Formation method for improving high-temperature cycle capacity fading of lithium battery
By circulating charge and discharge in lithium batteries, the problem of cyclic attenuation of lithium batteries at high temperatures is solved, the high-temperature performance and capacity retention rate of the battery are improved, and the cost-effectiveness is improved.
Patent Information
- Application Number
- CN202411188140.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
Existing lithium batteries have faster circulating attenuation in high temperature environments, mainly due to the rupture of solid electrolyte interface mask (SEI) and the consumption of lithium by repair, resulting in a decline in battery performance. The existing strategies increase costs and have limited results.
By cycling the lithium battery between 0-25% SOC and controlling the temperature at 45±2°C, the lithium battery is charged from 0SOC to 30% SOC to form a dense and thick SEI film to improve its thermal stability reduce side reactions at high temperatures.
It significantly improves the high-temperature cycling performance of lithium batteries, reduces the initial capacity attenuation problem, enhances the thermal stability of the battery cell, and does not change the existing production process, but only optimizes the process.
Smart Images

Figure CN119092855A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a formation method for improving the high-temperature cycle capacity attenuation of lithium batteries. Background Art
[0002] Energy storage battery applications focus more on economy, and pay more attention to battery cost, cycle life, safety, and full life cycle cost. Lithium iron phosphate batteries dominate the electrochemical energy storage market with their advantages of low production cost, high safety, and long cycle life.
[0003] There is currently little research on the application of LFP / graphite energy storage batteries in special high-temperature scenarios, mainly for staged high-temperature applications rather than long-term use in high-temperature environments. At present, the main strategies known to be used to improve the high-temperature performance of energy storage batteries are concentrated on the electrolyte and the negative electrode, such as adding high-temperature resistant film-forming additives to the electrolyte, and low specific surface area modified graphite to reduce side reactions. However, these strategies have the following problems: ① Multiple modifications of graphite reduce fine powder on the surface of particles, reduce the occurrence of side reactions, and increase process production costs; ② Adding high-temperature film-forming additives such as VC or MMDS, etc., the effect is not great when the addition amount is low, and increasing the addition amount will cause poor performance at room temperature, increased internal resistance and other effects, and limited improvement in the early cycle at high temperature; ③ Make a fuss about the lithium salt of the electrolyte, such as using lithium salts such as LiFSI, which have a high cost.
[0004] The rapid early cycle decay under high temperature environment is mainly due to the irreversible loss of lithium, which is mainly caused by the rupture and repair of SEI and the consumption of Li. Therefore, there is an urgent need for a method that can reduce the Li loss caused by the early SEI damage and repair, make SEI more stable at high temperature, and thus improve the high temperature performance and capacity retention rate of the battery. Summary of the invention
[0005] The first aspect of the present invention provides a formation method for improving the high temperature cycle capacity decay of a lithium battery, the formation method comprising the following steps:
[0006] (1) Charge the lithium battery from 0 SOC to 25% SOC and leave it alone;
[0007] (2) Discharge the lithium battery from 25% SOC to 0 SOC and leave it alone;
[0008] (3) Repeat steps (1) to (2) 2 or more times;
[0009] (4) Charge the lithium battery from 0 SOC to 30% SOC.
[0010] In one or more embodiments, the temperature is controlled at 45 ± 2 °C during the formation process.
[0011] In one or more embodiments, in step (1), the lithium battery is charged from 0 SOC to 25% SOC at a charge rate of 0.05C-0.3C.
[0012] In some embodiments, in step (1), the lithium battery is charged from 0 SOC to 9%-11% SOC and then to 25% SOC in 2-4 stages; preferably, the SOC increase is 1.5%-5% each time the charging is performed.
[0013] In one or more embodiments, in step (1), the lithium battery is charged in stages from 0 SOC to 1.5%-2% SOC, 4%-6% SOC, 9%-11% SOC, and finally to 25% SOC.
[0014] In one or more embodiments, in step (2), the battery is discharged to 0 SOC at a discharge rate of 0.05C-0.2C.
