Preparation method of MoP-coated Mn-SAC oxygen reduction electrocatalyst
By preparing MoP@Mn-SAC oxygen reduction electrocatalyst, the problem of low oxygen reduction reaction efficiency in zinc-air batteries was solved, and excellent electrocatalytic performance and long-term stability in zinc-air batteries were achieved, showing that in zinc-air batteries were Application potential in the field of air batteries.
Patent Information
- Application Number
- CN202411361431.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-12-06
AI Technical Summary
The slow kinetics and severe energy loss of oxygen reduction reactions in existing zinc-air batteries hinder the development of the system, and the most advanced catalyst is precious metal platinum, resulting in limited application.
Using the preparation method of MoP@Mn-SAC oxygen reduction electrocatalyst, ZIF-8 is subjected to high-temperature carbonization to obtain NC nanocubes, and then ion adsorption reaction is carried out in a mixed solution of manganese and molybdenum sources and mixed with phosphorus sources. By phosphating treatment, a MoP@Mn-SAC oxygen reduction electrocatalyst with excellent electrocatalytic properties was prepared.
Under alkaline conditions, MoP@Mn-SAC oxygen reduction electrocatalyst exhibits excellent electrocatalytic oxygen reduction performance and long-term stability, significantly improving the power density and stability of zinc-air batteries, and is innovative, efficient and easy to scale. Characteristics of transformation.
Smart Images

Figure CN119092727A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrocatalytic oxygen reduction, and in particular relates to a method for preparing a MoP@Mn-SAC oxygen reduction electrocatalyst. Background Art
[0002] With the ever-increasing demand for energy, it is necessary to develop low-cost and high-efficiency electrochemical energy devices using sustainable and clean energy. Zinc-air batteries (ZABs) are the most ideal storage devices for the future due to their simple battery structure, safe operation, environmental friendliness, economic feasibility, and high theoretical energy density. However, the sluggish kinetics and severe energy losses of the oxygen reduction reaction (ORR), which is the basis of energy conversion and storage processes and ultimately determines the cost-effectiveness of these technologies, have greatly hindered the development of such systems. To date, the most advanced ORR catalysts are various platinum (Pt)-based materials, while the high cost and scarcity of Pt have greatly hindered the widespread application of Zn-air batteries. Therefore, it is crucial to construct non-precious metal-based ORR electrocatalysts with satisfactory efficiency and durability, but it remains a huge challenge. Summary of the invention
[0003] In order to solve the above technical problems, the present invention proposes a method for preparing a MoP@Mn-SAC oxygen reduction electrocatalyst.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] The present invention provides a method for preparing a MoP@Mn-SAC oxygen reduction electrocatalyst, comprising the following steps:
[0006] (1) subjecting ZIF-8 to high temperature carbonization to obtain NC nanocubes;
[0007] (2) placing the NC nanocubes obtained in step (1) in a mixed solution of a manganese source and a molybdenum source to carry out an ion adsorption reaction, and then mixing with a phosphorus source to carry out a phosphating treatment to obtain the MoP@Mn-SAC oxygen reduction electrocatalyst.
[0008] Preferably, in step (1), the preparation method of ZIF-8 comprises the following steps: mixing hexadecyltrimethylammonium bromide and a zinc salt solution, then adding 2-methylimidazole, and performing a polymerization reaction to obtain the ZIF-8.
[0009] Preferably, the molar ratio of the hexadecyltrimethylammonium bromide, the zinc salt in the zinc salt solution and 2-methylimidazole is 0.15:1:55; and the concentration of the zinc salt solution is 0.1 mmol / mL.
[0010] Preferably, in step (1), the temperature of the high-temperature carbonization treatment is 1000° C., and the time of the high-temperature carbonization treatment is 2 hours.
[0011] Preferably, in step (2), the dosage ratio of the NC nanocubes to the manganese source is 50 mg: 0.075 mmol; the molar ratio of the manganese source to the molybdenum source in the mixed solution of the manganese source and the molybdenum source is 1: (0.5-1.5); the manganese source includes manganese nitrate, and the molybdenum source includes ammonium molybdate.
