Polycrystalline ultrahigh-nickel ternary positive electrode material and preparation method and application thereof
By using core layers doped with metal elements A and B and shell layers of cobalt and boron in ultra-high nickel ternary positive electrode materials, the problem of removing soluble lithium is solved, and the structural stability and electrochemical performance of the material are improved. , achieving environmentally friendly and efficient production.
Patent Information
- Application Number
- CN202411555908.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-04
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-11-04
AI Technical Summary
The existing ultra-high nickel ternary cathode materials require water washing to remove soluble lithium during the production process, resulting in structural instability, increasing safety risks, and the lithium-nickel mixed discharge cannot be avoided, affecting the circulation performance.
The core layer doped with metal elements A and metal elements B, combined with the shell layer of cobalt and boron, is prepared by sintering process to avoid water washing and enhance the structural stability and electrical properties of the material. Chemical properties.
Achieves a polycrystalline ultra-high nickel ternary cathode material with low soluble lithium content, improves the circulation performance and stability of the material, reduces the corrosion of the electrolyte on the material, enhances the electrochemical performance, and is environmentally friendly and does not require a water washing process to generate waste water. .
Smart Images

Figure CN119092694A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of new energy technology, and in particular to a polycrystalline ultra-high nickel ternary positive electrode material and a preparation method and use thereof. Background Art
[0002] Ultra-high nickel ternary cathode materials generally refer to ternary cathode materials with a high nickel content. Under current technical conditions, the high nickel ternary technology route has become the preferred choice for developing high-capacity batteries. As the nickel content increases, the energy density of ternary batteries will also increase significantly. At the same time, high nickel ternary cathode materials increase the proportion of relatively cheap nickel and also have certain advantages in terms of cost.
[0003] However, there are also some challenges and problems with ultra-high nickel ternary cathode materials. High nickel content can lead to lithium-nickel mixing, which can cause lithium precipitation and poor cycle performance. Traditional polycrystalline NCM particles are composed of submicron primary grains with random orientation, which can lead to Li + The diffusion path is enriched, and the Li concentration inside the particles is uneven, which in turn causes stress / strain concentration and final internal cracks along the grain boundaries. At the same time, the ratio of Ni, Co, and Mn in the ultra-high nickel ternary positive electrode material is biased towards Ni, resulting in less Mn elements as a support, making its structure more unstable.
[0004] Based on this, due to Li + Diffusion path enrichment makes the surface of ultra-high nickel materials have more soluble lithium. If it is not consumed or removed, the soluble lithium on the surface of the material will undergo a series of side reactions with the electrolyte after the material is made into a battery, resulting in battery bulging and increasing the occurrence of serious safety problems. The industry generally uses the high-nickel 8 series water washing process to reduce the soluble lithium on the surface of the material through water washing, but the structure of the ultra-high nickel material itself is unstable. During the water washing process, the H + Will react with Li in the material + Positional interchange occurs, resulting in structural lithium precipitation and material structure collapse.
[0005] In this regard, prior art 1: Chinese patent application 202410944242.X discloses a ternary positive electrode material and a preparation method thereof, comprising the following steps: lithium salt, a ternary precursor (Ni x Co y Mn z (OH2) and a metal compound containing element A are mixed to obtain a mixture; the mixture obtained in step 1 is sintered once to obtain a primary sintered material; the primary sintered material obtained in step 2 is crushed to obtain a powder; finally, the powder obtained in step 3 is mixed with a metal compound containing element B and then sintered twice to obtain a ternary positive electrode material; by improving the doping and coating processes, the residual lithium content on the surface of the positive electrode material is reduced; Further observing the specification of this solution, it can be seen that the doping element used is element A, specifically one or more of Zr, B, W, Ti, and Y, and element A at least includes Zr; The coating element used is element B, specifically one or more of Co, Ti, W, and Al, and element B at least includes Co; Among them, in paragraph 11 of the specification of this solution, the functions of the doping element A and the coating element B are described in relatively more detail. Specifically, "doping the metal element A can form a protective layer structure mainly composed of A-O bonds on the ternary cathode material, effectively inhibiting oxygen evolution and transition metal dissolution, and maintaining a relatively unobstructed Li + migration channel; the coating of the metal element B can effectively reduce the residual lithium in the material. The B element reacts with the free Li on the surface of the ternary cathode material, which can not only reduce the residual lithium but also generate a compound of B, effectively improving the electrochemical performance such as the rate and capacity of the material." It can be seen that the actual purpose of the doping element A in this solution is closer to protecting the surface of the cathode material and preventing the dissolution of nickel, cobalt, and manganese; The coating of the metal element B is designed for the residual lithium on the surface of the material.
