Preparation method of composite manganese-based lithium battery suitable for being used in wide temperature range

By combining lithium manganese oxide and lithium manganese iron phosphate and optimizing the process, a composite manganese-based lithium battery suitable for use in a wide temperature zone was prepared, which solved the problem of insufficient performance of lithium batteries in low temperature environments, and achieved the -20 Stable and efficient energy output from °C to 55°C.

CN119092837AActive Publication Date: 2024-12-06SHENYANG KINGPOWER TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411197951.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The performance of existing lithium batteries in low temperature environments is poor, especially the poor low temperature performance of lithium iron phosphate batteries, poor safety performance of ternary lithium batteries and poor cycle life of lithium manganate batteries, which seriously affects new energy vehicles. promotion and use.

Method used

Using the preparation method of composite manganese-based lithium battery, by combining lithium manganese oxide and lithium manganese iron phosphate, optimizing the ratio, combining the use of conductive agents, binders and organic solvents, we prepare suitable for use in wide temperature zones. The positive and negative electrode materials are made of polypropylene separators and specific electrolytes to improve battery performance through vacuum baking and liquid injection processes.

Benefits of technology

It significantly improves the discharge performance and energy density of lithium batteries under low temperature conditions, and at the same time enhances the stability and safety of harsh conditions such as high temperature and overcharge, so that the battery's energy output efficiency in an environment of -20℃ is increased to 80.8%. , reach 69.3% at -40°C environment, and maintain 100% energy output efficiency under high temperature environment of 55°C.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092837A_ABST
    Figure CN119092837A_ABST
Patent Text Reader

Abstract

The invention relates to the field of lithium ion battery manufacturing, in particular to a preparation method of a composite manganese-based lithium battery suitable for being used in a wide temperature range. The method comprises the following steps: preparing a positive electrode, preparing a negative electrode and preparing the composite manganese-based lithium battery, namely sequentially preparing positive electrode slurry, a positive electrode roll material and a positive plate from lithium manganate, lithium iron manganese phosphate, a conductive agent, a binding agent and the like, and sequentially preparing negative electrode slurry, a negative electrode roll material and a negative plate from artificial graphite, a thickening agent, the conductive agent, the binding agent and the like; a core package composed of the two positive plates, the two negative plates and the diaphragms is subjected to continuous ultrasonic welding and loaded into the aluminum shell, the cover plate and the aluminum shell are fused into a whole through laser welding, and the composite manganese-based lithium battery suitable for being used in the wide temperature range is prepared through liquid injection, formation and aging and can continuously and stably work in the wide temperature range of-40 DEG C to 55 DEG C; the problems that a lithium iron phosphate battery is low in energy density and poor in low-temperature performance, a ternary lithium battery is poor in safety and cannot be punctured, and a lithium manganate battery is poor in cycle performance are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lithium ion battery manufacturing, and in particular to a method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range. Background Art

[0002] In recent years, lithium-ion batteries have been continuously updated and upgraded, their electrical performance has gradually improved, and their adaptability to the environment has been strengthened. They have been widely used in mechanical processing, automobile manufacturing, electronic product production, new energy industry and other fields. The current mainstream lithium batteries in the market include lithium iron phosphate batteries with artificial graphite as the negative electrode, ternary, lithium manganese oxide batteries and lithium batteries with lithium titanate as the negative electrode. There are currently the following problems: lithium iron phosphate batteries with artificial graphite as the negative electrode have good cycle life and safety performance, low energy density and poor low-temperature discharge performance; ternary lithium batteries with artificial graphite as the negative electrode have high energy density, good low-temperature discharge performance, poor cycle life and safety performance; lithium manganese oxide batteries with artificial graphite as the negative electrode have high energy density, good low-temperature discharge performance and safety, and poor cycle life; lithium titanate as the negative electrode has good cycle life and low-temperature charge and discharge performance, but poor energy density and cost performance. Due to the cold winter in northern my country, the discharge energy of lithium batteries drops sharply, which seriously hinders the promotion and use of new energy vehicles in Northeast and Northwest my country. At present, the discharge energy of conventional lithium iron phosphate system lithium batteries at -20℃ is equivalent to 36% of the discharge energy at 25℃, and the cruising range of electric vehicles is seriously reduced. In view of the current problems, a preparation method of lithium batteries with comprehensive advantages in environmental temperature adaptability is urgently needed. Summary of the invention