[0012] Preferably, in step (2), the temperature of the ion adsorption reaction is 60° C., and the time of the ion adsorption reaction is 12 h.
[0013] Preferably, in step (2), the mass ratio of the phosphorus source to the NC nanocubes is 1:1; and the phosphorus source comprises red phosphorus.
[0014] Preferably, in step (2), the phosphating treatment temperature is 900-1100° C., and the phosphating treatment time is 2 hours.
[0015] The present invention provides a MoP@Mn-SAC oxygen reduction electrocatalyst prepared by the preparation method described in the above technical scheme.
[0016] The present invention also provides the use of the MoP@Mn-SAC oxygen reduction electrocatalyst described in the above technical solution in an electrocatalytic oxygen reduction reaction.
[0017] Compared with the prior art, the present invention has the following advantages and technical effects:
[0018] (1) The MoP@Mn-SAC oxygen reduction electrocatalyst prepared by the present invention has excellent electrocatalytic oxygen reduction performance under alkaline conditions and a long service life. It also exhibits excellent power density and good stability in the performance test of zinc-air batteries, showing practical application potential in zinc-air batteries.
[0019] (2) The preparation method of the MoP@Mn-SAC oxygen reduction electrocatalyst provided by the present invention is innovative, efficient, and easy to scale up.
[0020] (3) The preparation method of the MoP@Mn-SAC oxygen reduction electrocatalyst provided by the present invention is simple. By performing ion adsorption and phosphating treatment on the NC substrate, a MoP@Mn-SAC oxygen reduction electrocatalyst having excellent electrocatalytic oxygen reduction performance under alkaline conditions and exhibiting good long-term stability is obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0022] Figure 1 X-ray powder diffraction patterns of MoP@Mn-SAC prepared in Example 2, Mn-SAC prepared in Comparative Example 1, MoP@NC prepared in Comparative Example 2, and NC in step (4) of Example 2, wherein a is MoP@Mn-SAC, b is Mn-SAC, c is MoP@NC, and d is NC;
[0023] Figure 2 Characterization diagram of MoP@Mn-SAC prepared in Example 2, wherein a is a scanning electron microscope image of NC, b is a scanning electron microscope image of MoP@Mn-SAC, c is a transmission electron microscope image of MoP@Mn-SAC, d is a high-resolution transmission electron microscope image of MoP@Mn-SAC, e is the corresponding lattice spacing distribution in the high-resolution transmission electron microscope image of MoP@Mn-SAC, f is the crystal and atomic structure of MoP@Mn-SAC and the corresponding lattice spacing, and g is an element distribution diagram of MoP@Mn-SAC;
[0024] Figure 3 The X-ray photoelectron spectrum of MoP@Mn-SAC prepared in Example 2 and the extended X-ray absorption fine structure spectrum of Mn in MoP@Mn-SAC, wherein a is the 1s spectrum of C, b is the 2p spectrum of Mn, c is the 3d spectrum of Mo, d is the 1s spectrum of N, e is the 2p of P, and f is the extended X-ray absorption fine structure spectrum of Mn in MoP@Mn-SAC;
[0025] Figure 4 Electron paramagnetic resonance spectra of MoP@Mn-SAC prepared in Example 2, NC prepared in step (4) of Example 2, Mn-SAC prepared in Comparative Example 1, MoP@NC prepared in Comparative Example 2, and PNC prepared in Comparative Example 3;
[0026] Figure 5The linear scanning curves of electrocatalytic oxygen reduction of NC prepared in step (4) of Example 2, MoP@Mn-SAC prepared in Example 2, Mn-SAC prepared in Comparative Example 1, MoP@NC prepared in Comparative Example 2, and commercial Pt / C electrode (a), the linear scanning curves of electrocatalytic oxygen reduction of MoP@Mn-SAC prepared in Examples 2 and 4-5 (b), the linear scanning curves of electrocatalytic oxygen reduction of MoP@Mn-SAC prepared in Examples 1-3 (c), the linear scanning curves of electrocatalytic oxygen reduction of NC prepared in step (4) of Example 2, MoP@Mn-SAC prepared in Example 2, and PNC prepared in Comparative Example 3 (d), the linear scanning curves of hydrogen peroxide (H2O2) of MoP@Mn-SAC prepared in Example 2, Mn-SAC prepared in Comparative Example 1, and MoP@NC prepared in Comparative Example 2 2 O 2 ) yield and electron transfer number (n) (e), stability test results of MoP@Mn-SAC prepared in Example 2 and commercial Pt / C electrode (f);
