Semiconductor radio frequency chip back through hole high-capacity capacitor structure and preparation method thereof

By adopting a back through-hole capacitor structure in semiconductor RF chips, the limitations of capacitors in the back process compatibility, space efficiency and cost are solved, and efficient manufacturing process optimization and performance improvement are achieved, which is suitable for the complex circuit requirements of modern electronic equipment. .

CN119095478APending Publication Date: 2024-12-06XIDIAN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411184680.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing capacitors have limitations in back process compatibility, space utilization efficiency and manufacturing costs, making it difficult to meet the needs of modern electronic devices for miniaturization, high performance and strong back process compatibility.

Method used

Adopt a large-capacity capacitor structure for back through holes in the substrate layer and epitaxial layer. By etching the back through holes in the substrate layer and the epitaxial layer, the interdigital electrode and the dielectric layer are set to form a back through hole capacitor structure, which is compatible with the back of the chip process, optimizes the manufacturing process and Save chip area.

Benefits of technology

Improves production efficiency and device performance consistency, reduces costs, enhances chip integration and functional density, and is suitable for complex circuit layouts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095478A_ABST
    Figure CN119095478A_ABST
Patent Text Reader

Abstract

The invention discloses a back through hole high-capacity capacitor structure of a semiconductor radio frequency chip. The capacitor structure sequentially comprises a substrate layer and an epitaxial layer from bottom to top, a plurality of back through holes penetrating through the substrate layer and the epitaxial layer are formed between the substrate layer and the epitaxial layer, and back through hole capacitor structures are arranged in the back through holes; the back through hole capacitor structure comprises a right side electrode, a dielectric layer, a left side electrode and a front metal layer; the right side electrode and the left side electrode are both of a multi-layer structure and intersect with each other to form an interdigital electrode. The dielectric layer is filled between the right side electrode and the left side electrode which are mutually crossed, the dielectric layer is filled between the electrodes, the right side electrode is connected with the front side metal layer located on the front side of the chip, and the left side electrode is grounded. The back through hole capacitor structure provided by the invention is compatible with a back surface process of chip manufacturing, the manufacturing process can be effectively optimized, the production efficiency can be improved, the performance and the consistency of the device can be ensured, the chip area can be saved, the integration level can be improved, and the cost can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of capacitors, and in particular relates to a semiconductor radio frequency chip back through hole large-capacitance capacitor structure and a preparation method thereof. Background Art

[0002] Capacitors are common key components in electronic devices, used to store and release charges and regulate current and voltage in circuits. As electronic devices develop towards miniaturization, high performance and multifunctionality, the design and manufacture of capacitors face more and more challenges. Although there are many types of capacitors on the market, their limitations in back-side process compatibility, space utilization efficiency and manufacturing costs still exist. Specific problems include: First, the limitation of back-side process processing: traditional capacitor structures are often difficult to perfectly integrate with modern complex back-side processes. Second, the space occupancy efficiency is not high: some capacitor structures fail to maximize the use of the back space of the device. Third, the high manufacturing cost: the manufacturing cost and complexity of existing capacitors limit their application in mass production. With the diversification and intelligence of electronic devices, the market demand for miniaturized, high-performance and back-side process-compatible capacitors is increasing. These capacitors not only need to occupy less space in terms of area, but also need to be able to be easily integrated into the existing electronic device manufacturing process. Summary of the invention

[0003] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a semiconductor radio frequency chip back-through hole large-capacitance capacitor structure and a preparation method thereof. The back-through hole capacitor structure is compatible with the back-side process of chip manufacturing, can effectively optimize the manufacturing process, improve production efficiency, ensure device performance and consistency, and at the same time save chip area, improve integration and reduce costs.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is:

[0005] A semiconductor radio frequency chip back-through hole large-capacitance capacitor structure, the capacitor structure comprises a substrate layer and an epitaxial layer in sequence from bottom to top;

[0006] A plurality of back through holes are provided between the substrate layer and the epitaxial layer, and the back through holes have back through hole capacitor structures disposed inside them;

[0007] The back via capacitor structure includes a right electrode, a dielectric layer, a left electrode and a front metal layer;

[0008] The right electrode and the left electrode are both multi-layer structures, and the two cross each other to form interdigitated electrodes;

[0009] The dielectric layer is filled between the right electrode and the left electrode that cross each other, and the dielectric layer is filled between the electrodes. The right electrode is connected to the front metal layer located on the front of the chip, and the left electrode is grounded.