[0006] Prior art 2: Chinese Patent Application No. 202410595326.7 discloses a cathode material, its preparation method and application. The cathode material includes a cathode matrix and a coating layer located on the surface of the cathode matrix; the chemical general formula of the cathode matrix is Li z Ni 1-q-y-a Co q Mn y A a B b O2, where 0.95 < z < 1.3, 0 < q ≤ 0.2, 0 < y ≤ 0.2, 0 < a ≤ 0.1, 0 < b ≤ 0.1, element A is selected from at least one of Zr, Sr, Al, Sb, W, Y, and Ti, and B is selected from tetrahedral polyanions (FO4) n- and its derivative groups (F m O 3m+1 ), n- where F is selected from at least one of P, Si, S, As, Mo, and W; the coating layer contains element R, and element R is selected from at least one of Al, Ti, W, Co, and B; However, further observing this solution, it can be seen that in the coating treatment process of this solution, either the cathode material matrix is first washed, or the mixture of the cathode material and element R needs to be calcined and then washed with water. It can be seen that this solution requires washing with water; In addition, the scheme records the role of its dopant and coating agent in paragraph 36 of the specification: "By doping the polyanion group B in the positive electrode matrix, the TM-O bond of the layered oxide can be effectively stabilized to enhance the structural stability and thermal stability of the high-nickel ternary material, thereby improving the high-temperature performance of the material, and can effectively expand the spacing between the lithium layer and the transition metal layer, promote the migration of lithium ions, reduce the volume shrinkage of the unit cell during the cycle, thereby reducing the lattice strain and inhibiting the formation of microcracks. Doping the element A in the positive electrode matrix is beneficial to ensuring the conductivity and high capacity of the positive electrode material. Further coating the surface of the positive electrode matrix with a coating layer containing the elements Al, Ti, W, Co and B can further increase the capacity of the positive electrode material and inhibit the side reaction between the positive electrode material and the electrolyte." The problem that this solution needs to solve is: how to provide a polycrystalline ultra-high nickel ternary positive electrode material with low soluble lithium content and without the need to remove soluble lithium through water washing. Summary of the invention
[0007] The purpose of the present application is to provide a polycrystalline ultra-high nickel ternary positive electrode material with low soluble lithium content and no need to remove soluble lithium by water washing, as well as a preparation method for preparing the positive electrode material. The method can effectively stabilize the structure of the polycrystalline ternary positive electrode material in a high-voltage working platform, and can reduce the residual alkali on the surface during the production process, and can make the coating elements evenly coated on the surface.
[0008] Unless otherwise specified in this application: nM represents nanomole / liter, μM represents micromole / liter, mM represents millimole / liter, and M represents mole / liter; To achieve the above-mentioned purpose, the present application discloses a polycrystalline ultra-high nickel ternary positive electrode material, comprising a core layer doped with metal element A and metal element B at the same time and a shell layer containing cobalt element and boron element at the same time; The metal element A is selected from at least one of aluminum and magnesium; The metal element B is at least one selected from zirconium, yttrium, titanium, tungsten and strontium.
[0009] The doped metal element A has a small radius and is easy to enter the bulk phase. It is also an inert metal and will not undergo valence changes due to gain or loss of electrons during the redox reaction. Therefore, the metal element A is similar to manganese and provides a more stable support than manganese. The metal element B plays a role in fluxing and stabilizing the bulk phase during the sintering process, increasing the thickness of the grain boundary, and stabilizing the oxygen position without precipitation under long-cycle working conditions; and the metal element B can stabilize the crystal lattice; The crystals of ultra-high nickel positive electrode materials are more stable under the combined action of metal elements A and B, thereby reducing the soluble lithium content on the surface of the material; At the same time, a shell layer containing cobalt and boron elements is coated on the surface of the ultra-high nickel positive electrode material. On the one hand, the use of cobalt elements can form a protective layer to reduce the direct contact between the positive electrode material and the electrolyte. On the other hand, cobalt and boron further react with the soluble lithium on the surface of the ultra-high nickel ternary material, consuming the soluble lithium on the surface of the ternary material, further inhibiting the residual lithium on the surface of the positive electrode material.
[0010] Preferably, the matrix of the polycrystalline ultra-high nickel ternary positive electrode material is LiNi x Co y Mn z O2, x+y+z=1 and 0.8≤x≤0.95, y>0, z>0.
[0011] Preferably, the matrix of the polycrystalline ultra-high nickel ternary positive electrode material is LiNi x Co y Mn z O2, x+y+z=1 and 0.88≤x≤0.95, y>0, z>0.
[0012] As the nickel content continues to increase, the lithium-nickel mixing will become more serious, resulting in further precipitation of soluble lithium. Due to the strong inhibitory ability of metal element A, metal element B, and the shell containing cobalt and boron elements on soluble lithium, the advantages of this application will be further reflected when dealing with ternary positive electrode materials with higher nickel content.
[0013] Preferably, the grain size of the core layer doped with metal element A and metal element B is 300-350 nm; The mass of the metal element A is 1000-5000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of the metal element B is 1000-3000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of the cobalt element is 3000 to 30000 ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of the boron element is 300 to 2000 ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material.
