Preparation method of phosphoric acid and pyrophosphate ferric sodium composite positive electrode material

The high-pressure and high-temperature ethanol supercritical reaction with N-methylpyrrolidone coating addresses the limitations of polyanionic materials in sodium-ion batteries, ensuring complete reactions and preventing moisture absorption to enhance energy density and reduce costs.

CN119092670APending Publication Date: 2024-12-06无锡钠科能源科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411197818.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The preparation of polyanionic positive electrode materials for sodium-ion batteries faces issues such as incomplete reactions due to low heat treatment temperatures, water absorption leading to safety concerns, and low compaction resulting in reduced energy density and high costs.

Method used

A method involving high-pressure and high-temperature ethanol supercritical reaction followed by N-methylpyrrolidone coating is used to prepare a sodium iron phosphate pyrophosphate composite, enhancing molecular mixing, reducing water absorption, and increasing compaction density.

Benefits of technology

The method achieves stable structural integrity, improved electrochemical performance, and reduced battery cell costs by ensuring complete reactions and preventing moisture absorption, thereby enhancing energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092670A_ABST
    Figure CN119092670A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a phosphoric acid and pyrophosphate ferric sodium composite positive electrode material, and belongs to the technical field of sodium ion batteries. The preparation method comprises the following steps: S1, carrying out heat treatment, drying and crushing on a phosphorus source, an iron source, a sodium source, a carbon source and ethanol in a high-pressure reaction kettle to obtain a composite positive electrode material precursor; and S2, calcining the composite positive electrode material precursor and N-methyl pyrrolidone in a high-temperature furnace to obtain the phosphoric acid and ferric pyrophosphate composite positive electrode material. Absolute ethyl alcohol is adopted as a reaction medium, and a high-temperature and high-pressure ethyl alcohol supercritical reaction environment is created through a high-pressure reaction kettle, so that the energy density of the composite positive electrode material is improved, and the cell cost is reduced; n-methyl pyrrolidone is used for coating, so that the phosphate material is effectively prevented from absorbing moisture in air, and the damage of the moisture to the electrochemical performance of the material is avoided; in addition, uniform N doping is beneficial to rapid transfer of electrons, and the electron conductivity is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion batteries, and in particular relates to a method for preparing a sodium iron phosphate pyrophosphate composite positive electrode material. Background Art

[0002] Sodium-ion batteries are secondary batteries that rely on the movement of sodium ions between positive and negative electrodes to complete charging and discharging. Their working principle is similar to that of widely used lithium-ion batteries. With lithium resource supply facing bottlenecks and lithium-ion battery prices rising, sodium-ion batteries are favored because they are clean and environmentally friendly, have abundant raw material reserves, are widely distributed, are inexpensive, have higher safety, and have good high and low temperature performance. They have broad application prospects in power batteries, large-scale energy storage, and other fields.

[0003] In recent years, dozens of companies have emerged in China to promote the mass production of sodium-ion batteries and raw materials. They have achieved remarkable results in the research and development of key sodium-ion battery technologies, material preparation, battery production and application, and have ranked among the world's top. In terms of core technologies, China has mastered the production of sodium-ion soft-pack batteries, improved the energy density of sodium-ion batteries, and developed sodium-ion batteries with good low-temperature performance. The preparation and supply of positive and negative electrode materials for sodium-ion batteries have reached hundreds of tons. In terms of battery systems, Chinese companies have developed a lithium-sodium hybrid solution, which mixes sodium-ion batteries and lithium-ion batteries in a certain proportion and integrates them into the same battery system. This solution not only effectively solves the disadvantages of sodium-ion batteries in energy density, but also highlights the advantages of sodium-ion batteries in power and performance. In terms of technical applications, China has applied sodium-ion batteries in two-wheeled electric vehicles, A00-class electric vehicles and other fields. At present, the sodium-lithium hybrid batteries produced by Chinese companies have entered the stage of vehicle installation and trial, and the industrialization layout of sodium-ion batteries has been significantly accelerated.

[0004] Currently, the main positive electrode materials for sodium-ion batteries are layered oxides, polyanions, and Prussian blue. Polyanion materials are considered to be the most likely technology route for application in large-scale energy storage due to their naturally excellent structural stability and very low and abundant raw material costs.