[0015] In one or more embodiments, in step (2), the lithium battery is discharged to a 0SOC cutoff voltage of 2V.
[0016] In one or more embodiments, in step (1), the lithium battery is charged from 0 SOC to 25% SOC in stages, and the specific steps include:
[0017] The first stage: charge the lithium battery from 0 SOC to 1.5-2% SOC, the charging rate range is: 0.04-0.06C, and the charging time is: 10-30min;
[0018] The second stage: charging to 4-6% SOC, charging rate range: 0.04-0.06C, charging time: 30-50min;
[0019] The third stage: charging to 9-11% SOC, charging rate range: 0.05-0.2C, charging time: 20-40min;
[0020] Stage 4: Charge to 25% SOC, charging rate range: 0.1-0.3C, charging time: 30-50min.
[0021] In one or more embodiments, steps (1)-(2) are repeated 3-12 times.
[0022] In one or more embodiments, in step (4), the lithium battery is charged to 30% SOC at a charging rate of 0.2-0.5C for 50-70 minutes.
[0023] In one or more embodiments, the lithium battery is formed by constant current charging.
[0024] In one or more embodiments, the positive electrode active material of the lithium ion battery includes lithium iron phosphate, and the negative electrode active material includes graphite.
[0025] In one or more embodiments, the lithium-ion battery includes one of a soft-pack battery, a square battery, and a cylindrical battery.
[0026] The second aspect of the present invention provides a method for preparing a lithium battery, which includes the steps of performing a formation step using a formation method for improving the high-temperature cycle capacity attenuation of a lithium battery as described in any embodiment of the present invention, and before the formation, stacking or winding the positive electrode sheet, the separator, and the negative electrode sheet, and then encapsulating them in a shell, and then drying and injecting liquid.
[0027] A third aspect of the present invention provides a lithium battery, which is prepared using the method for preparing a lithium battery as described in any embodiment of the present invention.
[0028] A fourth aspect of the present invention provides the use of a formation method for improving high temperature cycle capacity decay of a lithium battery as described in any embodiment herein in promoting the production of inorganic salt components in a lithium battery SEI film.
[0029] A fifth aspect of the present invention provides the use of a formation method for improving high temperature cycle capacity decay of a lithium battery as described in any embodiment herein in forming a dense and thick SEI film in a lithium battery to enhance the thermal stability of the film.
[0030] The sixth aspect of the present invention provides the application of the formation method for improving the high temperature cycle capacity decay of lithium batteries as described in any embodiment of the present invention to reduce the SEI film side reactions caused by thermodynamics at high temperatures and improve the high temperature performance of lithium battery cells.
[0031] A seventh aspect of the present invention provides the use of a formation method for improving high temperature cycle capacity decay of a lithium battery as described in any embodiment herein in improving high temperature cycle capacity decay of a lithium battery.
[0032] An eighth aspect of the present invention provides the use of a formation method for improving high temperature cycle capacity decay of a lithium battery as described in any embodiment herein in the preparation of a lithium battery with improved capacity retention under high temperature applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 TEM images of the batteries of Example 1 and Comparative Example 1.
[0034] Figure 2 1C / 1C 100% DOD cycle curves of the batteries of Examples 1-4 and Comparative Example 1. DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in this article. Unless otherwise specified, all technical and scientific terms used in this article are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definitions in this article shall prevail.
[0036] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0037] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0038] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0039] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0040] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.
[0041] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0042] The inventors of the present invention have discovered that by cycling a lithium battery multiple times between 0 and 25% SOC during formation and then charging it to 30% SOC, the production of inorganic salt components in the SEI film of the lithium battery can be beneficial, forming a dense and thick SEI film, thereby improving its thermal stability, thereby reducing the SEI film side reactions caused by thermodynamics at high temperatures, and significantly improving the high temperature performance of the battery cell.
[0043] In the present invention, SOC refers to the state of charge of a lithium battery, also known as the remaining capacity.
[0044] In the present invention, the SEI film is a solid electrolyte interface film.
