its performance directly affects the stability of subsequent processes as well as the performance and safety of the battery cell. Therefore, the evaluation of the pole piece performance is particularly important. Among them, the pole piece resistivity and peel strength are important indicators for evaluating the pole piece performance and occupy an irreplaceable position in battery research and development and production.
[0003] Before the resistivity and peel strength test, it is necessary to take the positive / negative electrode sheets after rolling and cut the electrode sheets with a customized die cutter. At present, in the process of rolling the electrode sheets, in order to ensure that the electrode sheets reach the required compaction density, the battery negative electrode material electrode sheet compaction density test method disclosed in patent CN 107655791 A is usually used during the rolling process. This test method requires weighing the cut electrode sheets and current collectors, and measuring the thickness of the electrode sheets at three different positions after rolling at different pressures, and calculating through the electrode sheet surface density calculation formula and the compaction density calculation formula. It is not easy to operate, the process is cumbersome, and the rolling efficiency is low, which affects the preparation efficiency of battery electrodes. Summary of the invention
[0004] The embodiments of the present application provide a battery pole piece for performance testing and a method for preparing the same, aiming to improve the preparation efficiency of the battery pole piece.
[0005] To this end, according to one aspect of the present application, a method for preparing a battery electrode sheet for performance testing is provided, comprising the following steps:
[0006] S1. Use a tool knife to cut the coated and dried original electrode into electrode pieces with a specification of 30mm×300mm. Measure the thickness of each cut electrode piece at five different positions. Select the electrode piece with a thickness error of <2μm and take the average value of the thickness at five different positions as the initial electrode piece thickness d0. Calculate the target rolling thickness d according to the following formula 目标 :
[0007] d1≤d 目标 ≤d2
[0008] d1=(d0-d cf )·(100-(58-1))%+d cf
[0009] d2=(d0-d cf )·(100-(58+1))%+d cf
[0010] Where d0 is the initial pole piece thickness, d cf is the current collector thickness, and the target rolling thickness d 目标 Take the integer;
[0011] S2. Set the double roller linear speed of the electric roller machine to 2.0 m / min, and set the rolling pressure to 2 MPa as the starting value. After the pressure stabilizes, put the pole piece selected in step S1 into the electric roller machine for rolling. Increase the rolling pressure by 0.5 MPa in increments until the pole piece has wavy shapes on both sides and vertical lines appear in the middle of the pole piece.
[0012] S3. Use a micrometer to measure the thickness of the electrode at five different locations after rolling to meet the target rolling thickness d 目标 The pole pieces in which the difference in thickness between any two locations is less than 2 μm are qualified pole pieces.
[0013] Optionally, after step S3, the following steps are further included:
[0014] S4. Record the average value of the thickness at five different locations on the qualified electrode d 实 , calculate the actual compaction rate R according to the following formula 实 :
[0015] R 实 =1–{(d 实 -d cf )÷(d0-d cf )}·100%
[0016] Judge R 实 Is it within the range of 58%±1%? If so, it is qualified; otherwise, it is unqualified.
[0017] Optionally, in step S1, the drying condition is: placing in an oven at 110°C-130°C for 3 to 5 hours.
[0018] Optionally, in step S1, the drying condition is: placing in an oven at 120° C. for 4 hours.
[0019] Optionally, except for the drying in step S1, the rest of the battery pole piece preparation method is carried out under the conditions of 25±1° C. and humidity ≤60% RH.
[0020] According to another aspect of the present application, a battery pole piece for performance testing is provided, and the battery pole piece is prepared by the battery pole piece preparation method as described above.
[0021] The battery pole piece and the preparation method thereof for performance testing provided by the present application have the following beneficial effects: compared with the prior art, the battery pole piece and the preparation method thereof for performance testing of the present application use the battery pole piece compaction rate to replace the traditional compaction density test method to roll the pole piece, that is, firstly, the target compaction rate is calculated to be 58%±1% according to the target compaction density of the active material, and the target rolling thickness d of the pole piece is calculated according to the target compaction rate. 目标 In the subsequent rolling process, it is only necessary to compare the thickness of the electrode after rolling with the target rolling thickness d 目标 By comparison, it is possible to quickly determine whether the pole piece is qualified, which effectively improves the rolling efficiency. This method has the advantages of easy operation, good stability, speed and efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] in:
[0024] Figure 1 It is a schematic flow chart of a method for preparing a battery electrode sheet for performance testing according to an embodiment of the present application;
[0025] Figure 2 It is an average resistivity curve diagram of a battery electrode for performance testing provided by an embodiment of the present application during resistivity testing;
[0026] Figure 3 It is a graph showing the average peeling force of a battery electrode used for performance testing during a peeling strength test using an embodiment of the present application. DETAILED DESCRIPTION
[0027] The following is a preferred implementation of the embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the embodiment of the present invention. These improvements and modifications are also considered to be within the scope of protection of the embodiment of the present invention.