[0005] At present, the preparation of polyanion-sodium iron phosphate pyrophosphate composite positive electrode materials has the following shortcomings: First, the mainstream process is sand milling and spraying, which uses sand milling to crush the raw materials to nanometer scale, and then uses spray drying to obtain NFPP precursor, and then heat treatment and solid phase synthesis of NFPP positive electrode materials are carried out. However, polyanion materials are limited by their raw materials themselves, and their heat treatment temperature cannot reach the layer oxygen level. Under low-temperature heat treatment, solid phase synthesis itself has great defects, namely, the reaction of phosphorus source, sodium source and iron source is incomplete, there are too many miscellaneous substances, and there are few active substances, and high electrochemical performance cannot be achieved. Second, because phosphate itself has strong water absorption, and the electrochemical performance of this material will decline significantly after absorbing water, excessive water content will also generate a large amount of hydrogen due to electrolysis reaction during the charge and discharge cycle, resulting in battery bulging, and safety cannot be guaranteed. Third, due to the low compaction of phosphate positive electrode materials, its energy density is reduced and the cost of battery cells remains high. Summary of the invention

[0006] To this end, the technical problem to be solved by the present invention is to overcome the problems that the solid phase mixing used in the preparation process of polyanionic positive electrode materials in the prior art cannot be mixed at the molecular level, resulting in uneven mixing and uneven material particle size and excessive particle size; the prepared polyanionic positive electrode material exhibits severe water absorption when exposed to air, thereby affecting the electrochemical properties of the material; the polyanionic positive electrode material has a low compaction, resulting in a decrease in its energy density and high battery cell costs.

[0007] In order to solve the above technical problems, the present invention provides a method for preparing a sodium iron phosphate pyrophosphate composite positive electrode material.

[0008] The object of the present invention is to provide a method for preparing a composite positive electrode material of sodium ferric phosphate pyrophosphate, comprising the following steps:

[0009] S1, phosphorus source, iron source, sodium source, carbon source and ethanol are heat treated, dried and crushed in a high-pressure reactor to obtain a composite positive electrode material precursor;

[0010] The composite positive electrode material precursor described in S2 and S1 and N-methylpyrrolidone are calcined in a high-temperature furnace to obtain the sodium iron phosphate pyrophosphate composite positive electrode material.

[0011] In one embodiment of the present invention, in S1, the phosphorus source is selected from one or more of diammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, phosphorus pentoxide, ammonium sodium hydrogen phosphate, pyrophosphoric acid, sodium pyrophosphate and hypophosphorous acid.

[0012] In one embodiment of the present invention, in S1, the iron source is selected from one or more of ferrous sulfate, ammonium ferrous sulfate, ammonium ferrous sulfate, ferrous oxalate, ferrous ammonium oxalate, ferrous oxide, ferric oxide, ferrous chloride, ferric hydroxide, ferric citrate, ammonium ferric citrate, ferric phosphate and ferric nitrate.

[0013] In one embodiment of the present invention, in S1, the sodium source is selected from one or more of sodium acetate, sodium hydroxide, sodium carbonate, sodium oxalate, sodium nitrite, disodium hydrogen phosphate, sodium bicarbonate, sodium citrate, anhydrous sodium sulfate, sodium stearate, sodium oleate, sodium tartrate, sodium alginate, sodium carboxymethyl cellulose, sodium lactate, sodium humate, sodium gluconate and sodium ascorbate.

[0014] In one embodiment of the present invention, in S1, the carbon source is selected from one or more of glucose, citric acid, PEG, ascorbic acid, isoascorbic acid, sodium isoascorbate, tea polyphenols and hydroquinone.

[0015] In one embodiment of the present invention, in S1, the heat treatment temperature is 200°C-350°C, the gas pressure is 6.0MPa-8.0MPa, and the time is 5h-10h.

[0016] In one embodiment of the present invention, in S1, the drying temperature is 120°C-150°C, and the drying time is 3h-6h.

[0017] In one embodiment of the present invention, in S1, the crushed particle size of the composite positive electrode material precursor after crushing is less than 80 μm.

[0018] In one embodiment of the present invention, in S2, the calcination temperature is 400°C-600°C, and the calcination time is 8h-20h.