[0045] The present invention provides a formation method for improving the high temperature cycle capacity decay of a lithium battery, which comprises the following steps:
[0046] (1) Charge the lithium battery from 0 SOC to 25% SOC, and then discharge it to 0 SOC;
[0047] (2) Repeat step (1) 2 or more times;
[0048] (3) Charge the lithium battery from 0 SOC to 30% SOC.
[0049] In step (1), the lithium battery is charged from 0 SOC to 25% SOC at a charging rate of 0.05C-0.3C.
[0050] In step (1), the lithium battery can be charged from 0 SOC to 25% SOC in stages, for example, in 3-5 stages. In some embodiments, the lithium battery is charged from 0 SOC to 9%-11% SOC and then to 25% SOC in 2-4 stages; preferably, the increase in SOC each time is 1.5%-5%. In some embodiments, the lithium battery is charged from 0 SOC to 1.5%-2% SOC, 4%-6% SOC, 9%-11% SOC, and finally to 25% SOC.
[0051] In some specific embodiments, in step (1), the specific steps of charging the lithium battery from 0 SOC to 25% SOC include:
[0052] The first stage: charge the lithium battery from 0SOC to 1.5%-2% SOC, the charging rate range is: 0.04-0.06C, and the charging time is: 10-30min;
[0053] The second stage: charging to 4%-6% SOC, charging rate range: 0.04-0.06C, charging time: 30-50min;
[0054] The third stage: charging to 9%-11% SOC, charging rate range: 0.05-0.2C, charging time: 20-40min;
[0055] Stage 4: Charge to 25% SOC, charging rate range: 0.1-0.3C, charging time: 30-50min.
[0056] It should be understood that in the process of multi-stage charging, there is also a step of letting the battery rest between each stage. The resting time is generally greater than 5 minutes, such as 8-15 minutes. Since the lithium battery has polarization phenomenon in mass transfer and charge transfer during the charging process, resulting in a high voltage, the polarization can be eliminated by resting.
[0057] In step (1), after the battery is charged to 25% SOC, the resting time is generally greater than 5 minutes, such as 8-15 minutes.
[0058] In step (2), discharge to 0 SOC at a discharge rate of 0.05C-0.2C.
[0059] In step (2), the lithium battery is discharged to a 0SOC cut-off voltage of 2V.
[0060] In step (2), after discharging, the standing time is generally greater than 5 minutes, such as 8-15 minutes.
[0061] In step (3), step (1) may be repeated 3-12 times, for example 3, 7, 10, or 12 times.
[0062] In step (4), the lithium battery is charged to 30% SOC at a charging rate of 0.2-0.5C.
[0063] After charging the lithium battery from 0 SOC to 30% SOC, a resting step may be included, and the resting time is generally greater than 4 minutes, such as 5-10 minutes.
[0064] In the present invention, the charge and discharge rate refers to the current value required for the battery to discharge its rated capacity within a specified time. It is numerically equal to the multiple of the rated capacity of the battery, usually represented by the letter C. For example, 1C charging means that the battery can be fully charged from 0% to 100% in 1 hour, and vice versa. 0.2C charging means that the battery can be fully charged from 0% to 100% in 5 hours, and vice versa.
[0065] Lithium-ion battery (lithium battery)
[0066] A lithium-ion battery comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the separator is arranged between the positive electrode and the negative electrode.
[0067] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer (also called a positive electrode material layer) disposed on the positive electrode current collector. The positive electrode current collector may be an aluminum foil, a titanium foil, a nickel foil, an iron foil, a zinc foil, etc. The positive electrode active material layer includes a positive electrode active material (also called a positive electrode material) and a lithium supplement. The positive electrode active material may include a compound that can reversibly embed and deintercalate lithium ions. The positive electrode active material may be selected from a composite oxide containing lithium and at least one selected from cobalt, manganese, nickel and iron, preferably a lithium-containing composite oxide. The lithium-containing composite oxide is preferably LiMxOy and LiMxPO 4 One or more of, wherein M is a combination of one or more transition metals, 0<x≤3, 0<y≤4. Examples of positive electrode active materials include lithium cobalt oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium iron phosphate (LiFePO 4 )wait.