[0003] In view of the current disadvantages of poor low-temperature performance of lithium iron phosphate, poor safety performance of ternary lithium batteries that cannot pass the needle puncture test, and poor cycle performance of lithium manganese oxide batteries, the purpose of the present invention is to provide a preparation method for a composite manganese-based lithium battery that is suitable for use in a wide temperature range of -40°C to 55°C and has stable and reliable performance while taking into account safety performance. By composite blending and optimizing the ratio of the positive electrode main materials lithium manganese oxide and lithium iron manganese phosphate, the problems of poor low-temperature performance and low energy density of existing lithium iron phosphate positive electrode materials and poor safety of ternary positive electrode materials are solved.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] A method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range, characterized by the following steps:

[0006] The first step is cathode preparation

[0007] (1) First, according to the mass ratio of lithium manganese oxide (LiMn2O4): lithium iron manganese phosphate (LiMn 0.6 Fe0.4 PO4): conductive agent: binder = 74-78:18-22:2-4:1.6-2, added into a stirring tank; then an organic solvent is added and kneaded to make the solid content of the slurry in the stirring tank 70-80wt%, and at the same time, the stirring speed is 30-42rad / min and the dispersion speed is 2200-3200rad / min, and the duration is 2-3h; the organic solvent is continued to be added to make the solid content of the slurry in the stirring tank 65-75wt%, and at the same time, the stirring speed is 30-42rad / min and the dispersion speed is 2200-3200rad / min, and the duration is 0.5-2 hours; finally, the mixture is dispersed evenly to obtain a positive electrode slurry with a viscosity of 7000-8000mPa·s;

[0008] (2) The positive electrode slurry is filtered through a filter with a mesh size of 120 to 150. After filtering, the single-side surface density is 18 to 24.5 mg / cm according to a continuous coating method. 2 , double-sided surface density is 36~49mg / cm 2 The positive electrode coil is evenly coated on both sides of the positive electrode current collector, the positive electrode current collector is a carbon-coated aluminum foil, and the thickness of the carbon-coated aluminum foil is 12 to 18 μm, so as to obtain a positive electrode coil;

[0009] (3) The positive electrode coil is rolled using a roller mill at a temperature of 2.6 to 2.9 g / cm 3 The positive electrode coils are rolled to a compaction density of 1000 nm, and are slit into two positive electrode coils of equal width in the middle using a slitting machine. A metal die-cutting machine is used to punch out positive electrode sheets for each positive electrode coil to obtain positive electrode sheets of suitable size and shape.

[0010] Step 2: Negative electrode preparation

[0011] (1) First, artificial graphite, thickener, and conductive agent are added to a stirring tank according to the mass ratio of artificial graphite: thickener: conductive agent: binder = 94-95.5:1.2-1.5:1.5-1.9:1.5-2; then solvent is added for mixing to make the solid content of the slurry in the stirring tank 45-50wt%, and at the same time, the stirring speed is 28-32rad / min and the dispersion speed is 2200-3200rad / min, and the duration is 2-3h; the solvent is continued to be added, The solid content of the slurry in the stirring kettle is set to 40-46wt%, and the stirring speed is set to 28-32rad / min and the dispersion speed is set to 2200-3200rad / min for 0.5-2h. Finally, a binder is added, and the stirring speed is adjusted to 10-30rad / min and the dispersion speed is adjusted to 1000-2000rad / min for 0.5-1h. The slurry is evenly dispersed to obtain a negative electrode slurry with a viscosity of 3000-5000mPa·s.

[0012] (2) The negative electrode slurry is passed through a 150-200 mesh sieve, filtered and then coated, with a single-side surface density of 8-10.5 mg / cm 2 , double-sided surface density is 16-21 mg / cm 2 The slurry is evenly coated on both sides of the negative electrode current collector, the negative electrode current collector is a copper foil with a thickness of 6 to 8 μm, and a negative electrode coil is prepared;

[0013] (3) The above negative electrode coil is rolled by a roller mill to obtain a pressure of 1.4 to 1.5 g / cm 3 The compaction density is rolled, and the negative electrode sheet is punched using a full-page die-cutting laser knife die to produce a negative electrode sheet with a suitable size and shape;

[0014] Step 3: Preparation of composite manganese-based lithium battery

[0015] (1) Using a polypropylene diaphragm to insulate and separate the positive and negative electrode sheets, using a laminating machine to perform a "Z"-shaped lamination and gluing process to form a core package, welding the positive and negative electrode ears of the core package with the positive and negative electrode connecting sheets of the cover plate using an ultrasonic welding machine, installing a stop frame, using an outer vest to wrap and protect the core package as a whole, and placing it into an aluminum shell, pressing the cover plate and the upper edge of the aluminum shell tightly to keep the two in an interference fit state, and using a laser welding machine to melt and weld the cover plate and the upper edge of the aluminum shell into a whole, thereby assembling a non-liquid-injected assembly;

