Composition of diaphragm for battery, diaphragm as well as preparation method and application of diaphragm
By using polyethylene, polypropylene and polypropylene-polyethylene block copolymers, wet process parameters are optimized, and the problem of insufficient thermal stability and mechanical properties of wet separators at high temperatures is solved, and the lithium-ion battery separators are improved Puncture strength and heat shrinkage, suitable for high-capacity and high-power batteries.
Patent Information
- Application Number
- CN202411242556.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-06
AI Technical Summary
The thermal stability and mechanical properties of existing wet lithium battery separators at high temperatures are insufficient, which limits the safety and application range of the battery.
Polyethylene, polypropylene and polypropylene-polyethylene block copolymers are used as separator materials. By adjusting the material proportion and process parameters, the puncture strength, heat shrinkage and thermal stability of the separator are improved to prepare an excellent mechanical properties. Diaphragm.
It has achieved significant improvement in puncture strength and tensile strength on low-thick diaphragm, optimized film uniformity and pore size uniformity, enhanced thermal stability and safety performance of the diaphragm, and is suitable for high-capacity and high-power lithium-ion batteries.
Smart Images

Figure BDA0005030494820000181
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of separators / diaphragms, and more specifically, relates to a battery separator composition, a separator, and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are the representative of modern high-performance batteries, and are composed of four main parts: positive electrode materials, negative electrode materials, diaphragms, and electrolytes. Among them, the diaphragm is a thin film with a microporous structure. It is the key inner component with the most technical barriers in the lithium-ion battery industry chain. It plays the following two main roles in lithium batteries: 1) Separating the positive and negative electrodes of the lithium battery to prevent the positive and negative electrodes from contacting and forming a short circuit; 2) The micropores in the film allow lithium ions to pass through to form a charge and discharge circuit. High-performance lithium batteries require the diaphragm to have uniform thickness and excellent mechanical properties (including tensile strength and puncture resistance), physical and chemical properties (including wettability, chemical stability, thermal stability, and safety). The excellence of the diaphragm directly affects the capacity, cycle capacity, and safety performance of the lithium battery. A diaphragm with excellent performance plays an important role in improving the overall performance of the battery.
[0003] Specifically, the thickness of the diaphragm is one of the basic parameters. The thinning of the diaphragm can increase the energy density of lithium-ion batteries, reduce resistance, and thus improve endurance, which is an important trend in the development of the industry. Mechanical properties mainly include puncture strength and tensile strength. During the production process, the diaphragm material needs to go through the steps of curling, winding, packaging, battery assembly, etc. The rough surface of the positive and negative electrodes may puncture the diaphragm during the assembly process. It will also be subjected to physical impact, wear, compression, and tensile external forces during use. Excellent mechanical properties can effectively prevent battery short circuits. Thermal properties generally include thermal closure temperature, film rupture temperature, and thermal shrinkage rate. At present, lithium battery diaphragms can provide the additional function of thermal shutdown, providing additional safety protection for lithium batteries. The main parameters of this additional function are the closed pore temperature and the rupture temperature. Because the lithium battery diaphragm itself has a microporous structure, the closed pore temperature is the temperature when the micropores are closed, and the rupture temperature is the temperature when the diaphragm is ruptured and melted. The closed-pore temperature is the protective mechanism of the separator for the battery. When the battery generates a lot of heat and the temperature is close to the melting point of the material polymer, the micropores close to form a thermal shutdown, which can block the continued transmission of ions and form a short circuit, thus protecting the battery. Therefore, lithium battery manufacturers hope that the separator can have a lower closed-pore temperature and a higher membrane rupture temperature, which can improve the battery safety performance to a greater extent.
[0004] Polyolefin microporous membranes have become the most commercially used type of diaphragms due to their low price and simple sources. Their manufacturing materials mainly include polypropylene (PP) and polyethylene (PE) materials. The many characteristics of lithium battery diaphragms and the difficulty in taking into account their performance indicators determine that their production process has high technical barriers and is difficult to develop. The diaphragm production process includes many processes such as raw material formula adjustment, microporous preparation technology, and independent design of complete sets of equipment. Among them, microporous preparation technology is the core of the lithium battery diaphragm preparation process. According to the difference in micropore formation mechanism, the diaphragm process can be divided into dry and wet processes. Among them, the dry process is the most commonly used method. The main raw material for production is PP. The biggest difference from the wet process is that no solvent is used. The wet process is also called thermally induced phase separation method. The raw material is usually PE resin. Compared with the dry process, the wet process is complex, has high equipment requirements, and usually requires the use of solvents. However, the advantages of the wet process are more prominent. The film produced is thinner, which is conducive to improving the energy density of the battery; the porosity and pore size are easier to control, and the mechanical properties and uniformity are better, which can meet the high current requirements of power lithium-ion batteries; the main raw material PE of the wet process is more lyophilic than the raw material PP of the dry process, which can effectively improve the conductivity. Therefore, the wet process diaphragm currently occupies a dominant position in the market with the above advantages.
[0005] However, since the PE diaphragm is a thermoplastic polymer material, its glass transition temperature is about -68°C and its melting point is about 135°C, resulting in poor thermal stability at high temperatures. Therefore, as the working environment temperature increases, the PE diaphragm will experience a large thermal shrinkage phenomenon, which will cause the battery to have a short circuit risk. The closed-cell temperature is about 130°C and the melting destruction temperature is about 140°C, which means that the working environment of the PE diaphragm is severely restricted. Therefore, although the wet-process diaphragm currently occupies a dominant position in the market due to its many advantages, the lithium-ion battery diaphragm prepared by the wet process using PE as raw material still has room for improvement in its mechanical properties and thermal properties, and its lack of mechanical properties and thermal properties also restricts the application of wet-process diaphragms in high-power, high-capacity energy storage devices. Therefore, the modification of wet-process diaphragms has become a research hotspot in the field of lithium-ion battery diaphragms.
[0006] At present, for the modification of wet-process diaphragms, in order to solve the technical problem of how to improve the thermal properties of the diaphragm (such as high temperature resistance and / or thermal shrinkage and / or thermal stability), the technical means of composite modified layers are mostly used. For example, highly heat-resistant organic adhesives-inorganic particle coatings, or ceramic coatings, or resins with high melting points (fluororesins, polyester resins, etc.) are used for modification. Under the premise of maintaining the thermal shutdown performance of the polyolefin itself, the overall high temperature resistance of the diaphragm can be improved, the high-temperature rupture temperature is high, and short circuits are not easy to occur. In solving how to improve the mechanical properties of the diaphragm, the technical means of adjusting the specific components of the layer is also mainly used. For multi-layer polyolefin diaphragms, polypropylene is usually used for the outer layer, and polyethylene is used for the middle layer, or a high proportion of polypropylene and a low proportion of polyethylene are used for the outer layer, which can significantly improve the puncture strength of the diaphragm. Providing a high-strength film, non-woven fabric or coating on the base film can also improve the puncture strength of the diaphragm.
[0007] However, overall, the above modification methods have the risk of increasing the thickness of the separator or blocking the micropores of the separator, thereby reducing the energy and power density of the battery. Perhaps, there are also defects such as uneven particle distribution and poor surface binding ability. Summary of the invention
[0008] 1. Problem to be solved
[0009] In view of the problem that the mechanical properties of existing wet-process diaphragms need to be improved, the present invention provides a composition of a battery diaphragm and a battery diaphragm;
[0010] Furthermore, the present invention also provides a method for preparing a battery separator;
[0011] Meanwhile, the present invention also provides a battery containing the separator.
