Positive electrode slurry and preparation method thereof, positive plate and preparation method thereof, and battery

By using LiPF6 to coat the residual lithium on the surface of the ternary positive electrode material during the homogenization process, a fast ion conductor coating layer is generated, which solves the problems of insufficient conductivity and incomplete coating of the ternary positive electrode material, and achieves higher electrical power Chemical properties and lower costs.

CN119092678APending Publication Date: 2024-12-06BATTERO TECH CORP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411211767.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing ternary positive electrode materials have insufficient conductivity or incomplete coating and high cost.

Method used

During the homogenization process, add an appropriate amount of LiPF6 and react with residual lithium on the surface of the ternary positive electrode material to form fast ion conductors such as Li3PO4 and LiF coated on the surface of the ternary positive electrode material particles to enhance the conductivity of the material surface and reduce side reactions, and through uniformity, The fast ion conductor cladding improves electrochemical properties.

Benefits of technology

It extends battery life, improves the electrochemical performance of the material, uniformity and consistency of the coating, simpler operation and lower cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092678A_ABST
    Figure CN119092678A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of battery materials, and discloses positive electrode slurry and a preparation method thereof, a positive plate and a preparation method thereof, and a battery. The preparation method comprises the following steps: uniformly mixing and dispersing a ternary positive electrode material, a conductive agent, an adhesive, a solvent and LiPF6 to prepare the positive electrode slurry; and the mass ratio of the LiPF6 to the ternary positive electrode material is (0.01-10): 100. According to the positive electrode slurry prepared by the preparation method provided by the invention, the LiPF6 is added, and the LiPF6 reacts with residual lithium to generate fast ion conductors such as Li3PO4 and LiF to coat the surfaces of ternary positive electrode material particles, so that the effects of improving the surface conductivity of the material, reducing the side reaction of the material and an electrolyte and improving the cycle performance can be achieved, and the service life of a battery can be prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a positive electrode slurry and a preparation method thereof, a positive electrode sheet and a preparation method thereof, and a battery. Background Art

[0002] Conventional ternary slurries have problems such as poor cycle life and large surface impedance, and high-temperature cycles can only reach about 1,000 cycles.

[0003] The existing technology improves the surface conductivity of the material by removing residual lithium from the material end, doping or coating with additives with good conductivity, etc. This method can improve the conductivity of the material and thus improve the electrical performance, but there are still problems such as incomplete surface point coating and high ALD coating cost.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a positive electrode slurry and a preparation method thereof, a positive electrode sheet and a preparation method thereof, and a battery, aiming to improve the current problems of poor surface conductivity of ternary materials or incomplete surface coating of ternary materials and high cost.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides a method for preparing a positive electrode slurry, comprising:

[0008] The ternary positive electrode material, the conductive agent, the adhesive, the solvent and LiPF6 are mixed and dispersed uniformly to prepare a positive electrode slurry;

[0009] The mass ratio of LiPF6 to the ternary positive electrode material is 0.01:100 to 10:100.

[0010] In an optional embodiment, the feeding amounts are calculated by weight: the ternary positive electrode material is 90 to 99 parts, the conductive agent is 0.5 to 5 parts, the adhesive is 0.5 to 5 parts, and LiPF6 is 0.009 to 9.9 parts.

[0011] In an optional embodiment, the solid content of the positive electrode slurry is 40-80%.

[0012] In an optional embodiment, the chemical formula of the ternary cathode material is Li 1+z Ni a A b Co 1-(a+b) O2, wherein A is selected from at least one of Mn and Al, 0≤z≤0.1, 0.1≤a≤0.8, 0.1≤b≤0.8, a+b<1.

[0013] In an optional embodiment, the conductive agent is selected from at least one of conductive carbon black, carbon nanotubes and graphene.

[0014] In an optional embodiment, the adhesive is selected from at least one of PVDF, polytetrafluoroethylene, CMC and PAA.

[0015] In an optional embodiment, the solvent is selected from at least one of N-methylpyrrolidone, acetone and ethanol.

[0016] In an optional embodiment, the LiPF6 used to prepare the positive electrode slurry is in powder form with a particle size of 10 to 1000 nm.