[0010] In one embodiment, the right electrode is a multi-layer structure, including a right longitudinal metal layer arranged on the side wall of the back through hole and a plurality of right transverse electrode layers connected to the left side of the right longitudinal metal layer; the top of the right longitudinal metal layer and / or the top of the uppermost right transverse electrode layer is connected to the front metal layer;

[0011] The left electrode is a multi-layer structure, including a left longitudinal metal layer arranged on the side wall of the back through hole and a plurality of left transverse electrode layers connected to the right side of the left longitudinal metal layer. The left longitudinal metal layer and / or the left transverse electrode layer are grounded.

[0012] In one embodiment, the difference in number between the left lateral electrode layer and the right lateral electrode layer is 1.

[0013] In one embodiment, the material of the right longitudinal metal layer and the left longitudinal metal layer is any one or more of titanium nitride (TiN), tantalum nitride (TaN), titanium (Ti), tungsten (W), aluminum (Al), and gold (Au), with a height of 50-200μm; the material of the right lateral electrode layer and the left lateral electrode layer is any one or more of titanium nitride (TiN), tantalum nitride (TaN), titanium (Ti), tungsten (W), aluminum (Al), and gold (Au), with a thickness of 100-1000nm, the longitudinal distance between adjacent right lateral electrode layers and left lateral electrode layers is 10nm-1000nm, and the length of the lateral intersection portion is 30-40μm.

[0014] In one embodiment, the number of the right lateral electrode layers is three, and the number of the left lateral electrode layers is two.

[0015] In one embodiment, the material of the substrate layer is one of silicon carbide, silicon, sapphire, and gallium nitride, and the thickness after thinning is 50-200 μm; the material of the epitaxial layer is a group III nitride, and the thickness is 1-5 μm, and the group III nitride is a multi-component compound composed of one or two or more of gallium nitride, aluminum nitride, and indium nitride; the material of the dielectric layer is silicon dioxide (SiO 2 ), aluminum oxide (Al 2 O 3 ), hafnium oxide (HfO 2 ), Tantalum pentoxide (Ta 2 O 5 )、ZrO 2 ) any one or more of ).

[0016] The present invention also provides a method for preparing the semiconductor radio frequency chip back side through hole large-capacitance capacitor structure, comprising the following steps:

[0017] S1: Use the back-through hole etching process to etch the substrate layer and the epitaxial layer. The etching depth penetrates the substrate layer and the epitaxial layer until it contacts the front metal layer to form a back-through hole. In this step, a dilute HCl solution can be used to clean the thinned sample to remove possible contamination on the wafer. The etching process can use the inductively coupled plasma (ICP) method.

[0018] S2: In the back through hole, on the surface of the front metal layer, prepare the right lateral electrode layer, dielectric layer unit, left lateral electrode layer, dielectric layer unit, right lateral electrode layer, dielectric layer unit, ..., dielectric layer unit, right lateral electrode layer or left lateral electrode layer in sequence, etch into holes again and fill with metal, connect the right lateral electrode layers to obtain the right electrode, connect the left lateral electrode layers to obtain the left electrode, the right lateral electrode layers and the left lateral electrode layers form an interdigitated electrode structure, and each dielectric layer unit is filled between the electrodes to form a dielectric layer.