[0016] (2) The above-mentioned unfilled assembly is vacuum baked, the baking temperature is set to 80-90°C, the vacuum degree is -90-98KPa, and the baking time is 36-48h. After the baking is completed, the unfilled assembly is filled with liquid using a liquid filling machine at a liquid filling coefficient of 4.6-5.2g / Ah in a dry air atmosphere with a dew point of -35°C to -45°C, and is allowed to stand at 35-45°C for 24-48h to achieve sufficient infiltration of the electrolyte into the positive and negative electrode sheets and the separator to form a battery cell;

[0017] (3) Using a formation device to charge and activate the battery cell, the formation method is open formation;

[0018] (4) Open circuit aging;

[0019] (5) After the aging is completed, the battery cell is subjected to a capacity test to obtain the capacity and internal resistance performance parameters of the battery cell. After the test is completed, a composite manganese-based lithium battery suitable for use in a wide temperature range is obtained.

[0020] In the preparation method of the composite manganese-based lithium battery suitable for use in a wide temperature range, during the preparation of the positive electrode, the conductive agent selected is one of conductive carbon black, superconducting carbon black, and Ketjen black; the binder selected is polyvinylidene fluoride; and the organic solvent selected is N-methylpyrrolidone.

[0021] The method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range, in the process of preparing the negative electrode, the conductive agent selected is two of conductive carbon black, superconducting carbon black, Ketjen black, and carbon nanotubes; the thickener selected is sodium carboxymethyl cellulose, the binder selected is styrene-butadiene rubber; and the solvent selected is deionized water.

[0022] The method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range, during the preparation of the composite manganese-based lithium battery, the polypropylene diaphragm selected is a dry high-porosity diaphragm with a diaphragm thickness of 12 to 25 μm and a diaphragm porosity of 40 to 45%.

[0023] The method for preparing the composite manganese-based lithium battery suitable for use in a wide temperature range, in the process of preparing the composite manganese-based lithium battery, the size of the selected polypropylene diaphragm is: 20 μm in thickness and 129 mm in width.

[0024] The method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range, during the preparation of the composite manganese-based lithium battery, the electrolyte for liquid injection into the uninjected assembly: the solvent is selected from two of ethylene carbonate, dimethyl carbonate, propylene carbonate, and ethyl methyl carbonate, and the lithium salt is one or two of lithium hexafluorophosphate, lithium tetrafluoroborate, and lithium bistrifluoromethanesulfonyl imide.

[0025] The preparation method of the composite manganese-based lithium battery suitable for use in a wide temperature range, during the preparation process of the composite manganese-based lithium battery, the formation system is 0.05C constant current charging for 3.33h, 0.1C constant current charging for 4.5h, vacuum exhaust at a vacuum degree of -90kPa for 30min, 0.1C constant current charging to 4.2V, and after the above procedures are completed, sealing is performed.

[0026] The method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range, during the preparation process of the composite manganese-based lithium battery, the aging temperature of open circuit aging is 45° C., and the aging time is 72 hours.

[0027] The performance of lithium batteries is closely related to the selected positive electrode material. The design concept of the present invention is as follows:

[0028] In view of the deficiencies of existing lithium-ion battery positive electrode materials in low-temperature performance, energy density and safety, the present invention proposes an innovative improvement method. Although the existing lithium iron phosphate positive electrode material has good cycle life and thermal stability, its performance in low-temperature environments is poor and its energy density is low, which limits its use in high-energy density application scenarios. Although ternary positive electrode materials such as lithium nickel cobalt manganese oxide have high energy density and can meet the requirements for battery life, they have defects in safety, especially thermal stability, and are prone to cause safety problems under high temperature or overcharge conditions.