[0027] Figure 6 The model diagram of the solid-state zinc-air battery (a) and the voltage of the solid-state zinc-air battery of MoP@Mn-SAC prepared in Example 2 (b);
[0028] Figure 7 The performance test results of the solid-state zinc-air battery of MoP@Mn-SAC and commercial Pt / C electrode prepared in Example 2, wherein a is the battery open circuit voltage test result, b is the power density test result, and c is the stability test result;
[0029] Figure 8 The model diagram of the flexible zinc-air battery (a) and the voltage of the flexible zinc-air battery of MoP@Mn-SAC prepared in Example 2 at different temperatures (b);
[0030] Fig. 9 These are the performance test results of the flexible zinc-air battery with MoP@Mn-SAC and commercial Pt / C electrode prepared in Example 2, where a is the open circuit voltage test curve of the flexible zinc-air battery (the inset is a photo of the assembled flexible zinc-air battery lighting the LED board), b is the polarization curve and power density curve of the flexible zinc-air battery, and c is the long-term stability of the flexible zinc-air battery. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0033] The embodiment of the present invention provides a method for preparing a MoP@Mn-SAC oxygen reduction electrocatalyst, comprising the following steps:
[0034] (1) subjecting ZIF-8 to high temperature carbonization to obtain NC nanocubes;
[0035] (2) placing the NC nanocubes obtained in step (1) in a mixed solution of a manganese source and a molybdenum source to carry out an ion adsorption reaction, and then mixing with a phosphorus source to carry out a phosphating treatment to obtain the MoP@Mn-SAC oxygen reduction electrocatalyst.
[0036] In a preferred embodiment, in step (1), the preparation method of ZIF-8 comprises the following steps: mixing hexadecyltrimethylammonium bromide (CTAB) and a zinc salt solution, then adding 2-methylimidazole, and performing a polymerization reaction to obtain the ZIF-8. The CTAB in the present invention can be adsorbed on the (100) crystal plane of ZIF-8 to further reduce its size and present a more uniform cubic structure, so that ZIF-8 has a larger specific surface area. The high specific surface area helps to increase the contact area between the catalyst and the reactant, thereby enhancing the reaction efficiency.
[0037] In a preferred embodiment, the molar ratio of the hexadecyltrimethylammonium bromide (CTAB), the zinc salt in the zinc salt solution and 2-methylimidazole is 0.15:1:55; the concentration of the zinc salt solution is 0.1mmol / mL; the zinc salt includes zinc nitrate, preferably zinc nitrate hexahydrate. CTAB in the present invention is used to regulate the morphology of ZIF-8. The cubic morphology of ZIF-8 can be obtained by controlling the amount of CTAB within the above range; reducing the molar ratio of the zinc salt in the zinc salt solution and 2-methylimidazole will reduce the size of ZIF-8, which is not conducive to the loading of MoP nanoparticles.
[0038] In a preferred embodiment, the polymerization reaction temperature is 60° C., and the polymerization reaction time is 4 hours; the polymerization reaction includes stirring and standing; the stirring time is 2 hours; and the standing time is 2 hours.
[0039] In a preferred embodiment, in step (1), the temperature of the high temperature carbonization treatment is 1000° C., the time of the high temperature carbonization treatment is 2 h, and the atmosphere of the high temperature carbonization treatment is an argon atmosphere.
[0040] In a preferred embodiment, in step (2), the ratio of the amount of the NC nanocube to the manganese source is 50 mg: 0.075 mmol. The NC nanocube in the present invention can adsorb metal ions and form metal-nitrogen bonds (MN) with Mn ions during the subsequent phosphating process.
[0041] In a preferred embodiment, in step (2), the molar ratio of the manganese source to the molybdenum source in the mixed solution of the manganese source and the molybdenum source is 1:(0.5-1.5); the manganese source comprises manganese nitrate, preferably manganese nitrate trihydrate; and the molybdenum source comprises ammonium molybdate.