[0017] In an optional embodiment, the uniformly dispersed operation method is:

[0018] Place all raw materials in a mixer and disperse them at a linear speed of 1 to 50 m / s for 15 to 600 min.

[0019] In a second aspect, the present invention provides a positive electrode slurry, which is prepared by the preparation method of any one of the aforementioned embodiments.

[0020] In a third aspect, the present invention provides a method for preparing a positive electrode sheet, comprising applying the positive electrode slurry according to the aforementioned embodiment to the surface of a current collector and then rolling the resultant.

[0021] In a fourth aspect, the present invention provides a positive electrode sheet, which is prepared by the preparation method as described in the above embodiment.

[0022] In a fifth aspect, the present invention provides a battery, comprising a positive electrode sheet as described in the aforementioned embodiment.

[0023] The present invention has the following beneficial effects:

[0024] The preparation method provided by the present invention can improve the surface conductivity of the material, reduce the side reaction between the material and the electrolyte, and achieve the effect of improving the cycle, which helps to extend the battery life. Since the preparation method adds LiPF6 during the homogenization process, the coating layer formed on the surface of the ternary positive electrode material can be uniform in thickness and good in consistency, thereby further improving the electrochemical performance of the material; in addition, the preparation method can form a uniform fast ion conductor coating layer on the surface of the ternary positive electrode material by adding LiPF6 during the homogenization process. Compared with the current positive electrode material with a fast ion conductor coating layer prepared by sintering, the coating uniformity is better, the operation method is simpler and more convenient, and the manufacturing cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0026] Figure 1 This is a comparison chart of the high temperature cycle performance of the positive electrode sheets prepared in Example 1 and Comparative Example 2 after being assembled into batteries. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0028] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0029] The positive electrode slurry and its preparation method, the positive electrode and its preparation method, and the battery provided in the embodiments of the present invention are described in detail below.

[0030] An embodiment of the present invention provides a method for preparing a positive electrode slurry, comprising:

[0031] The ternary positive electrode material, the conductive agent, the adhesive, the solvent and LiPF6 are mixed and dispersed uniformly to prepare a positive electrode slurry;

[0032] The mass ratio of LiPF6 to the ternary positive electrode material is 0.01 to 10:100 (for example, 0.01:100, 0.1:100, 1:100, 2:100, 5:100 or 10:100).

[0033] The amount of lithium source added during the preparation of ternary positive electrode materials is usually excessive, so there is residual lithium in the finished ternary positive electrode material. The preparation method provided by the present invention adds an appropriate amount of LiPF6 during the homogenization process to react with the residual lithium on the surface of the ternary positive electrode material to generate fast ion conductors such as Li3PO4 and LiF that are coated on the surface of the ternary positive electrode material particles. This can improve the conductivity of the material surface, reduce the side reactions between the material and the electrolyte, and thus improve the cycle performance, which helps to extend the battery life. Since this preparation method adds LiPF6 during the homogenization process, the coating layer formed on the surface of the ternary positive electrode material can be uniform in thickness and consistency, thereby further improving the electrochemical properties of the material; in addition, if Figure 1 As shown, Figure 1The left picture in the middle shows the surface state of the positive electrode material particles in the traditional slurry, and the right picture shows the surface state of the positive electrode material particles in the slurry of the preparation method provided in this application. This preparation method can form a uniform fast ion conductor coating layer on the surface of the ternary positive electrode material by adding LiPF6 during the homogenization process. Compared with the current positive electrode material with a fast ion conductor coating layer deliberately prepared by sintering, it has better coating uniformity, simpler and more convenient operation, and lower manufacturing cost.

[0034] It should be noted that the amount of LiPF6 added should not be too much. Too much LiPF6 will absorb water and decompose, resulting in loss of activity. Therefore, the added amount within the range required by this application can obtain a positive electrode slurry with better electrochemical performance.