[0019] It is easy to understand that the ellipsis in this step refers to the cycle of left lateral electrode layer-dielectric layer unit-right lateral electrode layer-dielectric layer unit-left lateral electrode layer, or the cycle of left lateral electrode layer-dielectric layer unit-right lateral electrode layer-dielectric layer unit-left lateral electrode layer-dielectric layer unit-right lateral electrode layer. As needed, the number of left lateral electrode layers and right lateral electrode layers can be set, and the right lateral electrode layer or the left lateral electrode layer can be used to end the process.

[0020] In one embodiment, the right lateral electrode layer, the dielectric layer unit, the left lateral electrode layer, the dielectric layer unit, the right lateral electrode layer, the dielectric layer unit, ..., the dielectric layer unit, the right lateral electrode layer or the left lateral electrode layer are sequentially prepared on the surface of the front metal layer, and the implementation method is as follows:

[0021] S21: preparing a right lateral electrode layer on a portion of the surface of the front metal layer;

[0022] S22: preparing a dielectric layer unit on another part of the surface of the front metal layer and on the surface of the right lateral electrode layer obtained in S21;

[0023] S23: preparing a left lateral electrode layer on a part of the surface of the dielectric layer unit obtained in S22;

[0024] S24: preparing a dielectric layer unit on another part of the surface of the dielectric layer unit obtained in S22 and on the surface of the left lateral electrode layer obtained in S23;

[0025] S25: preparing a right lateral electrode layer on a portion of the surface of the dielectric layer unit obtained in S24;

[0026] S26: preparing a dielectric layer unit on another part of the surface of the dielectric layer unit obtained in S24 and on the surface of the right lateral electrode layer obtained in S25;

[0027] S27: Repeat S23 to S26, and end with preparing the left lateral electrode layer or preparing the right lateral electrode layer.

[0028] Since it is processed in the back through hole, it is easy to understand that the above-mentioned part of the surface and the other part of the surface of the present invention refer to the "lower surface" of the corresponding layer, which is divided into two parts, wherein the left lateral electrode layer is prepared on the left part of the dielectric layer unit, and the right lateral electrode layer is prepared on the right part of the dielectric layer unit.

[0029] In one embodiment, the holes are etched again and filled with metal, and the right side lateral electrode layers are connected to obtain the right side electrode, and the left side lateral electrode layers are connected to obtain the left side electrode. The implementation method is as follows:

[0030] By using photolithography and etching processes, the shapes of connection holes are etched on the right side of each right horizontal electrode layer and on the left side of each left horizontal electrode layer, and then metal is filled in the holes by electroplating to prepare the right vertical metal layer and the left vertical metal layer.

[0031] In one embodiment, the right lateral electrode layer and the left lateral electrode layer are both prepared by a photolithography-lift-off process, and the dielectric layer unit is both prepared by a plasma enhanced chemical vapor deposition (PECVD) method or a plasma enhanced atomic layer deposition (PEALD) method.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] First, the back-through-hole capacitor structure introduced in the present invention is more compatible with the back-side process flow of semiconductor RF wafers. Compatibility with the back-side process means that capacitor preparation and other device manufacturing and processing can be performed on the same chip at the same time. This can save costs and reduce the number of steps and time in the manufacturing process.

[0034] Second, more functional units and devices can be integrated on the same chip, improving the functional density and integration of the chip. This is particularly important for the design and manufacture of modern microelectronic devices, which can meet the requirements of increasingly complex and compact circuit layouts. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a structural schematic diagram of the chip front / back process of the present invention.

[0036] Figure 2 Schematic diagram of the structure of a back via capacitor in an embodiment of the present invention.

[0037] Figure 3 Schematic diagram of the structure of the right electrode in an embodiment of the present invention.

[0038] Figure 4 Schematic diagram of the structure of the left electrode in an embodiment of the present invention.