[0042] In a preferred embodiment, in step (2), the temperature of the ion adsorption reaction is 60° C., and the time of the ion adsorption reaction is 12 h.
[0043] In a preferred embodiment, in step (2), the mass ratio of the phosphorus source to the NC nanocubes is 1:1; and the phosphorus source comprises red phosphorus.
[0044] In a preferred embodiment, in step (2), the temperature of the phosphating treatment is 900-1100° C., the time of the phosphating treatment is 2 h, and the atmosphere of the phosphating treatment is an argon atmosphere.
[0045] The present invention provides a MoP@Mn-SAC oxygen reduction electrocatalyst prepared by the preparation method described in the above technical scheme.
[0046] The present invention also provides the use of the MoP@Mn-SAC oxygen reduction electrocatalyst described in the above technical solution in an electrocatalytic oxygen reduction reaction.
[0047] The room temperature in the embodiments of the present invention refers to "25±2°C".
[0048] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.
[0049] Examples 1-3
[0050] A method for preparing a MoP@Mn-SAC oxygen reduction electrocatalyst:
[0051] (1) Preparation of zinc nitrate solution: 0.89 g of zinc nitrate hexahydrate was weighed and dissolved in 30 mL of deionized water, and then 16 mg of CTAB powder was added. The mixture was ultrasonicated for 10 min and stirred for 20 min to obtain a zinc nitrate solution containing CTAB.
[0052] (2) Preparation of 2-methylimidazole solution: 165 mmol of 2-methylimidazole was weighed and dissolved in 150 mL of deionized water, and stirred for 20 min to obtain a 2-methylimidazole solution.
[0053] (3) Polymerization reaction: Pour the CTAB-containing zinc nitrate solution obtained in step (1) into the 2-methylimidazole solution obtained in step (2), stir for 2 h at 60° C., let stand for 2 h, then centrifuge, and then freeze-dry for 6 h to obtain a ZIF-8 precursor.
[0054] (4) Carbonization treatment: The ZIF-8 precursor obtained in step (3) was placed in a porcelain boat, heated to 1000° C. in an argon atmosphere, maintained for 2 h, and naturally cooled to room temperature to obtain a nitrogen-doped carbon material with a nanocube morphology, denoted as NC.
[0055] (5) Ion adsorption reaction: 50 mg of NC obtained in step (4) was placed in 30 mL of aqueous solution containing 0.075 mmol of manganese nitrate trihydrate and 0.0375 mmol (Example 1, recorded as 0.5-MoP@Mn-SAC), 0.075 mmol (Example 2, recorded as 1.0-MoP@Mn-SAC or MoP@Mn-SAC-1000) or 0.1125 mmol (Example 3, recorded as 1.5-MoP@Mn-SAC) of ammonium molybdate, and slowly stirred at 60°C for 12 h. After centrifugation, the mixture was dried at 60°C for 6 h to obtain NC adsorbing two metal ions.
[0056] (6) Phosphation treatment: The NC adsorbing two metal ions obtained in step (5) was mixed with an equal mass of red phosphorus, ground and placed in a porcelain boat, heated to 1000°C under an argon atmosphere, maintained for 2 hours, and naturally cooled to room temperature to obtain a Mn single-atom electrocatalyst loaded with MoP nanoparticles, namely, MoP@Mn-SAC oxygen reduction electrocatalyst.
[0057] Example 4
[0058] The difference from Example 2 is that in step (6), heating to 900° C. under argon atmosphere is maintained for 2 h, and the remaining steps are the same as Example 2, denoted as MoP@Mn-SAC-900.
[0059] Example 5
[0060] The difference from Example 2 is that in step (6), heating to 1100° C. under argon atmosphere is maintained for 2 h, and the remaining steps are the same as Example 2, denoted as MoP@Mn-SAC-1100.
[0061] Comparative Example 1
[0062] A method for preparing a Mn-SAC electrocatalyst:
[0063] The difference from Example 2 is that in step (5), manganese nitrate trihydrate is not added, and the remaining steps are the same as Example 2.