[0012] 2. Technical solution
[0013] The technical solution adopted by the present invention is as follows:
[0014] Based on the purpose of the present invention, the first aspect of the present invention provides a composition for a battery separator, the composition comprising:
[0015] Polyethylene;
[0016] Polypropylene;
[0017] Block copolymers of polypropylene and polyethylene;
[0018] Wherein, calculated by mass ratio, the ratio of polyethylene, polypropylene and block copolymer is (3-15): (5-15): (3-15). On this basis, the ratio of polyethylene, polypropylene and block copolymer can be further preferably (3-15): (5-15): (5-15), or (5-12): (5-12): (5-15), or (5-10): (5-10): (5-15).
[0019] According to the composition of the battery separator of any embodiment of the first aspect of the present invention, in the block copolymer of polypropylene and polyethylene, the mass ratio of polyethylene to polypropylene is 1:(1-3). On this basis, in the block copolymer of polypropylene and polyethylene, the mass ratio of polyethylene to polypropylene can further preferably be 1:(1-2.4), or 1:(1-1.5).
[0020] According to the composition of the battery separator of any embodiment of the first aspect of the present invention, the block copolymer of polypropylene and polyethylene is polymerized by polyethylene and polypropylene in a mass ratio of 1: (1 to 3). On this basis, the block copolymer of polypropylene and polyethylene can further preferably be polymerized by polyethylene and polypropylene in a mass ratio of 1: (1 to 2.4) or 1: (1 to 1.5).
[0021] As described herein, the "mass ratio of polypropylene to polyethylene in the block copolymer" will affect the puncture strength of the diaphragm. A higher amount of polypropylene than polyethylene is beneficial to improving the puncture strength of the diaphragm.
[0022] According to the composition for a battery separator of any embodiment of the first aspect of the present invention, the block copolymer of polypropylene and polyethylene is an AB-type diblock copolymer;
[0023] Wherein, the molecular weight of the block copolymer is 500,000 to 2,000,000;
[0024] The length of the polypropylene segment in the block copolymer is 150,000 to 250,000 units, and the length of the polyethylene segment in the block copolymer is 100,000 to 200,000 units.
[0025] According to the composition for a battery separator of any embodiment of the first aspect of the present invention, the block copolymer of polypropylene and polyethylene is an AB-type diblock copolymer;
[0026] The molecular weight of the block copolymer is 1 million to 1.8 million, the length of the polypropylene segment in the block copolymer is 190,000 to 250,000 units, and the length of the polyethylene segment in the block copolymer is 150,000 to 200,000 units.
[0027] According to the composition for a battery separator of any embodiment of the first aspect of the present invention, the block copolymer of polypropylene and polyethylene is an AB-type diblock copolymer;
[0028] The molecular weight of the block copolymer is 1.5 million to 1.8 million, the length of the polypropylene segment in the block copolymer is 230,000 to 250,000 units, and the length of the polyethylene segment in the block copolymer is 150,000 to 180,000 units.
[0029] As described herein, "the length of the polypropylene segment and the length of the polyethylene segment" will affect the puncture strength of the diaphragm. Specifically, the chain length of the polyethylene segment and the chain length of the polypropylene segment in the block copolymer will affect the compatibility of polypropylene and polyethylene, and the tight adhesion of the ternary structure (polyethylene, polypropylene, block copolymer) in the diaphragm, thereby affecting the puncture strength of the diaphragm.
[0030] According to the battery separator composition of any embodiment of the first aspect of the present invention, the polypropylene segment in the block copolymer is a syndiotactic polypropylene segment.
[0031] According to the battery separator composition of any embodiment of the first aspect of the present invention, the polypropylene is a syndiotactic polypropylene.
[0032] As described herein, selecting "syndiotactic polypropylene" can increase the flexibility and toughness of the diaphragm, and further improve the puncture strength of the diaphragm.
[0033] In the battery separator composition according to any embodiment of the first aspect of the present invention, the molecular weight of the polypropylene is in the range of 80,000 to 700,000.
[0034] According to the battery separator composition of any embodiment of the first aspect of the present invention, the polyethylene is a high-density polyethylene, and the molecular weight of the high-density polyethylene is in the range of 500,000 to 700,000, and more preferably in the range of 500,000 to 600,000.
[0035] In the battery separator composition according to any embodiment of the first aspect of the present invention, the high-density polyethylene has a melting point of 130 to 142°C.
[0036] Based on the purpose of the present invention, the second aspect of the present invention provides a battery separator, the separator comprising:
[0037] Polyethylene;
[0038] Polypropylene;
[0039] Block copolymer of polypropylene and polyethylene.
[0040] According to any embodiment of the second aspect of the present invention, the battery separator is calculated by mass ratio, and the ratio of the polyethylene, polypropylene, and block copolymer is (3-15): (5-15): (3-15). On this basis, the ratio of the polyethylene, polypropylene, and block copolymer can be further preferably (3-15): (5-15): (5-15), or (5-12): (5-12): (5-15), or (5-10): (5-10): (5-15).
[0041] According to any embodiment of the second aspect of the present invention, in the block copolymer of polypropylene and polyethylene, the mass ratio of polyethylene to polypropylene is 1: (1 to 3). On this basis, in the block copolymer of polypropylene and polyethylene, the mass ratio of polyethylene to polypropylene can further preferably be 1: (1 to 2.4), or 1: (1 to 1.5).
[0042] According to any embodiment of the second aspect of the present invention, the block copolymer of polypropylene and polyethylene is formed by polymerizing polyethylene and polypropylene in a mass ratio of 1: (1 to 3). On this basis, the block copolymer of polypropylene and polyethylene can further preferably be formed by polymerizing polyethylene and polypropylene in a mass ratio of 1: (1 to 2.4) or 1: (1 to 1.5).
[0043] As described herein, the "mass ratio of polypropylene to polyethylene in the block copolymer" will affect the puncture strength of the diaphragm. A higher amount of polypropylene than polyethylene is beneficial to improving the puncture strength of the diaphragm.
[0044] According to any embodiment of the second aspect of the present invention, the battery separator, the block copolymer of polypropylene and polyethylene is an AB type diblock copolymer;
[0045] Wherein, the molecular weight of the block copolymer is 500,000 to 2,000,000;
[0046] The length of the polypropylene chain segment is 150,000 to 250,000 units, and the length of the polyethylene chain segment is 100,000 to 200,000 units.
[0047] According to any embodiment of the second aspect of the present invention, the battery separator, the block copolymer of polypropylene and polyethylene is an AB type diblock copolymer;
[0048] The molecular weight of the block copolymer is 1 million to 1.8 million, the length of the polypropylene segment is 190,000 to 250,000 units, and the length of the polyethylene segment is 150,000 to 200,000 units.
[0049] According to any embodiment of the second aspect of the present invention, the battery separator, the block copolymer of polypropylene and polyethylene is an AB type diblock copolymer;
[0050] The molecular weight of the block copolymer is 1.5 million to 1.8 million, the length of the polypropylene segment is 230,000 to 250,000 units, and the length of the polyethylene segment is 150,000 to 180,000 units.