[0035] Specifically, the ternary positive electrode material, the conductive agent, the adhesive, the solvent and LiPF6 are uniformly mixed and dispersed in the following manner:

[0036] First, the ternary cathode material, the conductive agent, the adhesive and the LiPF6 dry powder are uniformly mixed, and then the uniformly mixed dry powder is mixed with the solvent and dispersed uniformly;

[0037] Alternatively, the ternary positive electrode material, the conductive agent and the binder are first dry-mixed to obtain a mixed dry powder, and LiPF6 is mixed with a small amount of solvent to obtain LiPF6 slurry; the mixed dry powder, LiPF6 slurry and the remaining solvent are mixed and dispersed uniformly;

[0038] Alternatively, a wet stirring process is used to prepare PVDF and a conductive agent in a certain proportion into a prefabricated slurry, and then the ternary positive electrode material, LiPF6 and a solvent are added and mixed and dispersed evenly.

[0039] Preferably, in order to ensure that each solid material can be fully and evenly dispersed in the solvent, the mixing and dispersion process of the ternary positive electrode material, conductive agent, adhesive, LiPF6 and solvent is carried out in a mixer, and the linear speed is set to 1 to 50 m / s (for example, 1 m / s, 5 m / s, 10 m / s, 30 m / s or 50 m / s), and the dispersion time is 15 to 600 min (for example, 15 min, 60 min, 120 min, 180 min, 240 min, 480 min or 600 min).

[0040] Optionally, to ensure that the prepared positive electrode slurry has better electrochemical properties, the feeding amounts are calculated by weight: 90 to 99 parts of ternary positive electrode material, 0.5 to 5 parts of conductive agent, 0.5 to 5 parts of adhesive, and 0.009 to 9.9 parts of LiPF6.

[0041] Optionally, to ensure that the positive electrode slurry has better fluidity for subsequent coating and rolling operations, the solid content of the positive electrode slurry is 40-80% (eg, 40%, 60% or 80%).

[0042] Optionally, the chemical formula of the ternary cathode material is Li 1+z Ni a A b Co 1-(a+b) O2, wherein A is selected from at least one of Mn and Al, 0≤z≤0.1, 0.1≤a≤0.8, 0.1≤b≤0.8, a+b<1.

[0043] Optionally, the conductive agent is selected from at least one of conductive carbon black, carbon nanotubes and graphene.

[0044] Optionally, the adhesive is selected from at least one of PVDF (polyvinylidene fluoride), polytetrafluoroethylene, CMC (carboxymethyl cellulose) and PAA (polyacrylic acid).

[0045] Optionally, the solvent is selected from at least one of NMP (N-methylpyrrolidone), acetone and ethanol.

[0046] Preferably, the particle size of the ternary positive electrode material used to prepare the positive electrode sheet is 0.2μm to 20μm. In order to enable LiPF6 to form a uniform fast ion conductor coating layer on the surface of the positive electrode material, the LiPF6 used to prepare the positive electrode slurry is in powder form with a particle size of 10 to 1000nm.

[0047] The positive electrode slurry provided in the embodiment of the present invention is prepared by the preparation method provided in the embodiment of the present invention. The positive electrode sheet prepared by the slurry has better cycle performance after being assembled into a battery.

[0048] The method for preparing a positive electrode sheet provided in an embodiment of the present invention comprises applying the positive electrode slurry provided in an embodiment of the present invention to the surface of a current collector and then rolling the surface of the current collector.

[0049] The positive electrode sheet provided in the embodiment of the present invention is prepared by the preparation method provided in the embodiment of the present invention.

[0050] The battery provided by the embodiment of the present invention includes the positive electrode sheet provided by the embodiment of the present invention.

[0051] Example 1

[0052] The chemical formula is LiNi 0.9 Mn 0.05 Co 0.05 90Kg of O2 ternary positive electrode material, 5Kg of conductive agent (conductive carbon black), 4.991Kg of binder (PVDF), 0.009Kg of LiPF6 powder and 150Kg of solvent (N-methylpyrrolidone) were placed in a mixer, the linear speed was set to 30m / s, and the positive electrode slurry was obtained after dispersion for 200min.

[0053] The particle size of the ternary positive electrode material is 0.2~20μm, the particle size of LiPF6 powder is 10~1000nm, and D50 is 150nm.

[0054] The positive electrode slurry is coated on aluminum foil, and then dried and rolled to obtain a positive electrode sheet.

[0055] Example 2

[0056] The chemical formula is LiNi 0.9 Mn 0.05 Co 0.05 99Kg of O2 ternary positive electrode material, 0.5Kg of conductive agent (conductive carbon black), 0.5Kg of binder (PVDF), 9.9Kg of LiPF6 and 37.5Kg of solvent (N-methylpyrrolidone) were placed in a mixer, the linear speed was set to 30m / s, and the positive electrode slurry was obtained after dispersion for 200min.