[0064] Comparative Example 2
[0065] A method for preparing MoP@NC electrocatalyst:
[0066] The difference from Example 2 is that in step (5), ammonium molybdate is not added, and the remaining steps are the same as Example 2.
[0067] Comparative Example 3
[0068] A method for preparing ZIF-8 derived phosphorus and nitrogen co-doped carbon nanocube electrocatalyst:
[0069] The difference from Example 2 is that in step (5), manganese nitrate trihydrate and ammonium molybdate are not added, and the remaining steps are the same as Example 2, denoted as PNC.
[0070] Effect Example 1
[0071] (1) The X-ray powder diffraction patterns of MoP@Mn-SAC prepared in Example 2, Mn-SAC prepared in Comparative Example 1, MoP@NC prepared in Comparative Example 2, and NC in step (4) of Example 2 are shown in FIG. Figure 1 , where a is MoP@Mn-SAC, b is Mn-SAC, c is MoP@NC, and d is NC. Figure 1 It can be seen that the MoP@Mn-SAC prepared in Example 2 is the same as the MoP@NC prepared in Comparative Example 2, both having typical MoP and single carbon diffraction peaks, and the NC prepared in step (4) of Example 2 and the Mn-SAC prepared in Comparative Example 1 both have typical carbon peaks.
[0072] (2) Characterization diagram of MoP@Mn-SAC prepared in Example 2 Figure 2 , where a is the scanning electron microscope image of NC, b is the scanning electron microscope image of MoP@Mn-SAC, c is the transmission electron microscope image of MoP@Mn-SAC, d is the high-resolution transmission electron microscope image of MoP@Mn-SAC, e is the corresponding lattice spacing distribution in the high-resolution transmission electron microscope image of MoP@Mn-SAC, f is the crystal and atomic structure of MoP@Mn-SAC and the corresponding lattice spacing, and g is the element distribution map of MoP@Mn-SAC.
[0073] from Figure 2 a and Figure 2 As can be seen in b, both NC and MoP@Mn-SAC exhibit nanocube morphology. Figure 2 As can be seen in Figure c, MoP@Mn-SAC has a nanocube morphology with clear boundaries and a size less than 300 nm. Figure 2 d to Figure 2 f shows that nanoparticles are distributed on the MoP@Mn-SAC nanocubes, and the lattice fringes of the nanoparticles are 0.215nm and 0.219nm, respectively, corresponding to the MoP (101) crystal plane. No obvious lattice fringes belonging to manganese-based species can be seen in the image, which means that manganese is embedded in the carbon framework, which is consistent with the XRD results. Figure 2 As can be seen from Figure 5, manganese, molybdenum, phosphorus and nitrogen are evenly distributed in the carbon matrix.
[0074] (3) The X-ray photoelectron spectrum of MoP@Mn-SAC prepared in Example 2 and the extended X-ray absorption fine structure spectrum of Mn in MoP@Mn-SAC are shown in Figure 3 , where a is the 1s spectrum of C, b is the 2p spectrum of Mn, c is the 3d spectrum of Mo, d is the 1s spectrum of N, e is the 2p of P, and f is the extended X-ray absorption fine structure spectrum of Mn in MoP@Mn-SAC.
[0075] from Figure 3 It can be seen from a that there are CN and CP chemical bonds in the MoP@Mn-SAC prepared in Example 2; Figure 3 As can be seen from b, Mn is mainly in the form of Mn 3+ and Mn 2+ Existence; from Figure 3 As can be seen from c, Mo is mainly Mo 6+ and Mo 3+ Existence; from Figure 3 As can be seen in d, there is a metal-nitrogen chemical bond (MN x / MN); from Figure 3 As can be seen from e, metal phosphides exist in MoP@Mn-SAC; Figure 3 As can be seen in f, there is a Mn-N bond in MoP@Mn-SAC; the above confirms the successful synthesis of Mn single atoms and MoP, and the coupling of single atoms with nanoparticles can improve the intrinsic catalytic activity of the catalyst.
[0076] (4) The electron paramagnetic resonance spectra of MoP@Mn-SAC prepared in Example 2, NC prepared in step (4) of Example 2, Mn-SAC prepared in Comparative Example 1, MoP@NC prepared in Comparative Example 2, and PNC prepared in Comparative Example 3 are shown in FIG. Figure 4 .