[0014] Furthermore, the present application further optimizes the doping amount of metal element A and metal element B, and the coating amount of cobalt element and boron element in the shell layer, so that the overall inhibition ability of metal element A, metal element B, cobalt element and boron element on soluble lithium is further improved. On the one hand, by optimizing the doping amount of metal element A and metal element B, the ternary positive electrode material has a more stable crystal structure, and the amount of soluble lithium is more suitable for the generation of a coating layer containing cobalt element and boron element. In addition, since the addition amount of cobalt element and boron element is optimized, the thickness of the coating layer is also directly changed, so that it has both good protection ability and electrochemical performance.
[0015] Preferably, the metal element A is provided by an oxide containing the metal element A; The metal element B is provided by an oxide containing the metal element B; The cobalt element is provided by cobalt oxyhydroxide and / or cobaltous oxide; The boron element is provided by boron nitride and / or boric acid and / or boron oxide.
[0016] Preferably, the metal element A is aluminum, and the metal element B is zirconium.
[0017] Preferably, the cobalt element is provided by cobalt oxyhydroxide; The boron element is provided by boron nitride.
[0018] Furthermore, during the experimental process, the present application conducted repeated experiments on a variety of cobalt sources and boron sources and found that cobalt oxyhydroxide and boron nitride exhibited the most excellent enhancement effects.
[0019] In addition, the present application also discloses a method for preparing the above-mentioned polycrystalline ultra-high nickel ternary positive electrode material, wherein metal element A and metal element B are doped into the matrix of the polycrystalline ultra-high nickel ternary positive electrode material and used as a core layer; Cobalt and boron elements are simultaneously coated on the surface of the core layer to obtain a polycrystalline ultra-high nickel ternary positive electrode material.
[0020] Preferably, the method comprises the following steps: Step 1: Mixing a nickel-cobalt-manganese precursor, an oxide containing a metal element A, an oxide containing a metal element B, and a lithium source together to obtain a first mixed material, and then placing the first mixed material in an oxygen-rich environment at a heating rate of 1 to 2°C / min to 520 to 580°C, and keeping the temperature for 1.5 to 2.5 hours; Then, the temperature is raised to 700-750°C at a rate of 0.5-1°C / min, kept at that temperature for 10-14 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a burnt material; Step 2: Mix the fired material obtained in step 1 with cobalt hydroxide oxide and / or cobaltous oxide, boron nitride and / or boric acid and / or boric oxide to obtain a second mixed material, then place the second mixed material in an oxygen-rich environment and heat it to 550-700°C at a heating rate of 1.2-1.8°C / min, keep it warm for 8-10 hours, then naturally cool it to room temperature, take it out and crush and sieve it to obtain a polycrystalline ultra-high nickel ternary positive electrode material.
[0021] In addition, the present application also discloses a battery comprising the above-mentioned polycrystalline ultra-high nickel ternary positive electrode material.
[0022] Compared with the prior art, the present invention has the following advantages: 1. There is no water washing process in the production process, and no wastewater containing heavy metals is produced, which is environmentally friendly. At the same time, the ultra-high nickel polycrystalline material does not undergo a water washing process, and the Li + Most of them can stably exist in the Li position, which greatly improves the stability of the material and thus improves the recycling performance of the material; 2. Through the simultaneous doping of metal elements A and B, on the one hand, the metal element B is used to stabilize the grain boundary in the lattice, and on the other hand, the metal element A plays a supporting role in the lattice like the Mn element, jointly stabilizing the structure of the ultra-high nickel crystal, thereby limiting the soluble lithium on the surface of the positive electrode material; 3. The shell containing cobalt and boron elements coated on the surface of the positive electrode material reacts with the soluble lithium on the surface of the positive electrode material, consuming most of the soluble lithium while generating a thin layer of lithium cobalt oxide coating on the surface to form a core-shell structure. This prevents the ultra-high nickel ternary material from directly contacting the electrolyte, slowing down the corrosion of the electrolyte on the main material and improving the cycle stability. At the same time, the boron element reacts with the soluble lithium on the surface to generate Li-BO fast ion conductors, thereby increasing ionic conductivity and thus increasing capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The cycle capacity test diagram of the positive electrode materials prepared in Example 1, Example 6 and Example 7; Figure 2 The cycle capacity test diagram of the positive electrode materials prepared in Comparative Example 7, Comparative Example 8 and Comparative Example 9; Figure 3 is a scanning electron microscope image of the second mixed material in Example 1; Figure 4 This is an electron microscope image of the polycrystalline ultra-high nickel ternary positive electrode material prepared in Example 1. DETAILED DESCRIPTION
[0024] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0025] Example 1 Step 1: Prepare the nickel-cobalt-manganese precursor (Ni 0.88 Co 0.6 Mn 0.6 O2), aluminum oxide, zirconium oxide and lithium carbonate are mixed together to obtain a first mixed material, wherein the molar ratio of the molar amount of lithium element in the lithium carbonate to the total molar amount of nickel, cobalt and manganese in the nickel, cobalt and manganese precursor is 1.03:1, and then the first mixed material is placed in an oxygen-rich environment and heated to 560°C at a rate of 1.5°C / min, and kept warm for 2 hours; Then, the temperature was raised to 720°C at a rate of 0.8°C / min, kept at the constant temperature for 12 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a burnt material; The mass of aluminum in alumina is added at 3000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of zirconium in zirconium oxide is added at 2000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; Step 2: mixing the calcined material obtained in step 1 with cobalt oxyhydroxide and boron nitride to obtain a second mixed material; The mass of cobalt element in cobalt oxyhydroxide is added at 15000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of boron element in boron nitride is added at 1000ppm of the total mass of polycrystalline ultra-high nickel ternary positive electrode material; The second mixed material was then placed in an oxygen-rich environment and heated to 620°C at a rate of 1.6°C / min, maintained at a constant temperature for 9 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a polycrystalline ultra-high nickel ternary positive electrode material.