[0029] In order to solve these problems, the present invention proposes to combine lithium manganese oxide (LiMn2O4) and lithium iron manganese phosphate (LiMn 0.6 Fe 0.4 The strategy of composite blending of lithium manganese oxide and lithium iron phosphate (LiMn2O4) is adopted. Through this combination, the high energy density and good electrical conductivity of lithium manganese oxide are utilized, while the excellent thermal stability and safety characteristics of lithium iron manganese phosphate are combined to achieve the effect of performance optimization. Lithium iron manganese phosphate has a dual voltage platform of 4.1V and 3.5V, which can well match the voltage of lithium manganese oxide (LiMn2O4). At the same time, lithium manganese oxide (LiMn2O4) has a spinel structure, and lithium iron manganese phosphate has an olivine structure, and the two have good lattice compatibility. In the mixing process of the composite material, the focus is on optimizing the ratio of lithium manganese oxide and lithium iron manganese phosphate to ensure that the performance advantages of the two materials can complement each other, thereby maximizing the overall performance of the battery. In addition, the electrochemical performance and stability of the material are further improved through process optimization such as surface modification of the material and particle size control. In the end, this design makes the prepared positive electrode material not only significantly improve the discharge performance under low temperature conditions, but also improve the energy density of the battery, while enhancing the stability and safety under harsh conditions such as high temperature and overcharge, meeting the needs of high energy density and high safety application scenarios. Through this innovative design, the present invention provides an effective solution for improving the performance of lithium-ion battery positive electrode materials and has broad application prospects.

[0030] The advantages and beneficial effects of the present invention are:

[0031] 1. The preparation method of the composite manganese-based lithium battery of the present invention uses two positive electrode materials, lithium manganese oxide and lithium iron manganese phosphate, for composite blending, while taking advantage of the performance advantages of lithium manganese oxide, which has a high platform voltage, high energy density, and low cost, and lithium iron manganese phosphate, which has good low-temperature performance, good safety performance, and long cycle life.

[0032] 2. The preparation method of the composite manganese-based lithium battery of the present invention is compatible with the conventional lithium iron phosphate system lithium battery process equipment and process environment standards, which greatly improves the adaptability of the preparation method and the feasibility of introducing mass production.

[0033] 3. The preparation method of the composite manganese-based lithium battery of the present invention achieves that the energy output efficiency of the lithium battery in a low temperature environment or working condition of -20°C is greatly improved (from 36% to 80.8%), while the safety performance and cost consumption of the lithium battery remain basically unchanged. The energy output efficiency in a low temperature environment of -40°C can reach 69.3% and operate stably. At the same time, the energy output efficiency at a high temperature of 55°C remains unchanged (about 100%). BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a diagram of the shape and size of the positive electrode sheet of the present invention.

[0035] Figure 2 This is a diagram of the shape and size of the negative electrode sheet of the present invention.

[0036] Figure 3 The cross-sectional schematic diagram of the core package structure of the present invention includes: (a) a front view, (b) a top view, and (c) a side view.

[0037] Figure 4 It is a schematic diagram of ultrasonic welding of the positive and negative electrode ears of the core package with the positive and negative electrode connecting pieces of the cover plate of the present invention.

[0038] Figure 5 The diagram is a schematic diagram of the internal structure of the non-liquid-filled assembly of the present invention, wherein (a) is a front view, (b) is a side view, and (c) is a cross-sectional view.

[0039] Figure 1-Figure 5 In the figure, the reference numerals are: 1 positive electrode sheet (11 positive electrode ear), 2 negative electrode sheet (21 negative electrode ear), 3 diaphragm, 4 core package, 5 cover plate, 6 pole column, 7 cover plate connecting piece, 8 pole ear, 9 ultrasonic welding head, 10 aluminum shell.

[0040] Figure 6 It is a schematic diagram comparing the normal temperature (25°C) vs. high temperature (55°C) 0.5C discharge performance curves of the present invention.

[0041] Figure 7-Figure 8 This is a schematic diagram comparing the normal temperature vs. low temperature 0.5C discharge performance curves of the present invention. Figure 7 It is a composite manganese-based lithium battery. Figure 8 It is a conventional lithium iron phosphate battery.

[0042] Figure 9-10 This is a schematic diagram of the comparison of the discharge energy at room temperature vs. low temperature 0.5C of the present invention. Figure 7 It is a composite manganese-based lithium battery. Figure 8 It is a conventional lithium iron phosphate battery. DETAILED DESCRIPTION

[0043] In order to better understand the structure and performance of the present invention, the present invention is further described in detail through embodiments and drawings.