[0068] The positive electrode active material layer may also include one or more selected from a conductive agent, a dispersant and a binder. The conductive agent is used to improve the conductivity of the electrode. Examples of the conductive agent of the positive electrode include one or more of conductive carbon black, carbon fiber (CF), acetylene black, Ketjen black, graphene and carbon nanotubes. The binder of the positive electrode improves the bonding performance between the positive electrode active material particles and between the positive electrode active material particles and the current collector. Examples of the binder of the positive electrode include at least one of fluorine-containing resin, polypropylene resin, fiber-type binder, rubber-type binder and polyimide-type binder. Examples of the dispersant of the positive electrode include one or more of polyetherimide, polyvinyl pyrrolidone and polyvinyl butyral resin. In some embodiments, the conductive agent in the positive electrode active material layer is conductive carbon black, the binder is polyvinylidene fluoride (PVDF), and the dispersant is polyetherimide.
[0069] The content ratio of each component in the positive electrode active material layer can be conventional. The mass fraction of the positive electrode active material in the positive electrode active material layer can be 90%-97%, for example, 91%, 93%, 93.5%, 94%, 94.7%, 95%, 95.2%, 96%, 96.8%, 97% or within the range composed of any two of the aforementioned values. The mass fraction of the conductive agent can be 0.5%-2%, for example, 1%, 1.1%, 1.5%, 1.8%, 2% or within the range composed of any two of the aforementioned values. The mass fraction of the binder can be 1.0%-2.5%, for example, 1%, 1.5%, 1.6%, 2% or within the range composed of any two of the aforementioned values. The mass fraction of the dispersant can be 0.08%-0.4%, for example, 0.08%, 0.1%, 0.2% or within the range composed of any two of the aforementioned values.
[0070] The positive electrode active material layer is obtained by coating a positive electrode slurry containing various components of the positive electrode active material layer and a solvent onto a positive electrode current collector, followed by drying and pressing. The solvent of the positive electrode slurry may be N-methylpyrrolidone (NMP).
[0071] The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer formed on the surface of the negative electrode current collector. The negative electrode current collector may be a copper foil. The negative electrode material layer includes a negative electrode active material, a conductive agent and a binder. The negative electrode material layer is obtained by coating a negative electrode slurry containing a negative electrode active material, a conductive agent, a binder and a solvent onto a positive electrode current collector, and then rolling and baking. The solvent of the negative electrode slurry may be water. The negative electrode active material may be one or more selected from carbon materials (such as graphite), silicon, silicon compounds, lithium titanate, tin and tin compounds. The negative electrode conductive agent may be one or more selected from conductive carbon black (SP), acetylene black, carbon nanotubes, carbon nanowires, carbon microspheres, carbon fibers and graphene. The negative electrode binder may be one or more selected from polyvinylidene fluoride, polytetrafluoroethylene, acrylonitrile multipolymer, polybutyl acrylate, polyacrylonitrile and styrene-butadiene rubber (SBR). The negative electrode material layer and the negative electrode slurry may also include a thickener, such as sodium carboxymethyl cellulose (CMC-Na). In some embodiments, the negative electrode active material in the negative electrode material layer is graphite, the conductive agent is conductive carbon black, the binder is styrene-butadiene rubber, and the thickener is sodium carboxymethyl cellulose.
[0072] The mass ratio of each component in the negative electrode material layer can be conventional. For example, the mass fraction of the negative electrode active material can be 90% to 98%, such as 93%, 95%, 95.7%, 96%, 97% or within the range composed of any two of the aforementioned values. The mass fraction of the conductive agent can be 0.5% to 5%, such as 1%, 1.5%, 2% or within the range composed of any two of the aforementioned values. The mass fraction of the binder can be 0.5% to 5%, such as 1%, 1.5%, 2%, 3% or within the range composed of any two of the aforementioned values. The mass fraction of the thickener can be 0 to 5%, such as 1%, 1.5%, 1.8%, 2%, 3% or within the range composed of any two of the aforementioned values.