[0026] Example 2 Step 1: Prepare the nickel-cobalt-manganese precursor (Ni 0.88 Co 0.6 Mn 0.6 O2), aluminum oxide, zirconium oxide and lithium carbonate are mixed together to obtain a first mixed material, wherein the molar ratio of the molar amount of lithium element in the lithium carbonate to the total molar amount of nickel, cobalt and manganese in the nickel-cobalt-manganese precursor is 1.03:1, and then the first mixed material is placed in an oxygen-rich environment and heated to 580°C at a rate of 2°C / min, and kept warm for 1.5 hours; Then, the temperature was raised to 750°C at a rate of 1°C / min, kept constant for 10 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a burnt material; The mass of aluminum in alumina is added at 5000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of zirconium in zirconium oxide is added at 3000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; Step 2: mixing the calcined material obtained in step 1 with cobalt oxyhydroxide and boron nitride to obtain a second mixed material; Among them, the mass of cobalt element in cobalt oxyhydroxide is 30000ppm of the total mass of polycrystalline ultra-high nickel ternary positive electrode material; The mass of boron element in boron nitride is 2000ppm of the total mass of polycrystalline ultra-high nickel ternary positive electrode material; The second mixed material was then placed in an oxygen-rich environment and heated to 700°C at a rate of 1.8°C / min, maintained at a constant temperature for 8 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a polycrystalline ultra-high nickel ternary positive electrode material.
[0027] Example 3 Step 1: Prepare the nickel-cobalt-manganese precursor (Ni 0.88 Co 0.6 Mn 0.6 O2), aluminum oxide, zirconium oxide and lithium carbonate are mixed together to obtain a first mixed material, wherein the molar ratio of the molar amount of lithium element in the lithium carbonate to the total molar amount of nickel, cobalt and manganese in the nickel, cobalt and manganese precursor is 1.03:1, and then the first mixed material is placed in an oxygen-rich environment and heated to 520°C at a rate of 1°C / min, and kept warm for 2.5 hours; Then, the temperature was raised to 700°C at a rate of 0.5°C / min, kept at the constant temperature for 14 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a burnt material; The mass of aluminum in alumina is added at 1000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of zirconium in zirconium oxide is added at 1000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; Step 2: mixing the calcined material obtained in step 1 with cobalt oxyhydroxide and boron nitride to obtain a second mixed material; The mass of cobalt element in cobalt oxyhydroxide is added at 3000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of the boron element in the boron nitride is added at 300ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The second mixed material was then placed in an oxygen-rich environment and heated to 550°C at a rate of 1.2°C / min, maintained at a constant temperature for 10 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a polycrystalline ultra-high nickel ternary positive electrode material.
[0028] Example 4 It is basically the same as Example 1, except that magnesium oxide is used to replace aluminum oxide, and the mass of magnesium in magnesium oxide is added at 3000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material.
[0029] Example 5 It is basically the same as Example 1, except that yttrium oxide is used to replace zirconium oxide, and the mass of yttrium in yttrium oxide is added at 2000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material.
[0030] Example 6 The same as Example 1, except that the nickel-cobalt-manganese precursor is Ni 0.8 Co 0.1 Mn 0.1 O2.
[0031] Example 7 The same as Example 1, except that the nickel-cobalt-manganese precursor is Ni 0.95 Co 0.02 Mn 0.03 O2.
[0032] Example 8 It is basically the same as Example 1, except that cobaltous oxide is used instead of cobalt oxyhydroxide, and the mass of cobalt element in cobaltous oxide is 15000ppm of the total mass of polycrystalline ultra-high nickel ternary positive electrode material.
[0033] Example 9 It is basically the same as Example 1, except that boric acid is used instead of boron nitride, and the mass of the boron element in the boric acid is 1000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material.
[0034] Example 10 The method is basically the same as Example 1, except that the mass of aluminum in alumina is added at 4000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of zirconium in zirconium oxide is added at 1000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material.
[0035] Embodiment 11 The method is basically the same as Example 1, except that the mass of aluminum in alumina is added at 1000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of zirconium in zirconium oxide is added according to 4000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material.
[0036] Example 12 The method is basically the same as Example 1, except that the mass of the cobalt element in the cobalt oxyhydroxide is added at 15700ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of the boron element in boron nitride is added at 300ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material.