[0077] from Figure 4It can be seen that the MoP@Mn-SAC prepared in Example 2 and the Mn-SAC prepared in Comparative Example 1 showed signals related to unpaired electrons when g=2.035, and the NC prepared in step (4) of Example 2, the MoP@NC prepared in Comparative Example 2, and the PNC prepared in Comparative Example 3 did not show signals related to unpaired electrons, indicating that the introduction of Mn has an important influence on the formation of unpaired electrons, and the EPR signal is enhanced with the coupling of MoP, indicating that the coupling of MoP will increase the number of unpaired electrons, and the number of unpaired electrons can adjust the electronic structure of the catalyst and the adsorption energy of the catalytic intermediates at the catalytic active sites, thereby further improving the electrocatalytic oxygen reduction activity.
[0078] Effect Example 2
[0079] Electrochemical testing
[0080] (1) Electrocatalytic oxygen evolution test: Electrochemical oxygen reduction test was performed on an electrochemical workstation (Shanghai CHI 760E and American PINE) using a three-electrode system. The test results are shown in Figure 5 . The catalysts prepared in Examples 1-5 and Comparative Examples 1-3 were respectively drop-coated on a glassy carbon electrode as a working electrode, a carbon rod as a counter electrode, and a saturated silver / silver chloride electrode as a reference electrode. The electrolyte was a 0.1 mol / L potassium hydroxide aqueous solution. The test was carried out at 25°C, the scan rate was 10 mV / s, and the voltage scan interval was set to -0.9 to -0.2 V. The electrode potential was measured relative to a saturated silver / silver chloride electrode and converted to a value relative to a reversible hydrogen electrode (RHE). The electrode potential was measured at a silver / silver chloride electrode and converted to a reversible hydrogen electrode (RHE) by the following Nernst equation: E RHE =E Ag / AgCl +0.196+0.059pH.
[0081] The linear scan curves of electrocatalytic oxygen reduction of NC prepared in step (4) of Example 2, MoP@Mn-SAC prepared in Example 2, Mn-SAC prepared in Comparative Example 1, MoP@NC prepared in Comparative Example 2 and commercial Pt / C electrode are shown in FIG. Figure 5 a; The linear scanning curve of electrocatalytic oxygen reduction of MoP@Mn-SAC prepared in Examples 2 and 4-5 is shown in Figure 5 b; The linear scanning curve of electrocatalytic oxygen reduction of MoP@Mn-SAC prepared in Example 1-3 is shown in Figure 5 c; The linear scan curves of electrocatalytic oxygen reduction of NC prepared in step (4) of Example 2, MoP@Mn-SAC prepared in Example 2, and PNC prepared in Comparative Example 3 are shown in FIG. Figure 5 d; Hydrogen peroxide (H2O2) of MoP@Mn-SAC prepared in Example 2, Mn-SAC prepared in Comparative Example 1, and MoP@NC prepared in Comparative Example 22 O 2 ) yield and electron transfer number (n) see Figure 5 e; The stability test results of MoP@Mn-SAC and commercial Pt / C electrodes prepared in Example 2 are shown in Figure 5 f, Figure 5 The 98% and 83% in f refer to the percentage of the performance after 10 h to the performance at 0 h.
[0082] from Figure 5 It can be seen from a that the MoP@Mn-SAC prepared in Example 2 has excellent electrocatalytic oxygen reduction catalytic performance in 0.1 mol / L potassium hydroxide solution; Figure 5 As can be seen from b, the MoP@Mn-SAC prepared in Example 2, that is, when the phosphating temperature is 1000°C, exhibits the best electrochemical oxygen reduction performance; Figure 5 As can be seen from Fig. 3, the MoP@Mn-SAC prepared in Example 2 exhibits the best electrochemical oxygen reduction performance when the amount of ammonium molybdate added is 0.075 mmol. Figure 5 d, it can be seen that the MoP@Mn-SAC prepared in Example 2 exhibits electrochemical oxygen reduction performance superior to that of PNC and NC. Figure 5 It can be seen from Figure 2 that the MoP@Mn-SAC prepared in Example 2 has good electronic electrocatalytic oxygen reduction performance; Figure 5 As can be seen from Fig. 5, the MoP@Mn-SAC prepared in Example 2 is 2 After running stably for 10 hours, there is no obvious performance degradation, showing good stability.