[0019] In one embodiment of the present invention, the amounts of the phosphorus source, iron source and sodium source satisfy the chemical formula Na α Fe β (PO4)2P2O7, wherein α+2β=10; the molar ratio of the phosphorus source to the carbon source is 1:(0.5-3); the mass ratio of the carbon source to N-methylpyrrolidone is (1-5):1.

[0020] The technical solution of the present invention has the following advantages over the prior art:

[0021] (1) The preparation method of the present invention uses anhydrous ethanol as a reaction medium, and creates a high-temperature, high-pressure ethanol supercritical reaction environment through a high-pressure reactor. The ethanol supercritical reaction environment has both a high diffusion coefficient and low viscosity comparable to that of a gas, and a density similar to that of a liquid and a good solubility for substances. It allows substances that are usually difficult to dissolve or insoluble to dissolve and recrystallize. Under the conditions of high temperature and high pressure, solute molecules can quickly diffuse into solute molecules and reach the reaction site by penetration and migration. High temperature accelerates the reaction rate between the solute and the solvent, while high pressure increases the selectivity and yield of the reaction, achieving a stable structure and sufficient reaction effect that cannot be achieved by general synthetic processes. The composite positive electrode material precursor recrystallizes in a high-temperature and high-pressure environment, and its density reaches the maximum. By increasing the density, the compaction density is increased, thereby improving the energy density of the composite positive electrode material and reducing the cost of the battery cell.

[0022] (2) The preparation method described in the present invention uses N-methylpyrrolidone for coating, and the idea of ​​liquid coating solid is used to achieve full carbon coating on the surface of the composite positive electrode material precursor without defects, which can effectively hinder the phosphate material from absorbing moisture in the air and avoid moisture damage to the electrochemical properties of the material; in addition, the nitrogen element in N-methylpyrrolidone uniformly N-dopes the carbon coating layer during the calcination process, which helps the rapid transfer of electrons and effectively improves the electronic conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0024] Figure 1 This is an electron microscope image of the sodium iron phosphate pyrophosphate composite positive electrode material of Example 1 of the present invention;

[0025] Figure 2 This is an electron microscope image of the sodium iron phosphate pyrophosphate composite positive electrode material of Comparative Example 1 of the present invention;

[0026] Figure 3 The charge and discharge curves of button-type batteries made of the sodium iron phosphate pyrophosphate composite positive electrode materials of Example 1 of the present invention and Comparative Examples 1-2 at 0.1C. DETAILED DESCRIPTION

[0027] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. It should be understood that the specific embodiments are only used to explain the present invention, but the embodiments are not intended to limit the present invention.

[0028] In the present invention, unless otherwise explained, technical and scientific terms used in the present invention have the same meanings as commonly understood by those skilled in the art to which the present invention belongs.

[0029] In the present invention, unless otherwise stated, the term "and / or" used in the present invention includes any and all combinations of one or more of the associated listed items.

[0030] In the present invention, unless otherwise stated, the experimental methods used in the embodiments of the present invention are conventional methods unless otherwise stated, and the materials, reagents, etc. used are all commercially available unless otherwise stated.

[0031] In the present invention, unless otherwise stated, when the terms "comprise" and / or "include" are used in the specification of the present invention, it indicates the existence of the described features, integers, steps, operations, raw materials or components, but does not exclude the existence or addition of one or more other features, integers, steps, operations, raw materials, components or their combinations.

[0032] Example 1

[0033] The sodium iron phosphate pyrophosphate composite positive electrode material and the preparation method thereof of this embodiment specifically include the following steps:

[0034] S1. Add 23.0 g of ammonium dihydrogen phosphate, 21.6 g of ferrous oxalate, 10.6 g of sodium carbonate, and 36.0 g of glucose to 0.5 L of anhydrous ethanol to obtain a mixed solution;

[0035] S2, adding the mixed solution into a 1L autoclave, setting the temperature of the autoclave to 270°C, controlling the gas pressure at 8.0MPa after the temperature stabilizes, heat treating for 10h, cooling to room temperature, and then drying in an oven at 140°C for 5h, crushing and sieving to less than 80μm after cooling, to obtain a composite positive electrode material precursor;

[0036] S3. Fully mix the composite cathode material precursor with 30 g of N-methylpyrrolidone, then place it in a tube furnace, and calcine it at 500° C. for 18 h under a nitrogen atmosphere to obtain a sodium ferric phosphate pyrophosphate composite cathode material.