[0039] In the figure, 1. substrate layer; 2. epitaxial layer; 3. back via; 4. right side electrode; 41. right side longitudinal metal layer; 42. first right side lateral electrode layer; 43. second right side lateral electrode layer; 44. third right side lateral electrode layer; 5. dielectric layer; 6. left side electrode; 61. left side longitudinal metal layer; 62. first left side lateral electrode layer; 63. second left side lateral electrode layer. DETAILED DESCRIPTION

[0040] The embodiments of the present invention are described in detail below with reference to the accompanying drawings and examples.

[0041] In order to reduce the space occupied by capacitors and integrate them into the existing electronic equipment manufacturing process, the present invention provides a semiconductor radio frequency chip back through hole large-capacitance capacitor structure, specifically as follows Figure 1 and Figure 2 As shown, the capacitor structure of the present invention includes a substrate layer 1 and an epitaxial layer 2 from bottom to top, wherein a plurality of back through holes 3 are provided between the substrate layer 1 and the epitaxial layer 2, and a back through hole capacitor structure is provided inside the back through hole 3. The back through hole capacitor structure includes a right electrode 4, a dielectric layer 5, a left electrode 6 and a front metal layer 7. The front metal layer 7 can be located above the epitaxial layer 2, that is, the front of the chip. The structure of the present invention enables the back through hole capacitor structure to be prepared inside the back through hole 3 while performing the back process on the basis of completing the front process. The right electrode 4 and the left electrode 6 are both multilayer structures, which intersect with each other to form multilayer interdigitated electrodes, and the dielectric layer 5 is filled between the electrodes. The right electrode 4 is connected to the front metal layer 7, and the left electrode 6 is grounded. Specifically, the right electrode 4 can be interconnected with the front metal layer 7 through the vertical metal of the back through hole side wall, connected to the front of the chip, and the left electrode 6 can be directly connected to the ground through the vertical metal of the back through hole side wall.

[0042] According to this structure, since the back-via capacitor structure is compatible with the back-side process flow of semiconductor RF wafers, capacitors and other devices can be prepared on the same chip at the same time, thereby reducing the number of steps and time in the manufacturing process. In addition, due to the use of the back-via capacitor structure, more devices can be integrated on the same chip area to meet the requirements of complex circuit layout.

[0043] In the embodiments of the present invention, see Figure 3 The right electrode 4 is a multi-layer structure, including a right longitudinal metal layer 41 disposed on the side wall of the back through hole 3 and a plurality of right transverse electrode layers connected to the left side of the right longitudinal metal layer 41. In this embodiment, three right transverse electrode layers are selected, which are the first right transverse electrode layer 42, the second right transverse electrode layer 43 and the third right transverse electrode layer 44 from bottom to top. The longitudinal direction, i.e., the up-down direction of the present invention, is the direction from the substrate layer 1 to the epitaxial layer 2, and the transverse direction is the horizontal direction.

[0044] In this embodiment, the first right lateral electrode layer 42, the second right lateral electrode layer 43 and the third right lateral electrode layer 44 are connected to the right longitudinal metal layer 41 through their respective right sides, and are connected to the front metal layer 7 through the right longitudinal metal layer 41 and / or the third right lateral electrode layer 44, thereby being connected to the front side of the chip.

[0045] The material of the right longitudinal metal layer (41) can be any one or more of titanium nitride (TiN), tantalum nitride (TaN), titanium (Ti), tungsten (W), aluminum (Al), and gold (Au), with a height of 50-200 μm; the material of each right transverse electrode layer can also be any one or more of titanium nitride (TiN), tantalum nitride (TaN), titanium (Ti), tungsten (W), aluminum (Al), and gold (Au), with a thickness of 100-1000 nm. The longitudinal distance between adjacent right transverse electrode layers and left transverse electrode layers is 10nm-1000nm, and the length of the transverse intersection is 30-40μm. In this embodiment, the material of the right longitudinal metal layer 41 is aluminum (Al), with a height of 100μm. The material of each right transverse electrode layer is titanium (Ti), and the thickness is 150nm.