[0044] Example 1

[0045] In this embodiment, a method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range includes the following steps:

[0046] 1. Cathode preparation

[0047] First, according to the mass ratio of lithium manganese oxide (LiMn2O4): lithium iron manganese phosphate (LiMn 0.6 Fe 0.4PO4): conductive agent: binder = 76.8:19.2:2.2:1.8, take 6.4kg of lithium manganese oxide, 1.6kg of lithium iron manganese phosphate, 0.183kg of conductive carbon black, and 0.15kg of polyvinylidene fluoride (PVDF), and add them into a stirring tank; then add 2.08kg of organic solvent N-methylpyrrolidone to make the solid content of the slurry in the stirring tank 80wt%, and start the stirring speed of 30rad / min and the dispersion speed of 2500rad / min at the same time, and last for 2.5h; continue to add 1.49kg of organic solvent N-methylpyrrolidone to make the solid content of the slurry in the stirring tank 70wt%, and start the stirring speed of 35rad / min and the dispersion speed of 2500rad / min at the same time, and last for 2 hours; finally disperse evenly to obtain a positive electrode slurry with a viscosity of 7600mPa·s;

[0048] The positive electrode slurry was filtered through a 150-mesh filter. After filtering, the single-side surface density was 24.25 mg / cm 2 , double-sided density 48.5mg / cm 2 The positive electrode coil is evenly coated on both sides of the positive electrode current collector, the positive electrode current collector is a carbon-coated aluminum foil, the carbon coating layer thickness is 1 μm, and the total thickness of the carbon-coated aluminum foil is 15 μm, to obtain a positive electrode coil;

[0049] The positive electrode coil was rolled using a roller mill at 2.89 g / cm 3 The compaction density is rolled, and a slitting machine is used to cut the positive electrode coils into two equal widths in the middle. A hardware die-cutting machine is used to punch out the positive electrode sheets for each positive electrode coil to obtain positive electrode sheets with shapes and sizes such as Figure 1 .

[0050] 2. Negative electrode preparation

[0051] According to the mass ratio of artificial graphite: thickener: conductive agent: binder = 95.05:1.4:1.85:1.7, 5kg of artificial graphite, 0.074kg of sodium carboxymethyl cellulose, and 0.097kg of conductive agent were taken and added into the stirring tank; then 5.4kg of deionized water was added for mixing, so that the solid content of the slurry in the stirring tank was 47.4wt%, and the stirring speed was turned on at 28rad / min and the dispersion speed was turned on at 2800rad / min for 2.5h; 0.56kg of deionized water was continued to be added to make the solid content of the slurry in the stirring tank 45.1wt%, and the stirring speed was turned on at 28rad / min and the dispersion speed was turned on at 2800rad / min for 1h, and the slurry was evenly dispersed; finally, 0.179kg of styrene-butadiene rubber with a solid content of 50wt% was added, the stirring speed was adjusted to 20rad / min, the dispersion speed was adjusted to 1500rad / min, and the duration was 0.5h to obtain a negative electrode slurry with a viscosity of 3500mPa·s.

[0052] The negative electrode slurry was passed through a 200-mesh sieve and filtered before coating. The single-sided surface density was 8.3 mg / cm 2 , double-sided surface density is 16.6mg / cm 2 The slurry is evenly coated on both sides of the negative electrode current collector, the negative electrode current collector is a copper foil with a thickness of 6 μm, and a negative electrode coil is prepared;

[0053] The above negative electrode coil is rolled by a roller mill at 1.5 g / cm 3 The compaction density is rolled, and the negative electrode sheet is punched using a full-page die-cutting laser knife die to make a negative electrode sheet with a shape and size such as Figure 2 .

[0054] 3. Preparation of composite manganese-based lithium battery

[0055] The positive and negative electrodes are insulated and separated by a conventional polypropylene diaphragm (diaphragm thickness 20 μm, width 129 mm), and a laminating machine is used to perform a "Z"-shaped lamination and glue application process to form a core package ( Figure 3 ), and then weld the positive and negative tabs of the core package and the positive and negative connecting pieces of the cover plate together using an ultrasonic welding machine ( Figure 4 ), then install the stop frame, use the outer vest to wrap the core package as a whole for protection, install it into the aluminum shell, press the cover plate and the upper edge of the aluminum shell tightly, so that the two maintain an interference fit state, and use a laser welding machine to melt and weld the cover plate and the upper edge of the aluminum shell into a whole, so that the assembly without liquid injection is assembled ( Figure 5 );

[0056] like Figure 3 As shown, the core package 4 structure includes a positive electrode sheet 1, a negative electrode sheet 2 and a separator 3. The positive electrode sheet 1 and the negative electrode sheet 2 are arranged alternately in sequence and insulated and separated by the separator 3. A positive electrode ear 11 is provided at one end of the positive electrode sheet 1, and a negative electrode ear 21 is provided at one end of the negative electrode sheet 2.