[0037] Comparative Example 1

[0038] The method is basically the same as Example 1, except that the mixed slurry solution is prepared and heat treated, and specifically includes the following steps:

[0039] S1. Add 23.0 g of ammonium dihydrogen phosphate, 21.6 g of ferrous oxalate, 10.6 g of sodium carbonate, and 36.0 g of glucose into 0.5 L of anhydrous ethanol, and grind by high-energy ball mill to obtain a mixed slurry solution;

[0040] S2. Drying and powdering the mixed slurry solution by spray drying equipment. The spray drying conditions are: drying chamber temperature of 450° C., feed rate of 350 mL / h, and discharge temperature of 100° C. to obtain a composite positive electrode material precursor.

[0041] S3. Fully mix the composite cathode material precursor with 30 g of N-methylpyrrolidone, then place it in a tube furnace, and calcine it at 500° C. for 18 h under a nitrogen atmosphere to obtain a sodium ferric phosphate pyrophosphate composite cathode material.

[0042] Comparative Example 2

[0043] The method is basically the same as Example 1, except that the supercritical ethanol method is not used, and specifically comprises the following steps:

[0044] S1. Add 23.0 g of ammonium dihydrogen phosphate, 21.6 g of ferrous oxalate, 10.6 g of sodium carbonate, and 36.0 g of glucose to 0.5 L of anhydrous ethanol to obtain a mixed solution;

[0045] S2. Add the mixed solution into a 1L hydrothermal reactor, place the hydrothermal reactor in a high-temperature furnace, set the temperature to 270°C, heat treat for 10 hours, cool to room temperature, and then place in a 140°C oven for drying for 5 hours. After cooling, crush and sieve to less than 80 μm to obtain a composite positive electrode material precursor;

[0046] S3. Fully mix the composite cathode material precursor with 30 g of N-methylpyrrolidone, then place it in a tube furnace, and calcine it at 500° C. for 18 h under a nitrogen atmosphere to obtain a sodium ferric phosphate pyrophosphate composite cathode material.

[0047] Comparative Example 3

[0048] The method is basically the same as Example 1, except that carbon coating is not performed, and specifically comprises the following steps:

[0049] S1. Add 23.0 g of ammonium dihydrogen phosphate, 21.6 g of ferrous oxalate, 10.6 g of sodium carbonate, and 36.0 g of glucose to 0.5 L of anhydrous ethanol to obtain a mixed solution;

[0050] S2, adding the mixed solution into a 1L autoclave, setting the temperature of the autoclave to 270°C, controlling the gas pressure at 8.0MPa after the temperature stabilizes, heat treating for 10h, cooling to room temperature, and then drying in an oven at 140°C for 5h, crushing and sieving to less than 80μm after cooling, to obtain a composite positive electrode material precursor;

[0051] S3. Place the composite cathode material precursor in a tubular furnace and calcine it at 500° C. for 18 h in a nitrogen atmosphere to obtain a sodium ferric phosphate pyrophosphate composite cathode material.

[0052] Comparative Example 4

[0053] The method is basically the same as Example 1, except that liquid carbon coating is not performed, and specifically comprises the following steps:

[0054] S1. Add 23.0 g of ammonium dihydrogen phosphate, 21.6 g of ferrous oxalate, 10.6 g of sodium carbonate, and 36.0 g of glucose to 0.5 L of anhydrous ethanol to obtain a mixed solution;

[0055] S2, adding the mixed solution into a 1L autoclave, setting the temperature of the autoclave to 270°C, controlling the gas pressure at 8.0MPa after the temperature stabilizes, heat treating for 10h, cooling to room temperature, and then drying in an oven at 140°C for 5h, crushing and sieving to less than 80μm after cooling, to obtain a composite positive electrode material precursor;

[0056] S3. The composite cathode material precursor was fully mixed with 27 g of glucose and 3 g of urea, and then placed in a tubular furnace, and calcined at 500° C. for 18 h under a nitrogen atmosphere to obtain a sodium ferric phosphate pyrophosphate composite cathode material.