[0051] As described herein, "the length of the polypropylene segment and the length of the polyethylene segment" will affect the puncture strength of the diaphragm. Specifically, the chain length of the polyethylene segment and the chain length of the polypropylene segment in the block copolymer will affect the compatibility of polypropylene and polyethylene, and the tight adhesion of the ternary structure (polyethylene, polypropylene, block copolymer) in the diaphragm, thereby affecting the puncture strength of the diaphragm.
[0052] According to any embodiment of the battery separator of the second aspect of the present invention, the polypropylene segment in the block copolymer is a syndiotactic polypropylene segment.
[0053] According to any embodiment of the battery separator of the second aspect of the present invention, the polypropylene is a syndiotactic polypropylene.
[0054] As described herein, selecting "syndiotactic polypropylene" can increase the flexibility and toughness of the diaphragm, and further improve the puncture strength of the diaphragm.
[0055] In the battery separator composition according to any embodiment of the second aspect of the present invention, the molecular weight of the polypropylene is in the range of 80,000 to 700,000.
[0056] According to any embodiment of the battery separator of the second aspect of the present invention, the polyethylene is high-density polyethylene, and the molecular weight of the high-density polyethylene is in the range of 500,000 to 700,000, and more preferably in the range of 500,000 to 600,000.
[0057] According to any embodiment of the battery separator of the second aspect of the present invention, the melting point of the high-density polyethylene is 130-142°C.
[0058] According to any embodiment of the second aspect of the present invention, the battery separator has the following characteristics when the thickness of the separator is 3 to 10 μm:
[0059] A membrane rupture temperature of 145 to 170°C; and / or
[0060] A membrane melting point of 135 to 155°C; and / or
[0061] Puncture strength of 300-500 gf; and / or,
[0062] A heat shrinkage in MD of no more than 2% at a temperature not exceeding 150°C; and / or,
[0063] A TD heat shrinkage of no more than 1.5% at a temperature not exceeding 150°C; and / or,
[0064] 2500~4000Kgf / cm 2 MD tensile strength; and / or,
[0065] 1500~3200Kgf / cm 2 TD tensile strength.
[0066] According to any embodiment of the second aspect of the present invention, the battery separator has the following characteristics when the thickness of the separator is 3 to 10 μm:
[0067] A membrane rupture temperature of 156 to 170°C; and / or
[0068] A membrane melting point of 143 to 155°C; and / or,
[0069] Puncture strength of 389-463 gf; and / or,
[0070] A heat shrinkage in MD of no more than 2% at a temperature not exceeding 150°C; and / or,
[0071] A TD heat shrinkage of no more than 1.5% at a temperature not exceeding 150°C; and / or
[0072] 3124~4000Kgf / cm 2 MD tensile strength; and / or,
[0073] 2156~3200Kgf / cm 2 TD tensile strength.
[0074] According to any embodiment of the second aspect of the present invention, the battery separator has the following characteristics when the membrane thickness is 8 to 10 μm:
[0075] Membrane rupture temperature of 160-170°C; and / or,
[0076] A membrane melting point of 140 to 155°C; and / or
[0077] Puncture strength of 410-500 gf; and / or,
[0078] A heat shrinkage in MD of no more than 2% at a temperature not exceeding 150°C; and / or,
[0079] A TD heat shrinkage of no more than 1.5% at a temperature not exceeding 150°C; and / or,
[0080] 3200~4000Kgf / cm 2 MD tensile strength; and / or,
[0081] 2100~3200Kgf / cm 2 TD tensile strength.
[0082] According to any embodiment of the second aspect of the present invention, the battery separator has the following characteristics when the thickness of the separator is 3 to 6 μm:
[0083] Or when the film thickness is 3 to 6 μm, the diaphragm has:
[0084] A membrane rupture temperature of 145 to 165°C; and / or
[0085] A membrane melting point of 135 to 150°C; and / or,
[0086] Puncture strength of 300-450 gf; and / or,
[0087] A heat shrinkage in MD of no more than 2% at a temperature not exceeding 150°C; and / or,
[0088] A TD heat shrinkage of no more than 1.5% at a temperature not exceeding 150°C; and / or,
[0089] 2500~3500Kgf / cm 2 MD tensile strength; and / or,
[0090] 1500~3500Kgf / cm 2 TD tensile strength.
[0091] As described herein, the "membrane rupture temperature" is tested with reference to the standard / method for heating a single-layer membrane sample and detecting the membrane resistance as the temperature changes. Machine model: ART-GMT-35;
[0092] "Diaphragm melting point" refers to the relationship between the power difference (such as heat) input to the sample and the reference material and the temperature when the diaphragm (1mg-5mg) is placed in a crucible and the diaphragm is heated in a gradient manner. The test is carried out according to the standard / method. Machine model: DSC3 professional type;
[0093] "Puncture strength" is tested with reference to GB / T 36363-2018 standard / method;
[0094] "Manditudinal heat shrinkage (MD heat shrinkage)" and "Transverse heat shrinkage (TD heat shrinkage)" are tested with reference to the GB / T 36363-2018 standard / method;
[0095] The "longitudinal tensile strength (MD tensile strength)" and "transverse tensile strength (TD tensile strength)" are tested with reference to the GB / T1040.3-2006 standard / method.
[0096] In the present application, the performance of the battery separator is mutually restricted by the combined effects of the mass ratio, molecular weight and preparation method of polyethylene, polypropylene, polypropylene and polyethylene block copolymer, pore former and extractant.
[0097] Based on the purpose of the present invention, the third aspect of the present invention provides a battery separator, wherein the raw materials for preparing the separator include: polyethylene, polypropylene, and a block copolymer of polypropylene and polyethylene;
[0098] Calculated by mass, the usage ratio of the polyethylene, polypropylene and the block copolymer of polypropylene and polyethylene is (3-15): (5-15): (3-15). On this basis, the usage ratio of the polyethylene, polypropylene and block copolymer can be further preferably (3-15): (5-15): (5-15), or (5-12): (5-12): (5-15), or (5-10): (5-10): (5-15).
[0099] According to any embodiment of the third aspect of the present invention, the raw materials for preparing the diaphragm further include: a pore former and an extractant, and the amount ratio of the polyethylene, polypropylene, polypropylene and polyethylene block copolymer, the pore former and the extractant is (3-15): (5-15): (3-15): (70-85): (60-80). On this basis, the amount ratio of the polyethylene, polypropylene, polypropylene and polyethylene block copolymer, the pore former and the extractant can further preferably be (5-13): (5-14): (5-14): (70-80): (65-80), or (5-10): (5-10): (5-15): (75-80): (70-80).
[0100] According to any embodiment of the third aspect of the present invention, in the block copolymer of polypropylene and polyethylene, the mass ratio of polyethylene to polypropylene is 1: (1 to 3). On this basis, in the block copolymer of polypropylene and polyethylene, the mass ratio of polyethylene to polypropylene can further preferably be 1: (1 to 2.4), or 1: (1 to 1.5).
[0101] According to any embodiment of the third aspect of the present invention, the block copolymer of polypropylene and polyethylene is formed by polymerizing polyethylene and polypropylene in a mass ratio of 1: (1 to 3). On this basis, the block copolymer of polypropylene and polyethylene can further preferably be formed by polymerizing polyethylene and polypropylene in a mass ratio of 1: (1 to 2.4) or 1: (1 to 1.5).