[0083] (2) Solid-state zinc-air battery test: The zinc-air battery test was carried out on an electrochemical workstation (Shanghai CHI 760E) and a blue battery test system (BT2016A). The MoP@Mn-SAC prepared in Example 2 or commercial Pt / C electrode was mixed with an equal mass of RuO 2 (as an electrocatalyst for cathode OER reaction) The mixture obtained after mixing was used as the air cathode of the solid-state zinc-air battery, the zinc plate was used as the anode, and a mixed solution of 6 mol / L potassium hydroxide and 0.2 mol / L zinc acetate was used as the electrolyte, and the test temperature was 25° C. The power density was calculated according to the following equation: P = UI.
[0084] The model diagram of the solid-state zinc-air battery and the voltage of the solid-state zinc-air battery of MoP@Mn-SAC prepared in Example 2 are shown in Figure 6 ; Where a is the model diagram and b is the voltage diagram. Figure 6 b It can be seen that the voltage of the solid zinc-air battery of MoP@Mn-SAC prepared in Example 2 is 1.5653V.
[0085] The performance test results of the solid-state zinc-air battery of MoP@Mn-SAC and commercial Pt / C electrode prepared in Example 2 are shown in Figure 7 , where a is the battery open circuit voltage test result, b is the power density test result, and c is the stability test result.
[0086] from Figure 7 It can be seen from a that the zinc-air battery assembled using the MoP@Mn-SAC prepared in Example 2 has a larger zinc-air battery open circuit voltage, which is better than the zinc-air battery assembled using the commercial Pt / C electrode; Figure 7 As can be seen from b, the zinc-air battery assembled with MoP@Mn-SAC prepared in Example 2 exhibits a greater peak power density, which is better than the commercial Pt / C electrode; Figure 7 As can be seen from Fig. 3, the performance of the zinc-air battery assembled with the MoP@Mn-SAC prepared in Example 2 showed almost no degradation after continuous operation for 840 h, which proves that the MoP@Mn-SAC prepared in the present invention has good application prospects in the field of zinc-air batteries.
[0087] (3) Flexible zinc-air battery test: The flexible zinc-air battery test was carried out on an electrochemical workstation (Shanghai CHI760E) and a blue battery test system (BT2016A). The MoP@Mn-SAC prepared in Example 2 or commercial Pt / C electrode was mixed with an equal mass of RuO 2 (as an electrocatalyst for cathode OER reaction) was mixed and dispersed on carbon cloth as the air cathode of flexible zinc-air battery. 5g of polyvinyl alcohol was dissolved in 50mL of deionized water and stirred at 90℃ for 1.5h to obtain a gel polymer electrolyte. Then 18M KOH and 0.02M Zn(CH 3 COO 2 The mixed solution was poured into the gel polymer electrolyte, stirred for 30 minutes, and frozen at -20°C to form an electrolyte gel. Finally, the prepared electrolyte gel, air cathode and a polished zinc foil were assembled into a flexible zinc-air battery.
[0088] The model diagram of the flexible zinc-air battery and the voltage of the flexible zinc-air battery of MoP@Mn-SAC prepared in Example 2 at different temperatures are shown in Figure 8 ; Where a is the model diagram and b is the voltage diagram. Figure 8 b It can be seen that at 0, 45°C and 90°C, the voltage of the flexible zinc-air battery of MoP@Mn-SAC prepared in Example 2 is basically the same.
[0089] The performance test results of the flexible zinc-air battery of MoP@Mn-SAC and commercial Pt / C electrode prepared in Example 2 are shown in Fig. 9 , where a is the open circuit voltage test curve of the flexible zinc-air battery (the inset is a photo of the assembled flexible zinc-air battery lighting up the LED board), b is the polarization curve and power density curve of the flexible zinc-air battery, and c is the long-term stability of the flexible zinc-air battery.