[0073] The negative electrode active material layer is obtained by coating a negative electrode slurry containing various components of the negative electrode active material layer and a solvent onto a negative electrode current collector, followed by drying and pressing. The solvent of the negative electrode slurry may be water.
[0074] The material of the separator can be one or more of polyethylene and polypropylene. In some preferred embodiments, the separator material is selected from PP (polypropylene), rubber-coated PP, PE (polyethylene) and rubber-coated PE.
[0075] The electrolyte solution includes a nonaqueous organic solvent and an electrolyte salt.
[0076] The non-aqueous organic solvent suitable for the electrolyte of the present invention can be selected from one or more of carbonate solvents, ether-based solvents, ketone-based solvents and other aprotic solvents. Examples of non-aqueous organic solvents include, but are not limited to, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate and ethyl propionate, etc. In some preferred embodiments, the non-aqueous organic solvent includes ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC). Preferably, the mass ratio of propylene carbonate:ethyl methyl carbonate:diethyl carbonate is preferably (0.5-2):(0.5-2):(0.5-2), for example, 1:1:1.
[0077] The electrolyte salt may include or be selected from a lithium salt. A lithium salt is a material that is easily soluble in a non-aqueous organic solvent. The lithium salt may be selected from one or more of an organic lithium salt and an inorganic lithium salt. Examples of lithium salts include, but are not limited to, LiCl, LiBr, LiI, LiClO 4 , LiBF 4 、LiPF 6 、LiCF 3 SO 3 、LiCF 3 CO 2 、LiAsF 6 、LiSbF 6 、LiAlCl 4 , CH 3 SO 3 Li, (CF 3 SO 2 ) 2 In some embodiments, the concentration of the electrolyte salt in the electrolyte is 0.5-2 mol / L, such as 0.8 mol / L, 1 mol / L, 1.5 mol / L, or within the range formed by any two of the foregoing values.
[0078] The electrolyte of the present invention may optionally contain various additives that can be used in the electrolyte, such as desolvating agents, cosolvents, film-forming additives, etc. The mass fraction of each type of additive in the electrolyte may be 0.1%-10%, such as 1%, 2%, 3%, 4%, 5%, or within the range formed by any two of the aforementioned values.
[0079] The electrolyte suitable for the present invention may be a commonly used commercially available electrolyte.
[0080] The positive electrode sheet, the negative electrode sheet and the separator are stacked or wound according to the design requirements, and then packaged in a shell, dried, injected (electrolyte is injected), sealed, and then formed by the formation method of the present invention, and finally aged and divided to obtain an electrochemical device, such as a lithium ion battery. The form of the lithium ion battery of the present invention is not particularly limited, and can be a cylindrical lithium ion battery, a soft-pack lithium ion battery or an aluminum shell lithium ion battery.
[0081] Beneficial effects achieved by the present invention:
[0082] The formation method of the present invention can improve the compactness and thermal stability of the SEI film in the battery, improve the high-temperature cycle performance of the battery core, and especially effectively reduce the problem of initial capacity attenuation under high-temperature application. The formation method of the present invention is applied to the preparation of lithium-ion batteries without changing the existing production process or adding new processes, and only the formation process is optimized.
[0083] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.
[0084] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
[0085] Example 1
[0086] (1) Preparation of positive electrode sheet: Lithium iron phosphate, conductive agent SP, and binder PVDF in a mass ratio of 96.2:1.8:2 are prepared by stirring, coating, cold pressing, slitting, and other processes to form a positive electrode sheet required for winding;
[0087] Preparation of negative electrode sheet: artificial graphite, conductive agent SP, binder CMC, and binder SBR in a mass ratio of 95.6:1.2:1.8:1.4 are mixed, coated, cold pressed, and slit to form the negative electrode sheet required for winding;
[0088] The positive and negative electrode sheets and separators (9umPE+3ccs+2pcs, where CCS is alumina ceramic and PCS is PVDF glue) are wound into a core, which is then covered with an insulating coating film and placed in a square aluminum shell. After baking and liquid injection, a battery cell is obtained.