[0102] According to any embodiment of the battery separator of the third aspect of the present invention, the polypropylene is a syndiotactic polypropylene.
[0103] As described herein, selecting "syndiotactic polypropylene" can increase the flexibility and toughness of the diaphragm, and further improve the puncture strength of the diaphragm.
[0104] In the battery separator composition according to any embodiment of the third aspect of the present invention, the molecular weight of the polypropylene is in the range of 80,000 to 700,000.
[0105] According to any embodiment of the battery separator of the third aspect of the present invention, the polyethylene is high-density polyethylene, and the molecular weight of the high-density polyethylene is in the range of 500,000 to 700,000, and more preferably in the range of 500,000 to 600,000.
[0106] According to any embodiment of the third aspect of the present invention, the battery separator, the pore-forming agent refers to a high-boiling-point hydrocarbon liquid or some substances with relatively low molecular weight, including any one, two or more of paraffin oil, kerosene and white oil;
[0107] The extractant includes any one, two or more of dichloromethane, chloroform, carbon tetrachloride, gasoline and hydrocarbon cleaning agent.
[0108] According to any embodiment of the battery separator of the third aspect of the present invention, the melting point of the high-density polyethylene is 130-142°C.
[0109] According to any embodiment of the third aspect of the present invention, the battery separator, the block copolymer of polypropylene and polyethylene is an AB type diblock copolymer;
[0110] Wherein, the molecular weight of the block copolymer is 500,000 to 2,000,000;
[0111] The length of the polypropylene segment in the block copolymer is 150,000 to 250,000 units, and the length of the polyethylene segment in the block copolymer is 100,000 to 200,000 units.
[0112] According to any embodiment of the third aspect of the present invention, the battery separator, the block copolymer of polypropylene and polyethylene is an AB type diblock copolymer;
[0113] The molecular weight of the block copolymer is 1 million to 1.8 million, the length of the polypropylene segment in the block copolymer is 190,000 to 250,000 units, and the length of the polyethylene segment in the block copolymer is 150,000 to 200,000 units.
[0114] According to any embodiment of the third aspect of the present invention, the battery separator, the block copolymer of polypropylene and polyethylene is an AB type diblock copolymer;
[0115] The molecular weight of the block copolymer is 1.5 million to 1.8 million, the length of the polypropylene segment in the block copolymer is 230,000 to 250,000 units, and the length of the polyethylene segment in the block copolymer is 150,000 to 180,000 units.
[0116] As described herein, "the length of the polypropylene segment and the length of the polyethylene segment" will affect the puncture strength of the diaphragm. Specifically, the chain length of the polyethylene segment and the chain length of the polypropylene segment in the block copolymer will affect the compatibility of polypropylene and polyethylene, and the tight adhesion of the ternary structure (polyethylene, polypropylene, block copolymer) in the diaphragm, thereby affecting the puncture strength of the diaphragm.
[0117] According to any embodiment of the battery separator of the third aspect of the present invention, the polypropylene segment in the block copolymer is a syndiotactic polypropylene segment.
[0118] Based on the purpose of the present invention, the fourth aspect of the present invention provides a method for preparing a battery diaphragm, wherein the diaphragm is prepared by a wet process.
[0119] According to the method for preparing a battery separator according to any embodiment of the fourth aspect of the present invention, the raw materials for preparing the separator include: polyethylene, polypropylene, a block copolymer of polypropylene and polyethylene, and a pore former;
[0120] Calculated by mass, the usage ratio of the polyethylene, polypropylene, polypropylene and polyethylene block copolymer, and pore-forming agent is (3-15): (5-15): (3-15): (70-85). On this basis, the usage ratio of the polyethylene, polypropylene, polypropylene and polyethylene block copolymer, and pore-forming agent can be further preferably (3-15): (5-15): (5-15): (70-85), or (5-12): (5-12): (5-15): (70-85), or (5-10): (5-10): (5-15): (70-85).
[0121] According to the method for preparing a battery separator according to any embodiment of the fourth aspect of the present invention, the raw materials for preparing the separator further include an extractant, and the amount ratio of the polyethylene, polypropylene, polypropylene and polyethylene block copolymer, pore former and extractant is (3-15): (5-15): (5-15): (70-85): (60-80). On this basis, the ratio of the polyethylene, polypropylene, polypropylene and polyethylene block copolymer, pore former and extractant can further preferably be (3-15): (5-15): (5-15): (70-85): (60-80), or (5-12): (5-12): (5-15): (70-85): (60-80), or (5-10): (5-10): (5-15): (70-85): (60-80).
[0122] According to the method for preparing a battery separator of any embodiment of the fourth aspect of the present invention, in the block copolymer of polypropylene and polyethylene, the mass ratio of polyethylene to polypropylene is 1:(1-3). On this basis, in the block copolymer of polypropylene and polyethylene, the mass ratio of polyethylene to polypropylene can further preferably be 1:(1-2.4), or 1:(1-1.5).
[0123] According to the method for preparing a battery separator of any embodiment of the fourth aspect of the present invention, the block copolymer of polypropylene and polyethylene is polymerized by polyethylene and polypropylene in a mass ratio of 1: (1 to 3). On this basis, the block copolymer of polypropylene and polyethylene can further preferably be polymerized by polyethylene and polypropylene in a mass ratio of 1: (1 to 2.4) or 1: (1 to 1.5).
[0124] In the method for preparing a battery separator according to any embodiment of the fourth aspect of the present invention, the polypropylene is a syndiotactic polypropylene.
[0125] As described herein, selecting "syndiotactic polypropylene" can increase the flexibility and toughness of the diaphragm, and further improve the puncture strength of the diaphragm.
[0126] In the battery separator composition according to any embodiment of the fourth aspect of the present invention, the molecular weight of the polypropylene is in the range of 80,000 to 700,000.
[0127] According to the method for preparing a battery separator of any embodiment of the fourth aspect of the present invention, the polyethylene is high-density polyethylene, and the molecular weight of the high-density polyethylene is in the range of 500,000 to 700,000, and more preferably in the range of 500,000 to 600,000.
[0128] According to the method for preparing a battery separator according to any embodiment of the fourth aspect of the present invention, the melting point of the high-density polyethylene is 130-142°C.
[0129] According to the method for preparing a battery separator according to any embodiment of the fourth aspect of the present invention, the block copolymer of polypropylene and polyethylene is an AB-type diblock copolymer;
[0130] Wherein, the molecular weight of the block copolymer is 500,000 to 2,000,000;
[0131] The length of the polypropylene segment in the block copolymer is 150,000 to 250,000 units, and the length of the polyethylene segment in the block copolymer is 100,000 to 200,000 units.
[0132] According to the method for preparing a battery separator according to any embodiment of the fourth aspect of the present invention, the block copolymer of polypropylene and polyethylene is an AB-type diblock copolymer;
[0133] The molecular weight of the block copolymer is 1 million to 1.8 million, the length of the polypropylene segment in the block copolymer is 190,000 to 250,000 units, and the length of the polyethylene segment in the block copolymer is 150,000 to 200,000 units. On this basis, the molecular weight of the block copolymer can also be preferably 1.2 million to 1.8 million, or 1.3 million to 1.8 million, or 1.4 million to 1.8 million.