[0037] Embodiment 13 The method is basically the same as Example 1, except that the mass of the cobalt element in the cobalt oxyhydroxide is added at 14000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of the boron element in boron nitride is added at 2000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material.
[0038] Embodiment 14 The method is basically the same as Example 1, except that the mass of aluminum in alumina is added at 5000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of zirconium in zirconium oxide is added according to 3000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material.
[0039] Embodiment 15 The method is basically the same as Example 1, except that the mass of the cobalt element in the cobalt oxyhydroxide is added at 30000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of the boron element in boron nitride is added at 2000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material.
[0040] Comparative Example 1 Step 1: Prepare the nickel-cobalt-manganese precursor (Ni 0.88 Co 0.6 Mn 0.6 O2), aluminum oxide, zirconium oxide and lithium carbonate are mixed together to obtain a first mixed material, wherein the molar ratio of the molar amount of lithium element in the lithium carbonate to the total molar amount of nickel, cobalt and manganese in the nickel, cobalt and manganese precursor is 1.03:1, and then the first mixed material is placed in an oxygen-rich environment and heated to 560°C at a rate of 1.5°C / min, and kept warm for 2 hours; Then, the temperature was raised to 720°C at a rate of 0.8°C / min, kept at the constant temperature for 12 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a burnt material; The mass of aluminum in alumina is added at 3000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of zirconium in zirconium oxide is added at 2000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The fired material was then placed in an oxygen-rich environment and heated to 620°C at a rate of 1.6°C / min, maintained at a constant temperature for 9 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain an ultra-high nickel ternary positive electrode material.
[0041] Comparative Example 2 Step 1: Prepare the nickel-cobalt-manganese precursor (Ni0.88 Co 0.6 Mn 0.6 O2) and lithium carbonate are mixed together to obtain a first mixed material, wherein the molar ratio of the molar amount of lithium element in the lithium carbonate to the total molar amount of nickel, cobalt and manganese in the nickel-cobalt-manganese precursor is 1.03:1, and then the first mixed material is placed in an oxygen-rich environment and heated to 560°C at a rate of 1.5°C / min, and kept warm for 2 hours; Then, the temperature was raised to 720°C at a rate of 0.8°C / min, kept at the constant temperature for 12 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a burnt material; Step 2: mixing the calcined material obtained in step 1 with cobalt oxyhydroxide and boron nitride to obtain a second mixed material; Among them, the mass of cobalt element in cobalt oxyhydroxide is 15000ppm of the total mass of polycrystalline ultra-high nickel ternary positive electrode material; The mass of boron element in boron nitride is 1000ppm of the total mass of polycrystalline ultra-high nickel ternary positive electrode material; The second mixed material was then placed in an oxygen-rich environment and heated to 620°C at a rate of 1.6°C / min, maintained at a constant temperature for 9 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a polycrystalline ultra-high nickel ternary positive electrode material.
[0042] Comparative Example 3 The method is substantially the same as Example 1, except that niobium oxide is used instead of aluminum oxide.
[0043] Comparative Example 4 The method is basically the same as Example 1, except that boron oxide is used instead of zirconium oxide.
[0044] Comparative Example 5 The method is substantially the same as Example 1, except that aluminum oxide is used to replace cobalt oxyhydroxide.
[0045] Comparative Example 6 The method is basically the same as Example 1, except that zirconium oxide is used instead of boron nitride.
[0046] Comparative Example 7 Step 1: Prepare the nickel-cobalt-manganese precursor (Ni 0.88 Co 0.6 Mn 0.6 O2) and lithium carbonate are mixed together to obtain a first mixed material, wherein the molar ratio of the molar amount of lithium element in the lithium carbonate to the total molar amount of nickel, cobalt and manganese in the nickel-cobalt-manganese precursor is 1.03:1, and then the first mixed material is placed in an oxygen-rich environment and heated to 560°C at a rate of 1.5°C / min, and kept warm for 2 hours; Then, the temperature was raised to 720°C at a rate of 0.8°C / min, kept at the constant temperature for 12 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a burnt material; Step 2: Place the calcined material obtained in step 1 in an oxygen-rich environment and heat it to 620°C at a rate of 1.6°C / min, maintain the temperature for 9 hours, then naturally cool it to room temperature, take it out and crush and sieve it to obtain an ultra-high nickel ternary positive electrode material.
[0047] Comparative Example 8 It is basically the same as Comparative Example 7, except that the nickel-cobalt-manganese precursor (Ni 0.8 Co 0.1 Mn 0.1 O2) replaces the nickel-cobalt-manganese precursor (Ni 0.88 Co 0.6 Mn 0.6 O2).
[0048] Comparative Example 9 It is basically the same as Comparative Example 7, except that the nickel-cobalt-manganese precursor (Ni 0.95 Co 0.02 Mn 0.03 O2) replaces the nickel-cobalt-manganese precursor (Ni 0.88 Co 0.6 Mn 0.6 O2).