[0028] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.
[0029] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0030] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0032] According to one aspect of the present application, an embodiment of the present application provides a method for preparing a battery electrode for performance testing, such as Figure 1 As shown, the battery pole piece preparation method comprises the following steps:
[0033] S1. Use a tool knife to cut the coated and dried original electrode into electrode pieces with a specification of 30mm×300mm. Measure the thickness of each cut electrode piece at five different positions. Select the electrode piece with a thickness error of <2μm and take the average value of the thickness at five different positions as the initial electrode piece thickness d0. Calculate the target rolling thickness d according to the following formula 目标 :
[0034] d1≤d 目标 ≤d2
[0035] d1=(d0-d cf )·(100-(58-1))%+d cf
[0036] d2=(d0-d cf )·(100-(58+1))%+d cf
[0037] Where d0 is the initial pole piece thickness, d cf is the current collector thickness, and the target rolling thickness d 目标 Take the integer;
[0038] S2. Set the double roller linear speed of the electric roller machine to 2.0 m / min, and set the rolling pressure to 2 MPa as the starting value. After the pressure stabilizes, put the pole piece selected in step S1 into the electric roller machine for rolling. Increase the rolling pressure by 0.5 MPa in increments until the pole piece has wavy shapes on both sides and vertical lines appear in the middle of the pole piece.
[0039] S3. Use a micrometer to measure the thickness of the electrode at five different locations after rolling to meet the target rolling thickness d 目标 The pole pieces in which the difference in thickness between any two locations is less than 2 μm are qualified pole pieces.
[0040] Note: To ensure the accuracy of thickness measurement and the consistency of electrode preparation, except for the drying in step S1, the rest of the battery electrode preparation method is carried out under the conditions of 25±1℃ and humidity ≤60%RH.
[0041] Formula explanation:
[0042] Density calculation formula ρ=m / V=m / πr 2 h=m / πr 2 d, due to the mass m and area πr at the same position 2 The same, so the density ρ is only related to the thickness d.
[0043] Material Tap density / g / cm3 Compacted density / g / cm3 <![CDATA[True density / g / cm 3 > Natural graphite ≥0.9 ≥1.45 2.20-2.26 Mesophase carbon microspheres artificial graphite ≥1.1 ≥1.40 2.20-2.26 Needle coke artificial graphite ≥0.8 ≥1.40 2.20-2.26 Petroleum coke artificial graphite ≥1.0 ≥1.3 2.20-2.26 Composite graphite ≥0.8 ≥1.3 2.20-2.26
[0044] From the above table, we can conclude that the compacted density of various graphites is between 1.45-2.26 g / cm 3 In the range, the present invention takes 2.20g / cm 3 For the target compaction density, a qualified circular electrode with a diameter of r is cut out by a slicer, and its mass m1 and the mass m of the current collector after removing the active material are weighed. cf , through the formula ρ = m / πr 2 d is the target active material thickness d 目标 -d cf =(m1-m cf ) / πr 2 ρ, from which we can further derive the target compaction rate R0 = [1-(d 目标 -d cf ) / (d0-d cf )]·100%, after substituting the measured thickness, R0 is 58%, and the target compaction rate is 58%±1%.
[0045] In the embodiment of the present application, the battery pole piece and its preparation method for performance testing are used to roll the pole piece by replacing the traditional compaction density test method with the battery pole piece compaction rate, that is, firstly, the target compaction rate is calculated to be 58%±1% according to the target compaction density of the active material, and then the target rolling thickness d of the pole piece is calculated according to the formula in step S1 according to the target compaction rate. 目标 In the subsequent rolling process, it is only necessary to compare the thickness of the electrode after rolling with the target rolling thickness d 目标 By comparison, it is possible to quickly determine whether the pole piece is qualified, which effectively improves the rolling efficiency. This method has the advantages of easy operation, good stability, speed and efficiency.
[0046] In one embodiment, after step S3, the following steps are further included:
[0047] S4. Record the average value of the thickness at five different locations on the qualified electrode d 实 , calculate the actual compaction rate R according to the following formula 实 :
[0048] R 实 =1–{(d 实 -d cf )÷(d0-d cf )}·100%
[0049] Judge R 实 Is it within the range of 58%±1%? If so, it is qualified; otherwise, it is unqualified.