[0057] The particle size of the ternary positive electrode material is 0.2~20μm, the particle size of LiPF6 powder is 10~1000nm, and D50 is 150nm.

[0058] The positive electrode slurry is coated on aluminum foil, and then dried and rolled to obtain a positive electrode sheet.

[0059] Example 3

[0060] The chemical formula is LiNi 0.9 Mn 0.05 Co 0.05 95 kg of O2 ternary positive electrode material, 1 kg of conductive agent (conductive carbon black), 1 kg of binder (PVDF), 9.5 kg of LiPF6 and 106.5 kg of solvent (N-methylpyrrolidone) were placed in a mixer, the line speed was set to 30 m / s, and the positive electrode slurry was obtained after dispersion for 200 min.

[0061] The particle size of the ternary positive electrode material is 0.2~20μm, the particle size of LiPF6 powder is 10~1000nm nm, and D50 is 150nm.

[0062] The positive electrode slurry is coated on aluminum foil, and then dried and rolled to obtain a positive electrode sheet.

[0063] Example 4

[0064] The chemical formula is LiNi 0.9 Mn 0.05 Co 0.05 93Kg of O2 ternary positive electrode material, 3Kg of conductive agent (conductive carbon black), 2Kg of binder (PVDF), 2Kg of LiPF6 and 67Kg of solvent (N-methylpyrrolidone) were placed in a mixer, the linear speed was set to 30m / s, and the positive electrode slurry was obtained after dispersion for 200min.

[0065] The particle size of the ternary positive electrode material is 0.2~20μm, the particle size of LiPF6 powder is 10~1000nm nm, and D50 is 150nm.

[0066] The positive electrode slurry is coated on aluminum foil, and then dried and rolled to obtain a positive electrode sheet.

[0067] Comparative Example 1

[0068] This comparative example is basically the same as Example 1, except that LiPF6 is not added.

[0069] Comparative Example 2

[0070] This comparative example is basically the same as Example 1, except that an equal amount of ternary positive electrode material is used to replace LiPF6.

[0071] Comparative Example 3

[0072] This comparative example is basically the same as Example 2, except that 20 kg of LiPF6 is added.

[0073] Comparative Example 4

[0074] This comparative example is basically the same as Example 3, except that: the ternary positive electrode material and LiPF6 are replaced by an equal amount of a ternary positive electrode material having a Li3PO3 fast ion conductor coating layer;

[0075] The ternary positive electrode material having a Li3PO3 fast ion conductor coating layer is prepared by the following method:

[0076] The matrix and the Li3PO3 fast ion conductor additive are mixed evenly and then sintered to obtain a ternary positive electrode material with a Li3PO3 fast ion conductor coating layer. The ratio of Li3PO3 to the ternary positive electrode material is exactly the same as that in Example 3.

[0077] Experimental example

[0078] The positive electrode sheets prepared in Examples 1-4 and Comparative Examples 1-3 were assembled into soft-pack batteries together with graphite negative electrode sheets, separators (PP), and electrolytes [1MLiPF6+EC:EMC(3:7wt)+3%FEC+0.5%VC].

[0079] The battery's 25℃ specific capacity, cycle performance, and rate performance were tested at 4.2-2.8V and 25℃, and the test results were recorded in Table 1 and Figure 1 middle.

[0080] Table 1 Performance of the positive electrode sheets prepared in various embodiments and comparative examples

[0081] Group capacity Cycle performance 3C rate Example 1 210.2mAh / g 500 weeks 95% 95.1% Example 2 207.7mAh / g 500 weeks 93% 97.3% Example 3 208.5mAh / g 500 weeks 96% 96.8% Example 4 210.9mAh / g 500 weeks 97% 95.7% Comparative Example 1 209.8mAh / g 500 weeks 94% 94.7% Comparative Example 2 208.3mAh / g 500 weeks 89% 94.5% Comparative Example 3 207.1mAh / g 500 weeks 97% 94.1% Comparative Example 4 209.3mAh / g 500 weeks 94% 94.9%

[0082] from Figure 1 As can be seen from Table 1, the multiple embodiments provided by the present invention all have a better capacity retention rate.