[0134] As described herein, "the length of the polypropylene segment and the length of the polyethylene segment" will affect the puncture strength of the diaphragm. Specifically, the chain length of the polyethylene segment and the chain length of the polypropylene segment in the block copolymer will affect the compatibility of polypropylene and polyethylene, and the tight adhesion of the ternary structure (polyethylene, polypropylene, block copolymer) in the diaphragm, thereby affecting the puncture strength of the diaphragm.
[0135] According to any embodiment of the battery separator of the fourth aspect of the present invention, the polypropylene segment in the block copolymer is a syndiotactic polypropylene segment.
[0136] A method for preparing a battery separator according to any embodiment of the fourth aspect of the present invention comprises the steps of:
[0137] S1. Raw materials are extruded and melted;
[0138] S2. Die extrusion;
[0139] S3. Casting cooling;
[0140] S4. Longitudinal stretching and transverse stretching;
[0141] S5. Extraction;
[0142] S6. Molding process.
[0143] As described in step S4 herein, the order of longitudinal stretching and transverse stretching generally depends on the specific process. For example, if it is asynchronous stretching, in order to ensure that the diaphragm is not torn and to save equipment space, the longitudinal stretching is generally selected first and the transverse stretching is selected later; if it is synchronous stretching, the longitudinal stretching and the transverse stretching will be carried out simultaneously.
[0144] According to the method for preparing a battery separator according to any embodiment of the fourth aspect of the present invention, in step S1, the raw materials include polyethylene, polypropylene, a block copolymer of polypropylene and polyethylene, and a pore former.
[0145] According to the method for preparing a battery separator of any embodiment of the fourth aspect of the present invention, the pore-forming agent refers to a high-boiling-point hydrocarbon liquid or some substances with relatively low molecular weight, including any one, two or more of paraffin oil, kerosene and white oil;
[0146] The extractant includes any one, two or more of dichloromethane, chloroform, carbon tetrachloride, gasoline and hydrocarbon cleaning agent.
[0147] According to the method for preparing a battery separator according to any embodiment of the fourth aspect of the present invention, in step S1, the extrusion temperature of the raw material is 140 to 205° C.;
[0148] In step S2, the extrusion temperature of the die head is 140-210°C;
[0149] In step S3, the casting cooling temperature is 15 to 35° C.;
[0150] In step S4, the temperature of the longitudinal stretching is 40-100°C; the temperature of the transverse stretching is 100-160°C; the ratio of the longitudinal stretching is 5-8; and the ratio of the transverse stretching is 4-9.
[0151] The extrusion temperature of the raw materials and the extrusion temperature of the die are 10 to 15°C higher than those of the conventional wet process, which can better fuse the ternary compounds and improve the consistency of the diaphragm.
[0152] A fifth aspect of the present invention provides a lithium battery, wherein the lithium battery comprises a separator;
[0153] The separator comprises the composition for battery separator according to any embodiment of the first aspect of the present invention; or
[0154] The separator is a battery separator according to any embodiment of the second aspect of the present invention; or
[0155] The separator is a battery separator according to any embodiment of the third aspect of the present invention; or
[0156] The diaphragm is a diaphragm prepared by the method described in any embodiment of the fourth aspect of the present invention.
[0157] Any embodiment of any aspect of the present invention can be combined with other embodiments without contradiction. In addition, in any embodiment of any aspect of the present invention, any technical feature can be applied to the technical feature in other embodiments without contradiction.
[0158] Under the premise that there is no contradiction, any technical feature of any aspect of the present invention or any embodiment of any aspect is also applicable to any other embodiment or any embodiment of any other aspect. Of course, when applicable to each other, the corresponding features can be appropriately modified if necessary. The various aspects and features of the present invention are further described below.
[0159] 3. Beneficial effects
[0160] Compared with the prior art, the present invention has the following beneficial effects:
[0161] First, the composition of the battery separator provided by the present invention, or the battery separator:
[0162] (1) The film is made of polyethylene, polypropylene, and polyethylene-polypropylene block copolymer, and the thickness of the film can be as low as 3 μm. On this basis, the film still has a qualified film rupture temperature and a qualified thermal shrinkage rate, and especially has significantly excellent mechanical properties such as puncture strength and tensile strength.
[0163] (2) The addition of the polyethylene-polypropylene block copolymer can enhance the compatibility between polypropylene and polyethylene, and at the same time increase the compatibility between polypropylene and the pore-forming agent, thereby improving the uniformity of the diaphragm, and improving the thickness consistency and pore size uniformity.
[0164] (3) On this basis, by controlling the quality of the polyethylene and polypropylene polymerization in the polypropylene-polyethylene block copolymer within a certain range, the uniformity of the membrane can be further optimized, the consistency of the membrane thickness and the uniformity of the pore size can be further improved, and the mechanical properties of the membrane, such as puncture strength and shrinkage rate, can be optimized.
[0165] Second, the raw material or preparation method of the battery separator provided by the present invention:
[0166] (1) The invention uses polyethylene, polypropylene, and polyethylene-polypropylene block copolymer as raw materials and adopts a wet process to prepare the diaphragm, while retaining the advantages of the diaphragm prepared by the wet process; the addition of the polyethylene-polypropylene block copolymer can enhance the compatibility of polypropylene and polyethylene, and at the same time increase the compatibility of the raw materials and the pore-forming agent, laying a foundation for extruding into a uniform melt, thereby ensuring the uniformity of the prepared diaphragm, the consistency of thickness, and the uniformity of pore size.
[0167] Based on the above one and two, it is further explained that, in order to obtain better physical properties of the membrane, especially considering the consistency of membrane pore formation and uniformity of pore size, as well as tensile strength and puncture strength; it is preferred that the amount of block copolymer is not less than the amount of polyethylene. DETAILED DESCRIPTION
[0168] All documents cited in the present invention are incorporated herein by reference in their entirety, and if the meanings expressed in these documents are inconsistent with the present invention, the description of the present invention shall prevail. In addition, the various terms and phrases used in the present invention have the general meanings known to those skilled in the art. Even so, the present invention still hopes to provide a more detailed description and explanation of these terms and phrases. If the terms and phrases mentioned are inconsistent with the known meanings, the meanings expressed in the present invention shall prevail.
[0169] When items are described by using the conjunction terms "... and / or...," etc., the description should be understood to include any one of the associated listed items and all combinations of one or more thereof.
[0170] In general, the use of the term "about" indicates an approximate value that may vary depending on the desired properties obtained by the disclosed subject matter, and will be interpreted in a context-dependent manner based on function. Therefore, one of ordinary skill in the art will be able to interpret a certain degree of difference on a case-by-case basis. In some cases, the number of significant figures used when expressing a particular value can be a representative technique for determining the difference allowed by the term "about". In other cases, a gradient in a range of values can be used to determine the range of differences allowed by the term "about". Further, all ranges in this disclosure are inclusive and combinable, and reference to the values stated in the range includes each value within the range.
[0171] In the present invention, the term "comprising" or "containing" means that various components can be used together in the composition of the present invention. Therefore, the terms "consisting mainly of" and "consisting of" are included in the terms "comprising" or "containing".
[0172] Unless otherwise defined, the "syndiotactic polypropylene" used herein may also be referred to as "syndiotactic polypropylene" or "syndiotactic polypropylene".
[0173] Unless otherwise defined, "molecular weight" as used herein is average molecular weight.
[0174] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the terms used herein and / or include any and all combinations of one or more of the associated listed items.