[0057] Comparative Example 5

[0058] The method is basically the same as Example 1, except that N-doping is not performed, and specifically includes the following steps:

[0059] S1. Add 23.0 g of ammonium dihydrogen phosphate, 21.6 g of ferrous oxalate, 10.6 g of sodium carbonate, and 36.0 g of glucose to 0.5 L of anhydrous ethanol to obtain a mixed solution;

[0060] S2, adding the mixed solution into a 1L autoclave, setting the temperature of the autoclave to 270°C, controlling the gas pressure at 8.0MPa after the temperature stabilizes, heat treating for 10h, cooling to room temperature, and then drying in an oven at 140°C for 5h, crushing and sieving to less than 80μm after cooling, to obtain a composite positive electrode material precursor;

[0061] S3. The composite cathode material precursor was fully mixed with 30 g of PEG 400, and then placed in a tube furnace, and calcined at 500° C. for 18 h under a nitrogen atmosphere to obtain a sodium ferric phosphate pyrophosphate composite cathode material.

[0062] Comparative Example 6

[0063] The method is basically the same as Example 1, except that N doping is performed separately, and specifically includes the following steps:

[0064] S1. Add 23.0 g of ammonium dihydrogen phosphate, 21.6 g of ferrous oxalate, 10.6 g of sodium carbonate, and 36.0 g of glucose to 0.5 L of anhydrous ethanol to obtain a mixed solution;

[0065] S2, adding the mixed solution into a 1L autoclave, setting the temperature of the autoclave to 270°C, controlling the gas pressure at 8.0MPa after the temperature stabilizes, heat treating for 10h, cooling to room temperature, and then drying in an oven at 140°C for 5h, crushing and sieving to less than 80μm after cooling, to obtain a composite positive electrode material precursor;

[0066] S3. The composite cathode material precursor was fully mixed with 27 g PEG 400 and 3 g urea, and then placed in a tube furnace and calcined at 500° C. for 18 h under a nitrogen atmosphere to obtain a sodium ferric phosphate pyrophosphate composite cathode material.

[0067] Comparative Example 7

[0068] The method is basically the same as Example 1, except that 1,3-dimethyl-2-imidazolidinone is used for N-doping and coating, and specifically includes the following steps:

[0069] S1. Add 23.0 g of ammonium dihydrogen phosphate, 21.6 g of ferrous oxalate, 10.6 g of sodium carbonate, and 36.0 g of glucose to 0.5 L of anhydrous ethanol to obtain a mixed solution;

[0070] S2, adding the mixed solution into a 1L autoclave, setting the temperature of the autoclave to 270°C, controlling the gas pressure at 8.0MPa after the temperature stabilizes, heat treating for 10h, cooling to room temperature, and then drying in an oven at 140°C for 5h, crushing and sieving to less than 80μm after cooling, to obtain a composite positive electrode material precursor;

[0071] S3. Fully mix the composite cathode material precursor with 30 g of 1,3-dimethyl-2-imidazolidinone, then place in a tube furnace, and calcine at 500° C. for 18 h under a nitrogen atmosphere to obtain a sodium ferric phosphate pyrophosphate composite cathode material.

[0072] Test Example 1

[0073] The sodium iron phosphate pyrophosphate composite positive electrode materials prepared in Example 1 and Comparative Example 1 were characterized. Figure 1-Figure 2 As shown. Figure 1-Figure 2 It can be seen that compared with Example 1, the sodium iron phosphate pyrophosphate composite positive electrode material of Comparative Example 1 presents a loose and porous morphology, with a large number of voids inside. These voids have an adverse effect on compaction, resulting in too low compaction. The energy density of the material will also be reduced accordingly under the same volume, thereby pushing up the cost of the battery cell.

[0074] Test Example 2

[0075] The single-point compaction density test of 220 MPa was performed on the phosphate iron pyrophosphate nanocomposite positive electrode materials prepared in Example 1 and Comparative Examples 1-2 using a powder compaction density meter. The pressure was maintained for 10 seconds, and the obtained powder compaction data was recorded. The results are shown in Table 1:

[0076] Table 1

[0077] Sample <![CDATA[Bulk density g / cm 3 > Example 1 2.5 Comparative Example 1 2.0 Comparative Example 2 2.2

[0078] As can be seen from Table 1, the powder compaction density of the phosphate-iron-pyrophosphate composite cathode material prepared by the supercritical method is significantly greater than that of the phosphate-iron-pyrophosphate composite cathode material prepared by the sand mill spray and hydrothermal method. The reason is that the ethanol supercritical reaction environment has both a high diffusion coefficient and low viscosity comparable to that of gas, and a density similar to that of liquid and good solubility for substances. It makes the usually insoluble or insoluble substances dissolve and recrystallize, and the composite cathode material precursor recrystallizes in a high temperature and high pressure environment, and its density reaches the maximum, and the compaction density is increased by increasing the density.