[0057] like Figure 4 As shown, when the two core packages 4 are connected, a cover plate connecting piece 7 and a pole 6 are respectively provided on the upper and lower parts of the cover plate 5, and the pole ears 8 of the positive and negative pole connecting pieces on the two core packages 4 are relatively arranged and overlapped with the cover plate connecting piece 7. The ultrasonic welding head 9 of the ultrasonic welding machine moves in the vertical direction to weld the pole ears 8 and the cover plate connecting piece 7, so that continuous ultrasonic welding of the two core packages 4 can be realized.

[0058] like Figure 5 As shown, the structure of the assembly is as follows: two core packages 4 are connected and folded in half and then loaded into the aluminum shell 10, the pole ears 8 of the two core packages 4 and the cover connecting pieces 7 connected to the pole ears 8 are bent separately, the cover plate 5 is located on the inner side of the top of the aluminum shell 10, and the pole 6 is located on the outer side of the top of the aluminum shell 10.

[0059] The uninjected assembly was vacuum baked, the baking temperature was set to 85°C, the relative vacuum degree was -98KPa, and the baking time was 36h. After the baking, the uninjected assembly was injected with liquid using an injection machine in a dry air atmosphere with a dew point of -45°C, with an injection volume of 156g. The assembly was left to stand at 45°C for 24h to achieve sufficient infiltration of the electrolyte into the positive and negative electrode sheets and the diaphragm to form a battery cell.

[0060] In this embodiment, the composition of the electrolyte is as follows: the solvent is selected from ethylene carbonate and dimethyl carbonate (volume ratio is 1:1), the lithium salt is lithium hexafluorophosphate, and the lithium salt concentration is 1 mol / L.

[0061] The battery cell was charged and activated using a formation device. The formation method was open formation. The formation system was 0.05C constant current charging for 3.33h, 0.1C constant current charging for 4.5h, vacuum exhaust (relative vacuum degree -90kPa, time 30min), 0.1C constant current charging to 4.2V. After the above procedures were completed, the battery cell was sealed.

[0062] Open circuit aging, aging temperature is 45℃, aging time is 72h;

[0063] The capacity test showed that the capacity was 28.84Ah and the internal resistance was 0.65mΩ, and a composite manganese-based lithium battery suitable for use in a wide temperature range was obtained.

[0064] This preparation method achieves a significant improvement in the energy output efficiency of lithium batteries in a low-temperature environment or working condition of -20°C (from 36% to 80.8%), while maintaining basically unchanged safety performance and cost consumption. The energy output efficiency can reach 69.3% in a low-temperature environment of -40°C and operate stably. At the same time, the energy output efficiency remains unchanged (about 100%) at a high temperature of 55°C.

[0065] like Figure 6 As shown, the above-mentioned composite manganese-based lithium battery was subjected to 0.5C normal temperature 25°C and high temperature 55°C discharge performance tests. The test results show that the composite manganese-based lithium battery has good discharge performance under high temperature 55°C environment, and its discharge capacity ratio is about 100% compared with that under normal temperature, and the discharge platform voltage is not lower than that under normal temperature.

[0066] like Figure 7-Figure 8As shown, the discharge performance test of the composite manganese-based lithium battery of the present invention is carried out at 0.5C room temperature 25℃, low temperature -20℃, and -40℃, and the discharge performance test of the conventional lithium iron phosphate battery is carried out at 0.5C room temperature 25℃ and low temperature -20℃. By comparing the test results, it can be seen that the discharge capacity ratio of the conventional lithium iron phosphate battery at a low temperature of -20℃ is about 45% compared with the discharge capacity at a normal temperature of 25℃, and the starting discharge voltage at a low temperature of -20℃ is about 2.85V, while the discharge capacity ratio of the composite manganese-based lithium battery at -20℃ and -40℃ is about 98% and 93% compared with the discharge capacity at a normal temperature of 25℃, and the starting discharge voltage at low temperatures of -20℃ and -40℃ is about 3.4V and 2.4V. Compared with the embarrassing situation that the conventional lithium iron phosphate cannot be discharged at a low temperature of -40℃, its low temperature discharge resistance is significantly enhanced.