[0175] The following will disclose any feature in this specification, unless otherwise stated, can be replaced by other equivalent or alternative features with similar purposes. Unless otherwise stated, each feature is just an example in a series of equivalent or similar features. It is described only to help understand the present invention and should not be regarded as a specific limitation of the present invention. Those who do not indicate specific conditions in the embodiment are carried out according to normal conditions or the conditions recommended by the manufacturer. Those who do not indicate the manufacturer of the reagents or instruments used are all conventional products that can be purchased.
[0176] The present invention is further described below in conjunction with specific embodiments.
[0177] Example 1
[0178] (1) The separator provided in this embodiment is shown in #1 of Table 1. Calculated by mass ratio, the separator contains high-density polyethylene, syndiotactic polypropylene, and a block copolymer of polyethylene and polypropylene in a ratio of 10:5:8.
[0179] Among them, the block copolymer of polypropylene and polyethylene is an AB type diblock copolymer, wherein the length of the polypropylene segment in the block copolymer is 190,000 units, and the length of the polyethylene segment in the block copolymer is 180,000 units; further, the block copolymer is formed by polymerizing polyethylene and polypropylene in a mass ratio of 1:1, and the molecular weight of the polyethylene used is: 1.3 million, and the molecular weight of the polypropylene is: 180,000.
[0180] The high-density polyethylene used in this embodiment has an average molecular weight of 600,000 and a melting point of 135-142°C.
[0181] The molecular weight of the syndiotactic polypropylene used in this embodiment is 170,000.
[0182] (2) The raw materials and proportions for preparing the diaphragm provided in this embodiment are as follows:
[0183] High-density polyethylene, syndiotactic polypropylene, block copolymer of polyethylene and polypropylene, paraffin oil pore former and dichloromethane extractant, wherein the dosage ratio of polyethylene, polypropylene, block copolymer of polypropylene and polyethylene, pore former and extractant is 10:5:8:77:70.
[0184] (3) Based on the raw materials and proportions provided in (2), this embodiment also provides a wet method for preparing the diaphragm, and the specific process includes:
[0185] The finished product is prepared after polyethylene, polypropylene, polypropylene and polyethylene block copolymer and pore-forming agent are mixed and subjected to extrusion melting, die extrusion, casting cooling, longitudinal stretching, transverse stretching, extraction with an extractant, drying, shaping, winding and slitting. The key parameters are set as follows: feed rate: 50±2kg / h, casting speed: 6.5±0.2m / min, fixed screw speed: 105rpm; extrusion temperature: 194±5℃; die temperature: 197℃; casting quenching temperature: 25℃; longitudinal stretching ratio: 7; transverse stretching ratio: 6; longitudinal stretching temperature: 92±2℃; transverse stretching temperature: 123±2℃; transverse stretching temperature (shaping): 131±2℃.
[0186] Based on the wet preparation process described in (3) above, in this embodiment, a separator for an ion battery with a porosity of 50% and a thickness of 9.3 (±0.2) μm as shown in #1 of Table 1 can be finally prepared.
[0187] (4) It should be noted that:
[0188] For example, by adjusting the process index of longitudinal stretching and transverse stretching, the parameters of the process index are within the range of longitudinal stretching temperature: 50-100°C, transverse stretching temperature: 110-160°C, longitudinal stretching ratio is 5-8, transverse stretching ratio is 4-9, the porosity of the membrane can be controlled within 40%-60%;
[0189] For example, by adjusting the process index of feed amount and casting speed so that the parameters of the process index are within the range of feed amount: 20-80 kg / h, casting speed: 4-12 m / min, the thickness of the film can be controlled within the range of 3-12 μm.
[0190] Example 2
[0191] (1) The diaphragm provided in this embodiment is shown in #2 of Table 1. Calculated by mass ratio, the diaphragm contains high-density polyethylene, syndiotactic polypropylene, and a block copolymer of polyethylene and polypropylene in a ratio of 10:10:5.
[0192] The block copolymer of polypropylene and polyethylene is prepared by polymerizing polyethylene and polypropylene in a mass ratio of 1:1.
[0193] (2) The raw materials and proportions for preparing the diaphragm provided in this embodiment are as follows:
[0194] High-density polyethylene, syndiotactic polypropylene, block copolymer of polyethylene and polypropylene, paraffin oil pore former and dichloromethane extractant, wherein the dosage ratio of polyethylene, polypropylene, block copolymer of polypropylene and polyethylene, pore former and extractant is 10:10:5:75:70.
[0195] (3) Based on the raw materials and proportions provided in (2), this embodiment also provides a wet preparation process for the diaphragm, and the preparation process is the same as the specific preparation process for the ion battery diaphragm shown in #1 of Example 1.
[0196] Example 3
[0197] (1) The diaphragm provided in this embodiment is shown in #3 of Table 1. Calculated by mass ratio, the diaphragm contains high-density polyethylene, syndiotactic polypropylene, and a block copolymer of polyethylene and polypropylene in a ratio of 5:8:10.
[0198] The block copolymer of polypropylene and polyethylene is prepared by polymerizing polyethylene and polypropylene in a mass ratio of 1:1.
[0199] (2) The raw materials and proportions for preparing the diaphragm provided in this embodiment are as follows:
[0200] High-density polyethylene, syndiotactic polypropylene, block copolymers of polyethylene and polypropylene, paraffin oil pore formers and dichloromethane extractants,
[0201] The dosage ratio of the polyethylene, polypropylene, polypropylene and polyethylene block copolymer, pore former and extractant is 5:8:10:77:70.
[0202] (3) Based on the raw materials and proportions provided in (2), this embodiment also provides a wet preparation process for the diaphragm, and the preparation process is the same as the specific preparation process for the ion battery diaphragm shown in #1 of Example 1.
[0203] Example 4
[0204] (1) The diaphragm provided in this embodiment is shown in #4 of Table 1. Calculated by mass ratio, the diaphragm contains high-density polyethylene, syndiotactic polypropylene, and a block copolymer of polyethylene and polypropylene in a ratio of 12:10:3.
[0205] The block copolymer of polypropylene and polyethylene is prepared by polymerizing polyethylene and polypropylene in a mass ratio of 1:1.
[0206] (2) The raw materials and proportions for preparing the diaphragm provided in this embodiment are as follows:
[0207] High-density polyethylene, syndiotactic polypropylene, block copolymer of polyethylene and polypropylene, paraffin oil pore former and dichloromethane extractant, wherein the dosage ratio of polyethylene, polypropylene, block copolymer of polypropylene and polyethylene, pore former and extractant is 12:10:3:75:70.
[0208] (3) Based on the raw materials and proportions provided in (2), this embodiment also provides a wet preparation process for the diaphragm, and the preparation process is the same as the specific preparation process for the ion battery diaphragm shown in #1 of Example 1.
[0209] Example 5
[0210] (1) The diaphragm provided in this embodiment is shown in #5 of Table 1. Calculated by mass ratio, the diaphragm contains high-density polyethylene, syndiotactic polypropylene, and a block copolymer of polyethylene and polypropylene in a ratio of 10:10:8.
[0211] The block copolymer of polypropylene and polyethylene is prepared by polymerizing polyethylene and polypropylene in a mass ratio of 1:1.