[0079] Test Example 3

[0080] The sodium ferric phosphate pyrophosphate composite positive electrode material prepared in Example 1 and Comparative Examples 1-2 was made into a button cell to test the electrical performance, wherein the weight ratio of the positive electrode component was sodium ferric phosphate pyrophosphate composite positive electrode material: conductive agent (acetylene black): binder (PVDF) = 90:5:5; the negative electrode used a sodium sheet, the electrolyte was NaClO4, the test temperature of the button cell was 25°C, and the charge and discharge performance at 0.1C was as follows Figure 3 As shown. Figure 3 It can be seen that the phosphate pyrophosphate iron sodium composite positive electrode material prepared by the solid phase synthesis method of comparative example 1 has an electrochemical performance far lower than that of the material obtained by the ethanol supercritical synthesis method in embodiment 1. The solid phase synthesis method is difficult to achieve full reaction during the low temperature heat treatment of polyanions, and the yield of the target active substance is low. The limitation of the hydrothermal synthesis material of comparative example 2 is that, although anhydrous ethanol is used as a solvent and the conditions for heat treatment are performed, due to its insufficient pressure, the ethanol state is still liquid, and the high diffusion coefficient and low viscosity of the supercritical state of ethanol and the good solubility of the substance cannot be achieved, so the effect of embodiment 1 cannot be achieved. The ethanol supercritical reaction environment dissolves and recrystallizes the usually insoluble or insoluble substances. Under the conditions of high temperature and high pressure, the solute molecules can quickly diffuse into the solute molecules, reach the reaction site by penetration and migration, and the high temperature accelerates the reaction speed between the solute and the solvent, while the high pressure increases the selectivity and yield of the reaction, achieving the structural stability and sufficient reaction effect that the general synthesis process cannot do.

[0081] Test Example 4

[0082] Based on Test Example 3, the sodium iron phosphate pyrophosphate composite positive electrode materials prepared in Example 1 and Comparative Examples 1-7 were made into button batteries to test the electrical performance. The results are shown in Table 2:

[0083] Table 2

[0084]

[0085]

[0086] As can be seen from Table 2, compared with Example 1, the moisture content of the carbon-free phosphate pyrophosphate sodium iron composite positive electrode material in Comparative Example 3 reaches more than 3000ppm after sintering and crushing. This is because the phosphate material itself has a strong water absorption. When exposed to the air after sintering, the dry material will absorb moisture in the air, resulting in an increase in water content, and the increase in water content will have a serious negative impact on the electrochemical performance of the material. Compared with Example 1, in Comparative Examples 4-5, the water content of the material does show a downward trend compared to the uncoated case when the material is solid-phase carbon-coated, but it still reaches more than 1000ppm; and when the material is liquid carbon-coated, the water content of the material decreases significantly, reaching less than 1000ppm. The reason is that when the material is coated with a liquid carbon source, the liquid carbon source can fully wrap the surface of the material, and will be evenly coated on the surface of the material during the high-temperature carbonization process. Since the carbon material itself has excellent hydrophobicity and is evenly and fully carbon-coated, It can prevent the internal material from contacting with moisture in the air, thereby achieving the effect of reducing the moisture content of the material; and the first charge and discharge specific capacity of the material in Example 1 is higher than that in Comparative Example 5, and the rate performance of the material at 0.1C\0.5\1.0C is much higher. This is because Example 1 uses N-containing carbon source N-methylpyrrolidone. During the high-temperature sintering process, the N-containing N-methylpyrrolidone is carbonized and carbonized into a complete and uniform N-doped carbon layer. Successfully doping N into the carbon layer can produce additional active sites, which helps to improve the capacity and rate performance of the electrode material. Compared with Example 1, Comparative Example 6 has a lower first charge and discharge specific capacity, first efficiency and rate performance of the obtained material than that in Example 1 because the additionally added N source cannot form a complete and uniform N-doped carbon layer. Comparative Example 7 Compared with Example 1, the NFPP sodium ion positive electrode material is weakly alkaline. Due to the urea structure, the conjugation effect of 1,3-dimethyl-2-imidazolidinone reduces the dipole and reduces the carbonyl reaction activity. On the other hand, the five atoms on the ring are coplanar, which reduces the chance of nucleophilic reagents entering the ring to attack the carbonyl group. Therefore, 1,3-dimethyl-2-imidazolidinone has a higher boiling point and stability than N-methylpyrrolidone under high temperature alkaline conditions, and will not decompose rapidly, resulting in the coating layer being unable to be fully carbonized to form a complete carbon coating. In addition, the residual 1,3-dimethyl-2-imidazolidinone will also hinder the rapid transfer of electrons, reducing the electronic conductivity.