[0046] In the embodiments of the present invention, see Figure 4 The left electrode 6 is a multi-layer structure, including a left longitudinal metal layer 61 disposed on the side wall of the back through hole 3 and a plurality of left transverse electrode layers connected to the right side of the left longitudinal metal layer 61. In this embodiment, the left transverse electrode layer is selected to be two layers, namely, a first left transverse electrode layer 62 and a second left transverse electrode layer 63 from bottom to top.

[0047] In this embodiment, the first left lateral electrode layer 62 and the second left lateral electrode layer 63 are connected to the left longitudinal metal layer 61 through the left side edges, and are connected to the ground through the left longitudinal metal layer 61 .

[0048] The material of the left longitudinal metal layer (61) can be any one or more of titanium nitride (TiN), tantalum nitride (TaN), titanium (Ti), tungsten (W), aluminum (Al), and gold (Au), with a height of 50-200 μm. The material of each left lateral electrode layer can also be any one or more of titanium nitride (TiN), tantalum nitride (TaN), titanium (Ti), tungsten (W), aluminum (Al), and gold (Au), with a thickness of 100-1000 nm. In this embodiment, the material of the left longitudinal metal layer 61 is aluminum (Al), with a thickness of 100 μm. The material of each left lateral electrode layer is titanium (Ti), and the thickness is 150 nm.

[0049] The material of the substrate layer 1 of the present invention can be one of silicon carbide, silicon, sapphire, and gallium nitride, and the thickness after thinning is 50-200 μm; the material of the epitaxial layer 2 is a group III nitride, and the thickness is 1-5 μm; the group III nitride can be, for example, a multi-component compound composed of one or two or more of gallium nitride, aluminum nitride, and indium nitride; the material of the dielectric layer 5 can be silicon dioxide (SiO 2 ), aluminum oxide (Al 2 O 3 ), hafnium oxide (HfO 2 ), Tantalum pentoxide (Ta 2 O 5 )、ZrO 2 ) in any one or more. In this embodiment, the material of the substrate layer 1 is silicon, and the thickness after thinning is 98 μm. The material of the epitaxial layer 2 is a multi-component compound composed of gallium nitride and aluminum gallium nitrogen, and the thickness is 2 μm. The material of the dielectric layer 5 is aluminum oxide (Al 2 O 3 ), with a total thickness of 80 μm.

[0050] In more embodiments, the number of left and right transverse electrode layers can be selected as needed. Generally speaking, the two numbers can be equal or differ by 1, and preferably the number of right transverse electrode layers is 1 more than the number of left transverse electrode layers.

[0051] On the basis of the above embodiments, the present invention further provides a semiconductor radio frequency chip back side through hole large-capacitance capacitor structure and a preparation method thereof, comprising the following steps:

[0052] S1: Clean the thinned wafer, and etch the substrate layer 1 and the epitaxial layer 2 using a back through hole etching process. The etching depth penetrates the substrate layer 1 and the epitaxial layer 2 until they contact the front metal layer 7 to form a back through hole 3.

[0053] S2: In the back through hole 3, on the surface of the front metal layer 7, prepare the right lateral electrode layer, dielectric layer unit, left lateral electrode layer, dielectric layer unit, right lateral electrode layer, dielectric layer unit, ..., dielectric layer unit, right lateral electrode layer or left lateral electrode layer in sequence, etch into holes again and fill with metal, connect the right lateral electrode layers to obtain the right electrode 4, connect the left lateral electrode layers to obtain the left electrode 6, the right lateral electrode layers and the left lateral electrode layers form an interdigitated electrode structure, and the dielectric layer units are filled between the electrodes to form a dielectric layer 5.

[0054] Taking three right lateral electrode layers and two left lateral electrode layers as an example, the preparation process of the present invention is described in detail as follows:

[0055] S1: First, the thinned bonded wafer is cleaned in a wet process module with a dilute HCl solution (volume ratio 1:10) to remove possible contamination on the wafer. 2 Plasma sweep cleaning modifies the wafer surface and increases metal adhesion.