[0050] Step S4 is used to further verify whether the electrode is qualified, thereby improving the accuracy.
[0051] In one embodiment, in step S1, the drying condition is: placing in an oven at 110° C.-130° C. for 3 to 5 hours. Preferably, the drying condition is: placing in an oven at 120° C. for 4 hours.
[0052] In one embodiment, a comparison table of battery pole pieces prepared using the battery pole piece preparation method provided by the present application and the compaction density test method mentioned in the background art and subsequent test data is as follows:
[0053]
[0054] Data summary: combined Figure 2 and Figure 3, the average peeling force data and average resistivity data from experiment 2 to experiment 2 are stable, while the average resistance data from experiment 1 to experiment 2 decreases, and the average peeling force data from experiment 1 to experiment 2 increases. Experimental description: 1. The pole piece compaction rate reaches 58%±1%, and the compaction density is also in the maximum compaction density range. 2. When the compaction rate is 56%, the compaction density decreases significantly. 3. It is confirmed that the method of rolling the pole piece by using the pole piece compaction rate test method instead of the compaction density test method in the battery pole piece preparation method in the embodiment of the present application is stable and effective.
[0055] According to another aspect of the present application, an embodiment of the present application further provides a battery electrode sheet for performance testing, and the battery electrode sheet is prepared by the battery electrode sheet preparation method in any of the above embodiments.
[0056] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0057] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A method for preparing a battery pole piece for performance testing, characterized in that: The following steps are involved: S1. Use a tool knife to cut the coated and dried original electrode into electrode pieces with a specification of 30mm×300mm. Measure the thickness of each cut electrode piece at five different positions. Select the electrode piece with a thickness error of <2μm and take the average value of the thickness at five different positions as the initial electrode piece thickness d0. Calculate the target rolling thickness d according to the following formula 目标 : d1≤d 目标 ≤d2 d1=(d0-d cf )·(100-(58-1))%+d cf d2=(d0-d cf )·(100-(58+1))%+d cf Where d0 is the initial pole piece thickness, d cf is the current collector thickness, and the target rolling thickness d 目标 Take the integer; S2. Set the double roller linear speed of the electric roller machine to 2.0 m / min, and set the rolling pressure to 2 MPa as the starting value. After the pressure stabilizes, put the pole piece selected in step S1 into the electric roller machine for rolling. Increase the rolling pressure by 0.5 MPa in increments until the pole piece has wavy shapes on both sides and vertical lines appear in the middle of the pole piece. S3. Use a micrometer to measure the thickness of the electrode at five different locations after rolling to meet the target rolling thickness d 目标 The pole pieces in which the difference in thickness between any two locations is less than 2 μm are qualified pole pieces.
2. The method for preparing a battery pole piece according to claim 1, characterized in that: After step S3, the following steps are also included: S4. Record the average value of the thickness at five different locations on the qualified electrode d 实 , calculate the actual compaction rate R according to the following formula 实 : R 实 =1–{(d 实 -d cf )÷(d0-d cf )}·100% Judge R 实 Is it within the range of 58%±1%? If so, it is qualified; otherwise, it is unqualified.
3. The method for preparing a battery pole piece according to claim 1, characterized in that: In step S1, the drying condition is: placing in an oven at 110°C-130°C for 3 to 5 hours.
4. The method for preparing a battery pole piece according to claim 3, characterized in that: In step S1, the drying condition is: placing in an oven at 120° C. for 4 hours.
5. The method for preparing a battery pole piece according to claim 1, characterized in that: Except for the drying in step S1, the rest of the battery electrode preparation method is carried out under the conditions of 25±1° C. and humidity ≤60% RH.
6. A battery pole piece for performance testing, characterized in that: The battery pole piece is prepared by the battery pole piece preparation method as described in any one of claims 1 to 5.
Citation Information
Patent Citations
Method for testing compacted density of battery negative electrode material electrode sheet
CN107655791A
Method for determining ultimate compaction of positive pole piece of lithium ion battery
CN116046566A
Electrode plate thickness control method and control system
CN116060453A
Roller press closed-loop control method and system and roller press
CN117139384A
Battery pole piece rolling monitoring control method and rolling production equipment
CN118417335A
Cited By
Preparation method of secondary battery, secondary battery, energy storage system and electric equipment
CN120356904A