[0049] Performance Testing: The polycrystalline ternary positive electrode materials obtained in Examples 1-15 and Comparative Examples 1-9 were subjected to electrochemical analysis of button cells, with the main comparison being the discharge capacity at 0.1C and the 100-cycle retention rate of 1C charge and discharge.
[0050] The lithium battery cycle life test method is: the capacity retention rate of the button battery after 100 cycles of 1C, the test standard is: voltage 3.0V-4.3V, charge and discharge rate 1C, temperature 25℃, nominal specific capacity 200mAh / g.
[0051] The lithium battery rate performance testing method is: the first cycle capacity of the button battery at different rates, the test standard is: 3.0-4.3V, the temperature is 25℃, the charge and discharge rates are: 0.1C, 0.5C, 1C, and the nominal specific capacity is 200mAh / g.
[0052] The method for detecting free lithium on the surface of materials is: calculation according to the acid-base titration method in Part 1: Determination of lithium carbonate content in GB / T 11064.1-2013 Chemical analysis method for lithium carbonate, lithium hydroxide monohydrate and lithium chloride.
[0053] The surface soluble lithium, pH, and lithium battery cycle life tests were performed on the examples and comparative examples. The specific conditions were the above method. The results are shown in Table 1: Table 1
[0054] Result analysis: 1. It can be seen from Examples 1-3 that when the production parameters, the mass ratios of the doping elements, and the mass ratios of the coating elements in the preparation processes of Examples 1-3 are slightly changed, although there are certain fluctuation trends in the lithium ion content, the charge and discharge rate, and the cycle retention rate between Examples 1-3, the overall amplitude is not obvious.
[0055] 2. Further observation of Example 1 and Examples 4-5 shows that when the types of metal element A and metal element B are changed, the lithium ion content of Examples 4 and 5 is improved relative to that of Example 1. The reason is that the improvement of the stabilization ability of magnesium to the crystal structure relative to aluminum is not obvious, which leads to the aggravation of lithium dissolution in Example 4 and the increase of lithium ion content. At the same time, with the increase of lithium ion content, the rate performance and cycle performance have a downward trend to varying degrees; On the other hand, after yttrium oxide was used instead of zirconium oxide in Example 5, the stabilizing ability of yttrium on the bulk phase of the material was poorer than that of zirconium, which resulted in an increase in the lithium ion content of Example 5, and a certain downward trend in rate performance and cycle performance.
[0056] 3. It can be seen from the observation of Example 1 and Examples 8-9 that when cobaltous oxide is used to replace cobalt oxyhydroxide, the lithium ion content of Example 8 increases, and the rate performance and cycle performance show a certain degree of downward trend. The reason is that the reaction activity of cobaltous oxide with the soluble lithium on the surface of the positive electrode material may be relatively low, which leads to too little consumption of soluble lithium, thereby increasing the lithium ion content of the positive electrode material, and then causing the rate performance and cycle performance of the material to decrease; At the same time, when boric acid is used to replace boron nitride in Example 9, although the amount of boron element used is the same, in the molecular structure of boron nitride, nitrogen and boron are connected by a covalent bond of a nitrogen-boron triple bond, and the bond energy is higher. Boron nitride is also more stable, and a higher temperature is required to break the bond to form active free radicals for reaction, so that it can still combine with the soluble lithium on the surface of the material in a high temperature environment of 620°C to form a Li-Co-BO fast ion conductor.
[0057] 4. It can be seen from Example 1, Example 10 and Example 11 that when the total amount of dopant remains unchanged and the mass ratio between aluminum and zirconium is changed, the lithium ion content of Examples 10 and 11 is increased relative to that of Example 1. The reason is that the aluminum element enters the bulk more through its smaller radius and plays a role in supporting the crystal structure, while zirconium is more on the surface or shallow layer of the crystal to improve the stability of the surface structure; The two cooperate with each other to improve the structural strength of the crystal, thereby inhibiting the mixing of lithium and nickel and the generation of soluble lithium. Therefore, even if the total amount of doping remains unchanged, the stability inside the crystal or on the surface of the crystal is too low, which will lead to the aggravation of the mixing of lithium and nickel relative to Example 1, and then the lithium ion content relative to Example 1 is increased, and the rate performance and cycle performance are deteriorated; Similarly, it can be seen from Example 12 and Example 13 that when the total amount of the coating agent remains unchanged, changing the mass ratio between cobalt and boron will also lead to an increase in the lithium ion content. The reason is that the cobalt element plays a role in forming a protective layer in the shell layer on the one hand, and on the other hand, it needs to form a Li-Co-BO fast ion conductor together with boron and lithium. When the thickness of the protective layer is too high and too much cobalt is consumed, the production of Li-Co-BO fast ion conductor will decrease, which will result in the inability to consume more soluble lithium. However, when the amount of cobalt added is too small, the protective layer becomes too sparse and it is difficult to provide sufficient protection, which in turn leads to a decrease in the overall rate performance and cycle performance.