[0067] like Figure 9-10 As shown, the battery cells of the composite manganese-based lithium battery of the present invention are subjected to 0.5C normal temperature 25°C, low temperature -20°C, and -40°C discharge energy tests, and the battery cells of the conventional lithium iron phosphate battery are subjected to 0.5C normal temperature 25°C, and low temperature -20°C discharge energy tests. By comparing the test results, it can be seen that the discharge energy of the conventional lithium iron phosphate battery at a low temperature of -20°C is about 36% compared with the discharge energy at a normal temperature of 25°C, while the discharge energy of the composite manganese-based lithium battery at -20°C and -40°C is about 80.8% and 69.3% compared with the discharge energy at a normal temperature of 25°C. At low temperatures of -20°C and -40°C, the energy output efficiency of the composite manganese-based lithium battery in low temperature environments is significantly stronger than that of the conventional lithium iron phosphate battery.

[0068] The implementation results show that the present invention adjusts the component ratio of the positive electrode material of the battery and optimizes the surface density design parameters, so that the performance advantages of the positive electrode active material such as low temperature resistance, good safety, low cost and high energy density can be fully utilized. The selection of an adapted wide-temperature electrolyte allows it to stably exert its performance in a wide temperature range, so that the battery can work safely and stably in different temperature environments. The preparation method of the present invention is compatible with the conventional lithium iron phosphate system lithium battery process equipment and process environment standards in the past, which greatly improves the adaptability of the preparation method and the feasibility of introducing mass production. The composite manganese-based lithium battery prepared by the present invention can work continuously and stably in a wide temperature range of -40°C to 55°C, and has excellent performance.

[0069] As described above, the present invention is described by some embodiments, and it is known to those skilled in the art that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited by the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of this application belong to the scope protected by the present invention.

Claims

1. A method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range, characterized in that: Proceed as follows: The first step is cathode preparation (1) First, according to the mass ratio of lithium manganese oxide (LiMn2O4): lithium iron manganese phosphate (LiMn 0.6 Fe 0.4 PO4): conductive agent: binder = 74-78:18-22:2-4:1.6-2, added into a stirring tank; then an organic solvent is added and kneaded to make the solid content of the slurry in the stirring tank 70-80wt%, and at the same time, the stirring speed is 30-42rad / min and the dispersion speed is 2200-3200rad / min, and the duration is 2-3h; the organic solvent is continued to be added to make the solid content of the slurry in the stirring tank 65-75wt%, and at the same time, the stirring speed is 30-42rad / min and the dispersion speed is 2200-3200rad / min, and the duration is 0.5-2 hours; finally, the mixture is dispersed evenly to obtain a positive electrode slurry with a viscosity of 7000-8000mPa·s; (2) The positive electrode slurry is filtered through a filter with a mesh size of 120 to 150. After filtering, the single-side surface density is 18 to 24.5 mg / cm according to a continuous coating method. 2 , double-sided surface density is 36~49mg / cm 2 The positive electrode coil is evenly coated on both sides of the positive electrode current collector, the positive electrode current collector is a carbon-coated aluminum foil, and the thickness of the carbon-coated aluminum foil is 12 to 18 μm, so as to obtain a positive electrode coil; (3) The positive electrode coil is rolled using a roller mill at a temperature of 2.6 to 2.9 g / cm 3 The positive electrode coils are rolled to a compaction density of 1000 nm, and are slit into two positive electrode coils of equal width in the middle using a slitting machine. A metal die-cutting machine is used to punch out positive electrode sheets for each positive electrode coil to obtain positive electrode sheets of suitable size and shape. Step 2: Negative electrode preparation (1) First, artificial graphite, thickener, and conductive agent are added to a stirring tank according to the mass ratio of artificial graphite: thickener: conductive agent: binder = 94-95.5:1.2-1.5:1.5-1.9:1.5-2; then solvent is added for mixing to make the solid content of the slurry in the stirring tank 45-50wt%, and at the same time, the stirring speed is 28-32rad / min and the dispersion speed is 2200-3200rad / min, and the duration is 2-3h; the solvent is continued to be added, The solid content of the slurry in the stirring kettle is set to 40-46wt%, and the stirring speed is set to 28-32rad / min and the dispersion speed is set to 2200-3200rad / min for 0.5-2h. Finally, a binder is added, and the stirring speed is adjusted to 10-30rad / min and the dispersion speed is adjusted to 1000-2000rad / min for 0.5-1h. The slurry is evenly dispersed to obtain a negative electrode slurry with a viscosity of 3000-5000mPa·s. (2) The negative electrode slurry is passed through a 150-200 mesh sieve, filtered and then coated, with a single-side surface density of 8-10.5 mg / cm 2 , double-sided surface density is 16-21 mg / cm 2 The slurry is evenly coated on both sides of the negative electrode current collector, the negative electrode current collector is a copper foil with a thickness of 6 to 8 μm, and a negative electrode coil is prepared; (3) The above negative electrode coil is rolled by a roller mill to obtain a pressure of 1.4 to 1.5 g / cm 3 The compaction density is rolled, and the negative electrode sheet is punched using a full-page die-cutting laser knife die to produce a negative electrode sheet with a suitable size and shape; Step 3: Preparation of composite manganese-based lithium battery (1) Using a polypropylene diaphragm to insulate and separate the positive and negative electrode sheets, using a laminating machine to perform a "Z"-shaped lamination and gluing process to form a core package, using an ultrasonic welding machine to weld the positive and negative electrode ears of the core package with the positive and negative electrode connecting sheets of the cover plate, installing a stop frame, using an outer vest to wrap and protect the core package as a whole, and placing it into an aluminum shell, pressing the cover plate and the upper edge of the aluminum shell tightly to keep the two in an interference fit state, and using a laser welding machine to melt and weld the cover plate and the upper edge of the aluminum shell into a whole, thereby assembling a non-liquid-injected assembly; (2) The above-mentioned unfilled assembly is vacuum baked, the baking temperature is set to 80-90°C, the vacuum degree is -90-98KPa, and the baking time is 36-48h. After the baking is completed, the unfilled assembly is filled with liquid using a liquid filling machine at a liquid filling coefficient of 4.6-5.2g / Ah in a dry air atmosphere with a dew point of -35°C to -45°C, and is allowed to stand at 35-45°C for 24-48h to achieve sufficient infiltration of the electrolyte into the positive and negative electrode sheets and the separator to form a battery cell; (3) Using a formation device to charge and activate the battery cell, the formation method is open formation; (4) Open circuit aging; (5) After the aging is completed, the battery cell is subjected to a capacity test to obtain the capacity and internal resistance performance parameters of the battery cell. After the test is completed, a composite manganese-based lithium battery suitable for use in a wide temperature range is obtained.