[0083] Comparing Example 1 with Comparative Example 1 and Comparative Example 2, the capacity retention rate of Example 1 is significantly higher than that of Comparative Example 1 and Comparative Example 2, which indicates that adding LiPF6 to the positive electrode slurry provided by the present invention has a higher capacity retention rate than conventional positive electrode slurry.

[0084] Comparing Example 1 with Comparative Example 3, the specific capacity and 3C rate performance of Comparative Example 3 are significantly worse, indicating that too much LiPF6 should not be added, as too much addition will reduce the specific capacity and rate performance.

[0085] Comparing Example 1 with Comparative Example 4, the specific capacity, cycle performance and 3C rate of Example 1 are not inferior to those of Comparative Example 4, which indicates that the performance of the positive electrode slurry prepared by adding LiPF6 during the homogenization of the positive electrode slurry provided by the present invention is not inferior to the performance of the positive electrode slurry obtained by directly sintering the ternary positive electrode material with a fast ion conductor coating layer.

[0086] In summary, the preparation method provided by the present invention can improve the conductivity of the material surface, reduce the side reaction between the material and the electrolyte, and thus improve the cycle performance, which helps to extend the battery life by adding an appropriate amount of LiPF6 during the homogenization process to react with the residual lithium on the surface of the ternary positive electrode material to generate fast ion conductors such as Li3PO4 and LiF to coat the surface of the ternary positive electrode material particles. This can improve the conductivity of the material surface, reduce the side reaction between the material and the electrolyte, and thus improve the cycle performance, which helps to extend the battery life. Since the preparation method adds LiPF6 during the homogenization process, the coating layer formed on the surface of the ternary positive electrode material can be uniform in thickness and consistency, thereby further improving the electrochemical performance of the material; in addition, the preparation method can form a uniform fast ion conductor coating layer on the surface of the ternary positive electrode material by adding LiPF6 during the homogenization process. Compared with the current preparation of positive electrode materials with fast ion conductor coating layers by sintering, the coating uniformity is better, the operation method is simpler and more convenient, and the manufacturing cost is low.

[0087] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a positive electrode slurry, characterized in that: include: The ternary positive electrode material, the conductive agent, the adhesive, the solvent and LiPF6 are mixed and dispersed uniformly to prepare a positive electrode slurry; The mass ratio of LiPF6 to the ternary positive electrode material is 0.01 to 10:

100.

2. The preparation method according to claim 1, characterized in that: The feeding amounts are calculated by weight: the ternary positive electrode material is 90 to 99 parts, the conductive agent is 0.5 to 5 parts, the adhesive is 0.5 to 5 parts, and LiPF6 is 0.009 to 9.9 parts.

3. The preparation method according to claim 1, characterized in that: The solid content of the positive electrode slurry is 40-80%.

4. The preparation method according to claim 1, characterized in that: The chemical formula of the ternary cathode material is Li 1+ z Ni a A b Co 1-(a+b) O2, wherein A is selected from at least one of Mn and Al, 0≤z≤0.1, 0.1≤a≤0.8, 0.1≤b≤0.8, a+b<1; Optionally, the conductive agent is selected from at least one of conductive carbon black, carbon nanotubes and graphene; Optionally, the adhesive is selected from at least one of PVDF, polytetrafluoroethylene, CMC and PAA; Optionally, the solvent is selected from at least one of N-methylpyrrolidone, acetone and ethanol.

5. The preparation method according to claim 1, characterized in that: The LiPF6 used to prepare the positive electrode slurry is in powder form, and its particle size is 10 to 1000 nm.

6. The preparation method according to claim 1, characterized in that: The operation method for uniform dispersion is: Place all raw materials in a mixer and disperse them at a linear speed of 1 to 50 m / s for 15 to 600 min.

7. A positive electrode slurry, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 6.

8. A method for preparing a positive electrode sheet, characterized in that: The method comprises coating the positive electrode slurry as claimed in claim 7 onto the surface of the current collector and then drying and rolling it.

9. A positive electrode sheet, characterized in that: The method is prepared according to claim 8.

10. A battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 9.