[0056] S2: Based on S1, a process of etching the back via 3 is performed, and the substrate layer 1 and the epitaxial layer 2 are etched by an inductively coupled plasma (ICP) etching method. The etching depth penetrates the substrate layer 1 and the epitaxial layer 2 until they contact the front metal layer 7, thereby preparing the back via 3.

[0057] S3: Based on S2, on the front metal layer 7, a photolithography process is first used to define the pattern of the third right lateral electrode layer 44, and then a 150nm Ti film is prepared as the third right lateral electrode layer 44 by magnetron sputtering. The sputtering gas is high-purity argon (purity 99.999%), and the argon flow rate is 15cm 3 / min. The back vacuum of the system during coating is 10 -5 Pa, and the working gas pressure is 0.2 Pa. After sputtering, the stripping process is used to soak the sample in acetone until the metal in the undefined area falls off, and then the sample is placed in isopropanol for 5 minutes to remove the acetone residue.

[0058] S4: Based on S3, 11nm Al was prepared by plasma enhanced atomic layer deposition (PEALD) 2 O 3 As a dielectric layer unit, the process temperature is 250℃, and the carrier gas is N 2 and Ar,N 2 The flow rate was 120 sccm, the Ar flow rate was 75 sccm, the chamber pressure was maintained at 7 hPa, and the oxygen flow rate was 2000 sccm.

[0059] S5: Based on S4, on the surface of the dielectric layer unit, a photolithography process is first used to define the pattern of the second left lateral electrode layer 63, and then a 150nm Ti film is prepared as the second left lateral electrode layer 63 by magnetron sputtering. The sputtering gas is high-purity argon (purity 99.999%), and the argon flow rate is 15cm 3 / min. The back vacuum of the system during coating is 10 -5 Pa, and the working gas pressure is 0.2 Pa. After sputtering, the stripping process is used to soak the sample in acetone until the metal in the undefined area falls off, and then the sample is placed in isopropanol for 5 minutes to remove the acetone residue.

[0060] S6: Based on S5, 11nm Al was prepared by plasma enhanced atomic layer deposition (PEALD) 2 O 3 As the dielectric layer unit, the process temperature is 250°C, and the carrier gas is N 2 and Ar,N 2 The flow rate was 120 sccm, the Ar flow rate was 75 sccm, the chamber pressure was maintained at 7 hPa, and the oxygen flow rate was 2000 sccm.

[0061] S7: Based on S6, on the surface of the dielectric layer unit, a photolithography process is first used to define the pattern of the second right lateral electrode layer 43, and then a 150nm Ti film is prepared as the second right lateral electrode layer 43 by magnetron sputtering. The sputtering gas is high-purity argon (purity 99.999%), and the argon flow rate is 15cm 3 / min. The back vacuum of the system during coating is 10 -5 Pa, and the working gas pressure is 0.2 Pa. After sputtering, the stripping process is used to soak the sample in acetone until the metal in the undefined area falls off, and then the sample is placed in isopropanol for 5 minutes to remove the acetone residue.

[0062] S8: Based on S7, 11nm Al was prepared by plasma enhanced atomic layer deposition (PEALD) 2 O 3 As the dielectric layer unit, the process temperature is 250°C, and the carrier gas is N 2 and Ar,N 2 The flow rate was 120 sccm, the Ar flow rate was 75 sccm, the chamber pressure was maintained at 7 hPa, and the oxygen flow rate was 2000 sccm.

[0063] S9: Based on S8, on the surface of the dielectric layer unit, a photolithography process is first used to define the pattern of the first left lateral electrode layer 62, and then a 150nm Ti film is prepared as the first left lateral electrode layer 62 by magnetron sputtering. The sputtering gas is high-purity argon (purity 99.999%), and the argon flow rate is 15cm 3 / min. The back vacuum of the system during coating is 10 -5 Pa, and the working gas pressure is 0.2 Pa. After sputtering, the stripping process is used to soak the sample in acetone until the metal in the undefined area falls off, and then the sample is placed in isopropanol for 5 minutes to remove the acetone residue.