[0089] (2) Formation:
[0090] The cells are formed at 45±2℃, specifically:
[0091] ①0.05C CC 20min, let stand for 10min,
[0092] ②0.05C CC 40min, let stand for 10min,
[0093] ③0.1C CC 30min, let stand for 10min,
[0094] ④0.2C CC 45min, let stand for 10min;
[0095] ⑤0.1C DC 2.0V, let stand for 10min,
[0096] ⑥Repeat ①~⑤ process 3 times,
[0097] ⑦0.3C CC 60min, let stand for 5min.
[0098] (3) After formation, the cells are divided into different capacities to obtain lithium-ion batteries.
[0099] Example 2
[0100] The difference between Example 2 and Example 1 is that the steps of formation are different, specifically:
[0101] ①0.05C CC 20min, let stand for 10min,
[0102] ②0.05C CC 40min, let stand for 10min,
[0103] ③0.1C CC 30min, let stand for 10min,
[0104] ④0.2C CC 45min, let stand for 10min
[0105] ⑤0.1C DC 2.0V, let stand for 10min,
[0106] ⑥Repeat ①~⑤ process 7 times,
[0107] ⑦0.3C CC 60min, let stand for 5min.
[0108] Example 3
[0109] The difference between Example 3 and Example 1 is that the steps of formation are different, specifically: ① 0.05C CC for 20 min, let stand for 10 min,
[0110] ②0.05C CC 40min, let stand for 10min,
[0111] ③0.1C CC 30min, let stand for 10min,
[0112] ④0.2C CC 45min, let stand for 10min,
[0113] ⑤0.1C DC 2.0V, let stand for 10min,
[0114] ⑥Repeat ①~⑤ process 10 times,
[0115] ⑦0.3C CC 60min, let stand for 5min.
[0116] Example 4
[0117] The difference between Example 4 and Example 1 is that the steps of chemical formation are different, specifically: ① 0.05C CC for 20 min, let stand for 10 min,
[0118] ②0.05C CC 40min, let stand for 10min,
[0119] ③0.1C CC 30min, let stand for 10min,
[0120] ④0.2C CC 45min, let stand for 10min,
[0121] ⑤0.1C DC 2.0V, let stand for 10min,
[0122] ⑥Repeat ①~⑤ process 12 times,
[0123] ⑦0.3C CC 60min, let stand for 5min.
[0124] Comparative Example 1
[0125] The difference between Comparative Example 1 and Example 1 is that the steps of formation are different, specifically: ① 0.05C CC for 20 min, let stand for 10 min,
[0126] ②0.05C CC 40min, let stand for 10min,
[0127] ③0.1C CC 30min, let stand for 10min,
[0128] ④0.2C CC 45min, let stand for 10min,
[0129] ⑤0.3C CC 10min, let stand for 5min.
[0130] Test Case
[0131] (1) The lithium batteries of Example 1 and Comparative Example 1 were tested using a transmission electron microscope (TEM) to determine the thickness of the SEI film formed under different formation processes. The results of the test are shown in FIG. Figure 1 shown.
[0132] Depend on Figure 1 It can be seen that a is the conventional formation process used in comparative example 1, and the formation process at 45°C and 30% SOC shows that the thickness of the formed SEI film is about 3.37nm. b is the optimized process used in Example 1, and at 45°C, through multiple charge and discharge between 0% and 25% SOC, and then charging to 30% SOC, it can be seen that the thickness of the formed SEI film is about 9.70nm.
[0133] (2) Figure 2 The following is a graph showing the 100% DOD cycle curves of the lithium batteries of Examples 1-4 and Comparative Example 1 at 45°C 1C / 1C. Figure 2 It can be seen that the capacity retention rate of the battery cells of Examples 1-4 under the same number of cycles is significantly improved by adopting the formation method of the present invention. This is mainly because multiple cycles of charge and discharge are beneficial to the production of inorganic salt components in SEI, forming a dense and thick SEI with a more stable structure. Under high temperature conditions, according to the Nernst equation, the activation energy will double for every 10°C increase in temperature. Therefore, thermodynamic influence is the main factor, and material kinetics has little effect on it.