[0058] 5. It can be seen from Examples 1, 14 and 15 that when the mass ratio difference between the dopant and the coating agent is further increased, the four elements of aluminum, zirconium, cobalt and boron inhibit soluble lithium from four dimensions respectively. When there is too much dopant, although the stability of the lattice is indeed improved and the amount of soluble lithium on the surface is reduced, the amount of soluble lithium on the surface is too low, which will lead to the formation of Li-Co-BO fast ion conductors. Because the material cannot provide enough lithium for the Li-Co-BO fast ion conductor, the protective ability of the positive electrode material shell to the core body is reduced during actual use, thereby increasing the lithium ion content and reducing the rate performance and cycle performance. At the same time, when there is too much coating agent, the shell layer generated by cobalt is too thick, which will cause the protective layer to fall off. After increasing the boron content, the mass of soluble lithium has not changed much. Therefore, the more advantageous Li-Co-BO fast ion conductor cannot be generated. As the cobalt falls off, the mass of the Li-Co-BO fast ion conductor will further decrease, which will lead to a decrease in the protection ability of the positive electrode material shell to the core, thereby increasing the lithium ion content and reducing the rate performance and cycle performance.
[0059] 6. Comparative Examples 1-2 show that when only the positive electrode material is doped or coated, the lithium ion content of the material will be further increased. The reason is that only doping is equivalent to completely giving up the ability of the shell to protect the core and the role of consuming soluble lithium through coating; Although coating alone can consume soluble lithium, the crystal structure is too fragile and the amount of soluble lithium is too much. Adding coating agent may cause the coating layer to fall off. Therefore, coating alone is still difficult to suppress the soluble lithium content on the surface of the material. By observing Comparative Examples 1-2 and Comparative Example 7 at the same time, it can be seen that although Comparative Examples 1-2 have a certain degree of improvement in the suppression of lithium ion content relative to Comparative Example 7, the lithium ion content of Comparative Example 1 is reduced by 384 relative to Comparative Example 7, and the lithium ion content of Comparative Example 2 is reduced by 412 relative to Comparative Example 7. However, by observing the difference between Example 1 and Comparative Example 7, it can be seen that the lithium ion content of Example 1 is reduced by 1488 relative to Comparative Example 7. It can be seen that the ability of Example 1 to suppress the lithium ion content exceeds the simple superposition of Comparative Examples 1 and Comparative Example 2. At the same time, the improvement of rate performance and cycle performance of Example 1 relative to Comparative Example 7 also exceeds the improvement of Comparative Example 1 and Comparative Example 2 relative to Comparative Example 7. It can be seen that when doping and coating are performed at the same time, a synergistic effect is generated between the two, which further suppresses the soluble lithium content of the positive electrode material.
[0060] 7. By observing Example 1 and Comparative Examples 3-6, it can be seen that after replacing any doping element or coating element in the present application with other commonly used doping elements or coating elements, the lithium ion content of Comparative Examples 3-6 is improved relative to that of Example 1, and the rate performance and cycle performance are reduced; The reason is that, on the one hand, the niobium used in Comparative Example 3 has a relatively large ionic radius, and it cannot play a supporting capacity similar to that of aluminum. After boron is used to replace zirconium for doping, the boron element will react with lithium hydroxide at a higher calcination temperature to form Li-BO oxide. Because the bond energy of Li-B after combination is higher than that of Li-Me (Me is Ni, Co, Mn), according to the principle of reaction kinetics, the reactants tend to move towards the products with lower energy, which leads to an increase in the surface lithium ion content and a lack of lattice lithium. When aluminum and zirconium are used to replace cobalt for coating, aluminum and zirconium are both inert metal oxides. Both have high melting points and low chemical activity. They cannot react with soluble lithium on the surface during the secondary calcination stage, which leads to an increase in the surface lithium ion content. However, the material can be coated to a certain extent, reducing the erosion of the electrolyte on the material and improving the cycle to a certain extent. However, because it is an inert metal, it cannot gain or lose electrons and cannot provide capacity during the battery charging and discharging process, which reduces the content of active substances and has a certain impact on the capacity.
[0061] 8. By comparing Example 1, Example 6, Example 7 and Comparative Examples 7-9, it can be seen that as the nickel content increases, the ability of the present application to suppress the lithium ion content is further amplified. When applied to a ternary positive electrode material with a nickel content of 0.95, its ability to suppress the lithium ion content is maximized. However, since the lithium-nickel mixing of the ultra-high nickel material is too serious, even if the nickel content has been suppressed to the maximum extent, it is still difficult to maintain good cycle performance as the positive electrode material is continuously used; For further reference, Figure 1-2 It can be seen that when no doping and coating treatment is done, the nickel-cobalt-manganese precursor (Ni 0.8 Co 0.1 Mn 0.1 O2) has a higher cathode material than the nickel-cobalt-manganese precursor (Ni 0.88 Co 0.6 Mn 0.6 O2), nickel-cobalt-manganese precursor (Ni 0.95 Co 0.02 Mn 0.03 O2) cycle capacity retention capability; However, with the application of doping and coating technology, nickel-cobalt-manganese precursor (Ni 0.88 Co 0.6 Mn 0.6 The cycle capacity retention ability of the positive electrode material prepared by O2) rises to the highest level. It can be seen that the doping and coating technology is relatively more suitable for the positive electrode material with higher nickel content. Also refer to Figure 3-4 It can be seen that before sintering, the surface of the second mixture is smoother because the coating layer of cobalt and boron has not yet formed. Figure 4 visible, Figure 4 The surface of the battery shows certain island-like protrusions. The reason is that during the generation process of Li-Co-BO, most of the soluble lithium on the surface of the positive electrode material is combined and coated on the outermost layer of the material, thereby forming island-like protrusions.