[0090] from Fig. 9 It can be seen from a that the flexible zinc-air battery assembled using the MoP@Mn-SAC prepared in Example 2 has a larger zinc-air battery open circuit voltage, which is better than the zinc-air battery assembled using the commercial Pt / C electrode; Fig. 9 As can be seen from b, the flexible zinc-air battery assembled with MoP@Mn-SAC prepared in Example 2 exhibits a greater peak power density, which is better than the commercial Pt / C electrode; Fig. 9 As can be seen from Figure c, the performance of the flexible zinc-air battery assembled with the MoP@Mn-SAC prepared in Example 2 showed almost no degradation after continuous operation for 12 h, while the performance of the flexible zinc-air battery assembled with the commercial Pt / C electrode began to decline after continuous operation for 8 h, confirming that the MoP@Mn-SAC prepared in the present invention has good application prospects in the field of flexible zinc-air batteries.
[0091] By comparing the NC prepared in step (4) of Example 2, the MoP@Mn-SAC prepared in Example 2, the MoP prepared in Comparative Example 1, the Mn-SAC prepared in Comparative Example 2, the PNC prepared in Comparative Example 3, the MoP@Mn-SAC with different phosphating temperatures prepared in Examples 2 and 4-5, and the MoP@Mn-SAC with different MoP loadings prepared in Examples 1-3, it was found that the MoP@Mn-SAC prepared in Example 2 exhibited electrocatalytic reduction performance (including the maximum half-wave potential and limiting current density) that was superior to that of commercial Pt / C under alkaline conditions, lower hydrogen peroxide yield, and superior stability.
[0092] Through the above research, it is found that the MoP@Mn-SAC oxygen reduction electrocatalyst prepared in Example 2 of the present invention has excellent electrocatalytic oxygen reduction performance under alkaline conditions and a long service life. It also shows excellent power density and good stability in solid-state and flexible zinc-air battery performance tests, showing practical application potential in the field of zinc-air batteries.
[0093] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a MoP@Mn-SAC oxygen reduction electrocatalyst, characterized in that: The following steps are involved: (1) subjecting ZIF-8 to high temperature carbonization to obtain NC nanocubes; (2) placing the NC nanocubes obtained in step (1) in a mixed solution of a manganese source and a molybdenum source to carry out an ion adsorption reaction, and then mixing with a phosphorus source to carry out a phosphating treatment to obtain the MoP@Mn-SAC oxygen reduction electrocatalyst.
2. The preparation method according to claim 1, characterized in that: In step (1), the preparation method of ZIF-8 comprises the following steps: mixing hexadecyltrimethylammonium bromide and zinc salt solution, then adding 2-methylimidazole, and performing polymerization reaction to obtain ZIF-8.
3. The preparation method according to claim 2, characterized in that: The molar ratio of the hexadecyltrimethylammonium bromide, the zinc salt in the zinc salt solution and 2-methylimidazole is 0.15:1:55; and the concentration of the zinc salt solution is 0.1 mmol / mL.
4. The preparation method according to claim 1, characterized in that: In step (1), the temperature of the high-temperature carbonization treatment is 1000° C., and the time of the high-temperature carbonization treatment is 2 hours.
5. The preparation method according to claim 1, characterized in that: In step (2), the dosage ratio of the NC nanocubes to the manganese source is 50 mg: 0.075 mmol; the molar ratio of the manganese source to the molybdenum source in the mixed solution of the manganese source and the molybdenum source is 1: (0.5-1.5); the manganese source includes manganese nitrate, and the molybdenum source includes ammonium molybdate.
6. The preparation method according to claim 1, characterized in that: In step (2), the temperature of the ion adsorption reaction is 60° C., and the time of the ion adsorption reaction is 12 h.
7. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of the phosphorus source to the NC nanocubes is 1:1; and the phosphorus source includes red phosphorus.
8. The preparation method according to claim 1, characterized in that: In step (2), the temperature of the phosphating treatment is 900-1100° C., and the time of the phosphating treatment is 2 hours.
9. The MoP@Mn-SAC oxygen reduction electrocatalyst prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the MoP@Mn-SAC oxygen reduction electrocatalyst according to claim 9 in an electrocatalytic oxygen reduction reaction.