[0064] S10: Based on S9, 11nm Al was prepared by plasma enhanced atomic layer deposition (PEALD) 2 O 3 As the dielectric layer unit, the process temperature is 250°C, and the carrier gas is N 2 and Ar,N 2 The flow rate was 120 sccm, the Ar flow rate was 75 sccm, the chamber pressure was maintained at 7 hPa, and the oxygen flow rate was 2000 sccm.

[0065] S11: Based on S10, on the surface of the dielectric layer unit, a photolithography process is first used to define the pattern of the first right lateral electrode layer 42, and then a 150nm Ti film is prepared as the first right lateral electrode layer 42 by magnetron sputtering. The sputtering gas is high-purity argon (purity 99.999%), and the argon flow rate is 15cm 3 / min. The back vacuum of the system during coating is 10 -5 Pa, and the working gas pressure is 0.2 Pa. After sputtering, the stripping process is used to soak the sample in acetone until the metal in the undefined area falls off, and then the sample is placed in isopropanol for 5 minutes to remove the acetone residue.

[0066] S12: Based on S11, photolithography and etching processes are used to etch out the shapes of the right longitudinal metal layer 41 and the left longitudinal metal layer 61. Finally, metal Al is filled in the hole by electroplating to a height of 100 μm to prepare the right longitudinal metal layer 41 and the left longitudinal metal layer 61. At this point, the process flow ends.

[0067] In another embodiment of the present invention, the material of the right longitudinal metal layer 41 is aluminum (Al) with a thickness of 100 μm. The material of the first right lateral electrode layer 42, the second right lateral electrode layer 43, and the third right lateral electrode layer 44 is tantalum nitride (TaN) with a thickness of 150 nm. The material of the left longitudinal metal layer 61 is aluminum (Al) with a thickness of 100 μm. The material of the first left lateral electrode layer 62 and the second left lateral electrode layer 63 is tantalum nitride (TaN) with a thickness of 150 nm. The material of the substrate layer 1 is silicon, and the thickness after thinning is 98 μm. The material of the epitaxial layer 2 is a multi-component compound composed of gallium nitride and aluminum gallium nitrogen, with a thickness of 2 μm. The material of the dielectric layer 5 is hafnium oxide (HfO 2 ), with a total thickness of 60 μm. The preparation method thereof comprises the following steps:

[0068] S1: First, the thinned bonded wafer is cleaned in a wet process module with a dilute HCl solution (volume ratio 1:10) to remove possible contamination on the wafer. 2 Plasma sweep cleaning modifies the wafer surface and increases metal adhesion.

[0069] S2: Based on S1, a back through hole etching process is performed, and an inductively coupled plasma (ICP) etching method is used to etch the substrate layer 1 and the epitaxial layer 2. The etching depth penetrates the substrate layer 1 and the epitaxial layer 2 until it contacts the front metal layer 7.

[0070] S3: Based on S2, on the front metal layer 7, a photolithography process is first used to define the pattern of the third right lateral electrode layer 44, and then a 150nm TaN film is prepared as the third right lateral electrode layer 44 by magnetron sputtering. The sputtering gas is Ar-N 2 Mixed gas, Ar partial pressure is 3.4×10 -1 Pa,N 2 The partial pressure is 0.2×10 -1 Pa. The back vacuum of the system during coating is 6×10 -4 Pa, and the working gas pressure is 0.4 Pa. After sputtering, the stripping process is used to soak the sample in acetone until the metal in the undefined area falls off, and then the sample is placed in isopropanol for 5 minutes to remove the acetone residue.