[0062] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A polycrystalline ultra-high nickel ternary positive electrode material, It is characterized in that It includes a core layer doped with metal element A and metal element B at the same time and a shell layer containing cobalt element and boron element at the same time; The metal element A is selected from at least one of aluminum and magnesium; The metal element B is at least one selected from the group consisting of zirconium, yttrium, titanium, tungsten and strontium.
2. The polycrystalline ultra-high nickel ternary positive electrode material according to claim 1, It is characterized in that The matrix of the polycrystalline ultra-high nickel ternary positive electrode material is LiNi x Co y Mn z O 2 , x+y+z=1 and 0.8≤x≤0.95, y>0, z>0.
3. The polycrystalline ultra-high nickel ternary positive electrode material according to claim 1, It is characterized in that The matrix of the polycrystalline ultra-high nickel ternary positive electrode material is LiNi x Co y Mn z O 2 , x+y+z=1 and 0.88≤x≤0.95, y>0, z>0.
4. The polycrystalline ultra-high nickel ternary positive electrode material according to claim 2, It is characterized in that The grain size of the core layer doped with metal element A and metal element B is 300-350nm; The mass of the metal element A is 1000-5000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of the metal element B is 1000-3000ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of the cobalt element in the shell layer is 3000 to 30000 ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material; The mass of the boron element in the shell layer is 300 to 2000 ppm of the total mass of the polycrystalline ultra-high nickel ternary positive electrode material.
5. The polycrystalline ultra-high nickel ternary positive electrode material according to claim 1, It is characterized in that The metal element A is provided by an oxide containing the metal element A; The metal element B is provided by an oxide containing the metal element B; The cobalt element is provided by cobalt oxyhydroxide and / or cobaltous oxide; The boron element is provided by boron nitride and / or boric acid and / or boron oxide.
6. The polycrystalline ultra-high nickel ternary positive electrode material according to claim 1, It is characterized in that The metal element A is aluminum, and the metal element B is zirconium.
7. The polycrystalline ultra-high nickel ternary positive electrode material according to claim 5, It is characterized in that The cobalt element is provided by cobalt oxyhydroxide; The boron element is provided by boron nitride.
8. A method for preparing the polycrystalline ultra-high nickel ternary positive electrode material according to any one of claims 1 to 7, It is characterized in that The metal element A and the metal element B are doped into the matrix of the polycrystalline ultra-high nickel ternary positive electrode material and used as a core layer; Cobalt and boron elements are simultaneously coated on the surface of the core layer to obtain a polycrystalline ultra-high nickel ternary positive electrode material.
9. The method for preparing the polycrystalline ultra-high nickel ternary positive electrode material according to claim 8, It is characterized in that The following steps are involved: Step 1: Mixing a nickel-cobalt-manganese precursor, an oxide containing a metal element A, an oxide containing a metal element B, and a lithium source together to obtain a first mixed material, and then placing the first mixed material in an oxygen-rich environment at a heating rate of 1 to 2°C / min to 520 to 580°C, and keeping the temperature for 1.5 to 2.5 hours; Then, the temperature is raised to 700-750°C at a rate of 0.5-1°C / min, kept at that temperature for 10-14 hours, then naturally cooled to room temperature, taken out, crushed, and sieved to obtain a burnt material; Step 2: Mix the fired material obtained in step 1 with cobalt hydroxide oxide and / or cobaltous oxide, boron nitride and / or boric acid and / or boric oxide to obtain a second mixed material, then place the second mixed material in an oxygen-rich environment and heat it to 550-700°C at a heating rate of 1.2-1.8°C / min, keep it warm for 8-10 hours, then naturally cool it to room temperature, take it out and crush and sieve it to obtain a polycrystalline ultra-high nickel ternary positive electrode material.
10. A battery, It is characterized in that Contains the polycrystalline ultra-high nickel ternary positive electrode material as described in any one of claims 1-7.
Citation Information
Patent Citations
Y / La-doped Co / B co-coated nickel-cobalt-manganese ternary positive electrode material and preparation method thereof
CN108550802A
High-nickel ternary positive electrode material and preparation method thereof
CN111244397A
High-nickel low-cobalt type high-voltage-resistant ternary positive electrode material and preparation method thereof
CN111384392A
Positive electrode material as well as preparation method and application thereof
CN113328077A
Composite coating agent for positive electrode material, high-nickel single-crystal positive electrode material and battery
CN115036493A