[0212] (2) The raw materials and proportions for preparing the diaphragm provided in this embodiment are as follows:
[0213] High-density polyethylene, syndiotactic polypropylene, block copolymer of polyethylene and polypropylene, paraffin oil pore former and dichloromethane extractant, wherein the dosage ratio of polyethylene, polypropylene, block copolymer of polypropylene and polyethylene, pore former and extractant is 10:10:8:72:70.
[0214] (3) Based on the raw materials and proportions provided in (2), this embodiment also provides a wet preparation process for the diaphragm, and the preparation process is the same as the specific preparation process for the ion battery diaphragm shown in #1 of Example 1.
[0215] Example 6
[0216] (1) The diaphragm provided in this embodiment is shown in #6 of Table 1. The only difference compared with Example 2 is that the polypropylene used is not a syndiotactic polypropylene but an isotactic polypropylene. The rest is the same as Example 2.
[0217] (2) The raw materials and proportions for preparing the diaphragm provided in this embodiment are also basically the same as those in Example 2, with the only difference being that the polypropylene used is not a syndiotactic polypropylene but an isotactic polypropylene.
[0218] (3) Based on the raw materials and proportions provided in (2), this embodiment also provides a wet preparation process for the diaphragm, and the preparation process is the same as that in Example 2.
[0219] Example 7
[0220] (1) The diaphragm provided in this embodiment is shown in #7 of Table 1. The only difference compared with Example 2 is that the block copolymer of polypropylene and polyethylene is polymerized by polyethylene and polypropylene in a mass ratio of 3:7. The rest is the same as Example 2.
[0221] (2) The raw materials and proportions for preparing the diaphragm provided in this embodiment are also basically the same as those in Example 2, except that the block copolymer of polypropylene and polyethylene used is polymerized from polyethylene and polypropylene in a mass ratio of 3:7.
[0222] (3) Based on the raw materials and proportions provided in (2), this embodiment also provides a wet preparation process for the diaphragm, and the preparation process is the same as that in Example 2.
[0223] Example 8
[0224] (1) The diaphragm provided in this embodiment is shown in #8 of Table 1. The only difference compared with Example 2 is that the block copolymer of polypropylene and polyethylene is polymerized by polyethylene and polypropylene in a mass ratio of 1:3. The rest is the same as Example 2.
[0225] (2) The raw materials and proportions for preparing the diaphragm provided in this embodiment are also basically the same as those in Example 2, except that the block copolymer of polypropylene and polyethylene used is polymerized from polyethylene and polypropylene in a mass ratio of 1:3.
[0226] (3) Based on the raw materials and proportions provided in (2), this embodiment also provides a wet preparation process for the diaphragm, and the preparation process is the same as that in Example 2.
[0227] Example 9
[0228] (1) The diaphragm provided in this embodiment is shown in #9 of Table 1. Calculated by mass ratio, the diaphragm contains high-density polyethylene, syndiotactic polypropylene, and a block copolymer of polyethylene and polypropylene in a ratio of 12:10:15.
[0229] The rest is the same as Example 4.
[0230] (2) The raw materials and proportions for preparing the diaphragm provided in this embodiment are as follows:
[0231] High-density polyethylene, syndiotactic polypropylene, block copolymer of polyethylene and polypropylene, paraffin oil pore former and dichloromethane extractant, wherein the dosage ratio of polyethylene, polypropylene, block copolymer of polypropylene and polyethylene, pore former and extractant is 12:10:15:75:70.
[0232] The rest is the same as Example 4.
[0233] (3) Based on the raw materials and proportions provided in (2), this embodiment also provides a wet preparation process for the diaphragm, and the preparation process is the same as the specific preparation process for the ion battery diaphragm shown in #1 of Example 1.
[0234] Comparative Example 1
[0235] (1) The diaphragm provided in this comparative example is shown in D#1 in Table 1. According to the mass ratio, the diaphragm contains high-strength polyethylene and high-density polyethylene, and does not contain a block copolymer of polyethylene and polypropylene;
[0236] The ratio of the high-density polyethylene to the high-strength polyethylene is 11:10, and the rest is the same as in Example 2.
[0237] The high-density polyethylene used in this embodiment is the same as that in Example 1;
[0238] The high-strength polyethylene used is UHMWPE, a high-performance polymer with a molecular weight of over 1 million.
[0239] (2) The raw materials and proportions for preparing the diaphragm provided in this comparative example are as follows:
[0240] High-density polyethylene, high-strength polyethylene, paraffin oil pore-forming agent and dichloromethane extractant, wherein the dosage ratio of the polyethylene, polypropylene, pore-forming agent and extractant is 11:10:79:70.
[0241] (3) Based on the raw materials and proportions provided in (2), the wet process for preparing the diaphragm described in this comparative example, after repeated experiments, the optimal preparation parameters are as follows:
[0242] The finished product is prepared after the processes of extrusion melting, die extrusion, cast cooling, longitudinal stretching, transverse stretching, extraction, drying, shaping, winding and slitting, wherein the key parameter settings are as follows: fixed screw speed: 98rpm; extrusion temperature: 190°C; die temperature: 193°C; cast quenching temperature: 25°C; longitudinal stretching ratio: 6.5; transverse stretching ratio: 6; longitudinal stretching temperature: 70°C; transverse stretching temperature: 112°C; transverse stretching temperature (shaping): 120°C.
[0243] Comparative Example 2
[0244] (1) The diaphragm provided in this comparative example is shown in D#2 in Table 1. The only difference compared with Example 2 is that the membrane no longer contains the block copolymer of polyethylene and polypropylene.
[0245] (2) The raw materials for preparing the diaphragm provided in this comparative example are also basically the same as those in Example 2, with the only difference being that among the raw materials used, a physical mixture of polyethylene and polypropylene is used to replace the block copolymer of polyethylene and polypropylene used in the original Example 2, wherein the physical mixture of polyethylene and polypropylene is formed by physically mixing polyethylene and polypropylene in a mass ratio of 1:1.
[0246] The rest are the same as in Example 2;
[0247] (3) Based on the raw materials and proportions provided in (2), the wet preparation process of the diaphragm provided in this comparative example is the same as that in Example 2.
[0248] Comparative Example 3
[0249] (1) The diaphragm provided in this comparative example is shown in D#3 in Table 1. The only difference compared with Example 2 is that the membrane no longer contains polypropylene and no longer contains a block copolymer of polyethylene and polypropylene.
[0250] (2) The raw materials for preparing the diaphragm provided in this comparative example are also basically the same as those in Example 2, with the only difference being that polyethylene is used to replace the syndiotactic polypropylene used in the original Example 2; and polyethylene is used to replace the block copolymer of polyethylene and polypropylene used in the original Example 2.
[0251] The rest are the same as in Example 2;
[0252] (3) Based on the raw materials and proportions provided in (2), the wet preparation process of the diaphragm provided in this comparative example is the same as that in Example 2.
[0253] Comparative Example 4
[0254] (1) The diaphragm provided in this comparative example is shown in D#4 in Table 1. The only difference compared with Example 4 is that, calculated by mass ratio, the diaphragm contains high-density polyethylene, syndiotactic polypropylene, and a block copolymer of polyethylene and polypropylene in a ratio of 12:10:1.
[0255] The rest is the same as Example 4.
[0256] Table 1 Parameters of membranes prepared in the examples of the present invention and comparative examples
[0257]
[0258]
[0259] Example 10
[0260] The separator provided in this embodiment is shown in #10 of Table 1. The raw materials and proportions for preparing the separator provided in this embodiment are the same as those in Example 1. The only difference is that the thickness of the membrane finally prepared is expected to be close to 3 μm.