Claims
1. A formation method for improving the high temperature cycle capacity decay of a lithium battery, characterized in that: The formation method comprises the following steps: (1) Charge the lithium battery from 0 SOC to 25% SOC and leave it alone; (2) Discharge the lithium battery from 25% SOC to 0 SOC and leave it alone; (3) Repeat steps (1) to (2) 2 or more times; (4) Charge the lithium battery from 0 SOC to 30% SOC.
2. The formation method for improving the high temperature cycle capacity decay of a lithium battery according to claim 1, characterized in that: The temperature was controlled at 45±2°C during the formation process.
3. The formation method for improving the high temperature cycle capacity decay of a lithium battery according to claim 1, characterized in that: The method has one or more of the following features: In step (1), the lithium battery is charged from 0 SOC to 25% SOC at a charging rate of 0.05C-0.3C; In step (1), the lithium battery is charged in stages from 0 SOC to 1.5%-2% SOC, 4%-6% SOC, 9%-11% SOC, and finally to 25% SOC; In step (2), the battery is discharged at a discharge rate of 0.05C-0.2C to 0 SOC; In step (2), the lithium battery is discharged to a 0SOC cut-off voltage of 2V.
4. The formation method for improving the high temperature cycle capacity decay of a lithium battery according to claim 3, characterized in that: In step (1), the lithium battery is charged from 0 SOC to 25% SOC in stages, and the specific steps include: The first stage: charge the lithium battery from 0SOC to 1.5-2%SOC, the charging rate range is: 0.04-0.06C, and the charging time is: 10-30min; The second stage: charging to 4-6% SOC, charging rate range: 0.04-0.06C, charging time: 30-50min; The third stage: charging to 9-11% SOC, charging rate range: 0.05-0.2C, charging time: 20-40min; Stage 4: Charge to 25% SOC, charging rate range: 0.1-0.3C, charging time: 30-50min.
5. The formation method for improving high temperature cycle capacity decay of a lithium battery according to claim 1, characterized in that: Repeat steps (1)-(2) 3-12 times; and / or In step (4), the lithium battery is charged to 30% SOC at a charging rate of 0.2-0.5C for 50-70 minutes.
6. The formation method for improving high temperature cycle capacity decay of a lithium battery according to claim 1, characterized in that: The lithium battery is formed by constant current charging.
7. The formation method for improving high temperature cycle capacity decay of a lithium battery according to claim 1, characterized in that: The positive electrode active material of the lithium ion battery includes lithium iron phosphate, and the negative electrode active material includes graphite; and / or The lithium-ion battery includes one of a soft-pack battery, a square battery, and a cylindrical battery.
8. A method for preparing a lithium battery, characterized in that: The method comprises the steps of performing formation by using the formation method for improving the high temperature cycle capacity attenuation of a lithium battery as described in any one of claims 1 to 7, and before the formation, laminating or winding the positive electrode sheet, the separator and the negative electrode sheet, and then encapsulating them in a shell, and then drying and injecting liquid.
9. A lithium battery, characterized in that: It is prepared by the lithium battery preparation method as claimed in claim 8.
10. Application of the formation method for improving high temperature cycle capacity decay of lithium batteries according to any one of claims 1 to 7 in one or more of the following aspects: (1) Promote the production of inorganic salt components in the SEI film of lithium batteries; (2) Forming a dense and thick SEI film in lithium batteries and improving the thermal stability of the film; (3) Reduce the SEI film side reactions caused by thermodynamics at high temperatures and improve the high temperature performance of lithium battery cells; (4) Improve the capacity decay of lithium batteries during high temperature cycles; and (5) Prepare lithium batteries with improved capacity retention under high temperature applications.