2. The method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range according to claim 1, characterized in that: In the process of preparing the positive electrode, the conductive agent selected is one of conductive carbon black, superconducting carbon black and Ketjen black; the binder selected is polyvinylidene fluoride; and the organic solvent selected is N-methylpyrrolidone.

3. The method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range according to claim 1, characterized in that: In the process of preparing the negative electrode, the conductive agents selected are two of conductive carbon black, superconducting carbon black, Ketjen black, and carbon nanotubes; the thickener selected is sodium carboxymethyl cellulose, the binder selected is styrene-butadiene rubber; and the solvent selected is deionized water.

4. The method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range according to claim 1, characterized in that: In the preparation process of composite manganese-based lithium batteries, the polypropylene diaphragm selected is a dry-process high-porosity diaphragm with a diaphragm thickness of 12 to 25 μm and a diaphragm porosity of 40 to 45%.

5. The method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range according to claim 1, characterized in that: During the preparation of composite manganese-based lithium batteries, the polypropylene diaphragm size selected is: 20μm in thickness and 129mm in width.

6. The method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range according to claim 1, characterized in that: During the preparation of the composite manganese-based lithium battery, the electrolyte for liquid injection into the unfilled assembly: the solvent is selected from two of ethylene carbonate, dimethyl carbonate, propylene carbonate, and ethyl methyl carbonate, and the lithium salt is one or two of lithium hexafluorophosphate, lithium tetrafluoroborate, and lithium bis(trifluoromethanesulfonyl)imide.

7. The method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range according to claim 1, characterized in that: During the preparation process of the composite manganese-based lithium battery, the formation system is 0.05C constant current charging for 3.33h, 0.1C constant current charging for 4.5h, vacuum exhaust at a vacuum degree of -90kPa for 30min, 0.1C constant current charging to 4.2V, and after the above procedures are completed, sealing is carried out.

8. The method for preparing a composite manganese-based lithium battery suitable for use in a wide temperature range according to claim 1, characterized in that: During the preparation of the composite manganese-based lithium battery, the aging temperature of the open circuit aging was 45°C and the aging time was 72h.

Citation Information

Patent Citations

  • Preparation method of lithium iron phosphate battery suitable for being used in wide temperature range

    CN114566717A

  • Lithium manganate system lithium ion battery positive electrode and lithium ion battery

    CN115101714A

  • Lithium manganese iron phosphate and lithium manganate mixed positive electrode slurry and lithium battery

    CN115241441A

  • Lithium ion battery and preparation method thereof

    CN118448705A

  • Battery positive electrode material and application thereof

    US20240145715A1