[0261] The wet preparation process of the diaphragm described in this embodiment specifically includes:
[0262] The finished product is prepared after polyethylene, polypropylene, polypropylene and polyethylene block copolymer and pore-forming agent are mixed and subjected to extrusion melting, die extrusion, casting cooling, longitudinal stretching, transverse stretching, extraction with an extractant, drying, shaping, winding and slitting. The key parameters are set as follows: feed rate: 42±2kg / h, casting speed: 7.8±0.2m / min, fixed screw speed: 105rpm; extrusion temperature: 194±5℃; die temperature: 197℃; casting quenching temperature: 25℃; longitudinal stretching ratio: 6.5; transverse stretching ratio: 6.5; longitudinal stretching temperature: 91±2℃; transverse stretching temperature: 122±2℃; transverse stretching temperature (shaping): 130±2℃.
[0263] Based on the wet preparation process described in (3) above, a lithium ion battery separator with a porosity of 47% and a thickness of 3.4 (±0.4) μm as shown in #10 in Table 1 can be finally prepared in this embodiment.
[0264] Embodiment 11
[0265] The separator provided in this embodiment is shown in #11 of Table 1. The raw materials and proportions for preparing the separator provided in this embodiment are the same as those in Example 1. The only difference is that the thickness of the membrane finally prepared is expected to be close to 5 μm.
[0266] The wet preparation process of the diaphragm described in this embodiment specifically includes:
[0267] The finished product is prepared after polyethylene, polypropylene, polypropylene and polyethylene block copolymer and pore-forming agent are mixed and subjected to extrusion melting, die extrusion, casting cooling, longitudinal stretching, transverse stretching, extraction with an extractant, drying, shaping, winding and slitting. The key parameters are set as follows: feed rate: 45±2kg / h, casting speed: 7.2±0.2m / min, fixed screw speed: 105rpm; extrusion temperature: 194±5℃; die temperature: 197℃; casting quenching temperature: 25℃; longitudinal stretching ratio: 6.5; transverse stretching ratio: 6.5; longitudinal stretching temperature: 91±2℃; transverse stretching temperature: 122±2℃; transverse stretching temperature (shaping): 130±2℃.
[0268] Based on the wet preparation process described in (3) above, a lithium-ion battery separator with a porosity of 47% and a thickness of 5.2 (±0.4) μm as shown in #11 in Table 1 can be finally prepared in this embodiment.
[0269] At the same time, based on the separators #1 to #11 provided by the present invention, any of the separators can be applied to lithium-ion batteries.
Claims
1. A composition for a battery separator, characterized in that: The composition comprises: Polyethylene; Syndiotactic polypropylene; Block copolymers of polypropylene and polyethylene; Wherein, calculated by mass ratio, the ratio of polyethylene, polypropylene and block copolymer is (3-15): (5-15): (3-15).
2. The composition for battery separator according to claim 1, characterized in that In the block copolymer of polypropylene and polyethylene, the mass ratio of polyethylene to polypropylene is 1:(1-3); or, The block copolymer of polypropylene and polyethylene is prepared by polymerizing polyethylene and polypropylene in a mass ratio of 1: (1-3).
3. The composition for battery separator according to claim 1 or 2, characterized in that: The block copolymer of polypropylene and polyethylene is an AB type diblock copolymer; Wherein, the molecular weight of the block copolymer is 500,000 to 2,000,000; The length of the polypropylene chain segment is 150,000 to 250,000 units, and the length of the polyethylene chain segment is 100,000 to 200,000 units.
4. The composition for battery separator according to claim 1 or 2, characterized in that: The molecular weight range of the polypropylene is 80,000 to 700,000; And / or, the polyethylene is a high-density polyethylene with a molecular weight ranging from 500,000 to 700,000.
5. A battery separator, characterized in that: The separator comprises the composition of the battery separator according to any one of claims 1 to 4; Alternatively, the raw material for preparing the separator includes the composition for battery separator according to any one of claims 1 to 4.
6. The battery separator according to claim 5, characterized in that: When the film thickness is 3 to 10 μm, the separator has: A membrane rupture temperature of 145 to 170°C; and / or A membrane melting point of 135 to 155°C; and / or Puncture strength of 300-500 gf; and / or, A heat shrinkage in MD of no more than 2% at a temperature not exceeding 150°C; and / or, A TD heat shrinkage of no more than 1.5% at a temperature not exceeding 150°C; and / or, 2500~4000Kgf / cm 2 MD tensile strength; and / or, 1500~3200Kgf / cm 2 TD tensile strength; Alternatively, when the film thickness is 8 to 10 μm, the separator has: Membrane rupture temperature of 160-170°C; and / or, A membrane melting point of 140 to 155°C; and / or Puncture strength of 410-500 gf; and / or, A heat shrinkage in MD of no more than 2% at a temperature not exceeding 150°C; and / or, A TD heat shrinkage of no more than 1.5% at a temperature not exceeding 150°C; and / or, 3200~4000Kgf / cm 2 MD tensile strength; and / or, 2100~3200Kgf / cm 2 TD tensile strength; Alternatively, when the film thickness is 3 to 6 μm, the separator has: A membrane rupture temperature of 145 to 165°C; and / or A membrane melting point of 135 to 150°C; and / or, Puncture strength of 300-450 gf; and / or, A heat shrinkage in MD of no more than 2% at a temperature not exceeding 150°C; and / or, A TD heat shrinkage of no more than 1.5% at a temperature not exceeding 150°C; and / or, 2500~3500Kgf / cm 2 MD tensile strength; and / or, 1500~3500Kgf / cm 2 TD tensile strength.
7. The battery separator according to claim 5 or 6, characterized in that: The raw materials for preparing the diaphragm also include a pore-forming agent and an extractant; The dosage ratio of the polyethylene, polypropylene, polypropylene and polyethylene block copolymer, pore former and extractant is (3-15): (5-15): (3:15): (70-85): (60-80).
8. The battery separator according to claim 7, characterized in that: The diaphragm is prepared by a wet process.
9. A method for preparing a battery separator, characterized in that: The diaphragm is prepared by a wet process, comprising the steps of: S1. Raw materials are extruded and melted; S2. Die extrusion; S3. Casting cooling; S4. Longitudinal stretching and transverse stretching; S5. Extraction; S6. Molding process; Wherein, in step S1, the raw materials include polyethylene, polypropylene, polypropylene and polyethylene block copolymer and pore former in a dosage ratio of (3-15): (5-15): (3:15): (70-85).
10. The method for preparing a battery separator according to claim 9, characterized in that: In step S1, the extrusion temperature of the raw material is 140-205°C; In step S2, the extrusion temperature of the die head is 140-210°C; In step S3, the casting cooling temperature is 15 to 35° C.; In step S4, the temperature of the longitudinal stretching is 40-100°C; the temperature of the transverse stretching is 100-160°C; the ratio of the longitudinal stretching is 5-8; and the ratio of the transverse stretching is 4-9.
11. A lithium battery comprising a separator, characterized in that: The separator comprises the battery separator composition according to any one of claims 1 to 4; or The separator is the battery separator according to any one of claims 5 to 8; or The diaphragm is a diaphragm prepared by the method according to any one of claims 9 to 10.