[0087] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for preparing a sodium ferric phosphate pyrophosphate composite positive electrode material, characterized in that: The following steps are involved: S1, phosphorus source, iron source, sodium source, carbon source and ethanol are heat treated, dried and crushed in a high-pressure reactor to obtain a composite positive electrode material precursor; The composite positive electrode material precursor described in S2 and S1 and N-methylpyrrolidone are calcined in a high-temperature furnace to obtain the sodium iron phosphate pyrophosphate composite positive electrode material.

2. The method for preparing the sodium iron phosphate pyrophosphate composite positive electrode material according to claim 1, characterized in that: In S1, the phosphorus source is selected from one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, phosphorus pentoxide, ammonium sodium hydrogen phosphate, pyrophosphoric acid, sodium pyrophosphate and hypophosphorous acid.

3. The method for preparing the sodium iron phosphate pyrophosphate composite positive electrode material according to claim 1, characterized in that: In S1, the iron source is selected from one or more of ferrous sulfate, ammonium ferrous sulfate, ammonium ferrous sulfate, ferrous oxalate, ferrous ammonium oxalate, ferric oxide, ferric oxide, ferrous chloride, ferric hydroxide, ferric citrate, ammonium ferric citrate, ferric phosphate and ferric nitrate.

4. The method for preparing the sodium iron phosphate pyrophosphate composite positive electrode material according to claim 1, characterized in that: In S1, the sodium source is selected from one or more of sodium acetate, sodium hydroxide, sodium carbonate, sodium oxalate, sodium nitrite, disodium hydrogen phosphate, sodium bicarbonate, sodium citrate, anhydrous sodium sulfate, sodium stearate, sodium oleate, sodium tartrate, sodium alginate, sodium carboxymethyl cellulose, sodium lactate, sodium humate, sodium gluconate and sodium ascorbate.

5. The method for preparing the sodium iron phosphate pyrophosphate composite positive electrode material according to claim 1, characterized in that: In S1, the carbon source is selected from one or more of glucose, citric acid, PEG, ascorbic acid, isoascorbic acid, sodium isoascorbate, tea polyphenols and hydroquinone.

6. The method for preparing the sodium iron phosphate pyrophosphate composite positive electrode material according to claim 1, characterized in that: In S1, the heat treatment temperature is 200°C-350°C, the gas pressure is 6.0MPa-8.0MPa, and the time is 5h-10h.

7. The method for preparing the sodium iron phosphate pyrophosphate composite positive electrode material according to claim 1, characterized in that: In S1, the drying temperature is 120°C-150°C, and the drying time is 3h-6h.

8. The method for preparing the sodium iron phosphate pyrophosphate composite positive electrode material according to claim 1, characterized in that: In S1, the crushed particle size of the composite positive electrode material precursor is less than 80 μm.

9. The method for preparing the sodium iron phosphate pyrophosphate composite positive electrode material according to claim 1, characterized in that: In S2, the calcination temperature is 400°C-600°C, and the calcination time is 8h-20h.

10. The method for preparing the sodium iron phosphate pyrophosphate composite positive electrode material according to claim 1, characterized in that: The amounts of the phosphorus source, iron source and sodium source satisfy the chemical formula Na α Fe β (PO4)2P2O7, wherein α+2β=10; the molar ratio of the phosphorus source to the carbon source is 1:(0.5-3); the mass ratio of the carbon source to N-methylpyrrolidone is (1-5):1.