[0071] S4: Based on S3, 15nm HfO was prepared by plasma enhanced atomic layer deposition (PEALD) 2 As the dielectric layer unit, the process temperature is 300 ° C, tetrakis (ethylmethylamino) hafnium (TEMAHf) and deionized water (H 2 O) as the precursor, and high-purity nitrogen (99.999%) as the protection and cleaning gas (the volume flow rate was set to 200cm 3 / min), and the reaction chamber pressure was set to 1000 Pa. In each ALD cycle, TEMAHf and H 2 The carrier gas volume flow rate of O was 120 cm 3 / min and 150cm 3 / min, the pulse times are 1.5s and 0.3s respectively, and the purge time is 4.0s.

[0072] S5: Based on S4, on the surface of the dielectric layer unit, a photolithography process is first used to define the pattern of the second left lateral electrode layer 63, and then a 150nm TaN film is prepared as the second left lateral electrode layer 63 by magnetron sputtering. The sputtering gas is Ar-N 2 Mixed gas, Ar partial pressure is 3.4×10 -1 Pa,N 2 The partial pressure is 0.2×10 -1 Pa. The back vacuum of the system during coating is 6×10 -4 Pa, and the working gas pressure is 0.4 Pa. After sputtering, the stripping process is used to soak the sample in acetone until the metal in the undefined area falls off, and then the sample is placed in isopropanol for 5 minutes to remove the acetone residue.

[0073] S6: Based on S5, 15nm HfO was prepared by plasma enhanced atomic layer deposition (PEALD) 2 As the dielectric layer unit, the process temperature is 300 ° C, tetrakis (ethylmethylamino) hafnium (TEMAHf) and deionized water (H 2 O) as the precursor, and high-purity nitrogen (99.999%) as the protection and cleaning gas (the volume flow rate was set to 200cm 3 / min), and the reaction chamber pressure was set to 1000 Pa. In each ALD cycle, TEMAHf and H 2 The carrier gas volume flow rate of O was 120 cm 3 / min and 150cm 3 / min, the pulse times are 1.5s and 0.3s respectively, and the purge time is 4.0s.

[0074] S7: Based on S6, on the surface of the dielectric layer unit, a photolithography process is first used to define the pattern of the second right lateral electrode layer 43, and then a 150nm TaN film is prepared as the second right lateral electrode layer 43 by magnetron sputtering. The sputtering gas is Ar-N 2 Mixed gas, Ar partial pressure is 3.4×10 -1 Pa,N 2 The partial pressure is 0.2×10 -1 Pa. The back vacuum of the system during coating is 6×10 -4Pa, and the working gas pressure is 0.4 Pa. After sputtering, the stripping process is used to soak the sample in acetone until the metal in the undefined area falls off, and then the sample is placed in isopropanol for 5 minutes to remove the acetone residue.

[0075] S8: Based on S7, 15nm HfO was prepared by plasma enhanced atomic layer deposition (PEALD) 2 As the dielectric layer unit, the process temperature is 300 ° C, tetrakis (ethylmethylamino) hafnium (TEMAHf) and deionized water (H 2 O) as the precursor, and high-purity nitrogen (99.999%) as the protection and cleaning gas (the volume flow rate was set to 200cm 3 / min), and the reaction chamber pressure was set to 1000 Pa. In each ALD cycle, TEMAHf and H 2 The carrier gas volume flow rate of O was 120 cm 3 / min and 150cm 3 / min, the pulse times are 1.5s and 0.3s respectively, and the purge time is 4.0s.

[0076] S9: Based on S8, on the surface of the dielectric layer unit, a photolithography process is first used to define the pattern of the first left lateral electrode layer 62, and then a 150nm TaN film is prepared as the first left lateral electrode layer 62 by magnetron sputtering. The sputtering gas is Ar-N 2 Mixed gas, Ar partial pressure is 3.4×10 -1 Pa,N 2 The partial pressure is 0.2×10 -1 Pa. The back vacuum of the system during coating is 6×10 -4 Pa, and the working gas pressure is 0.4 Pa. After sputtering, the stripping process is used to soak the sample in acetone until the metal in the undefined area falls off, and then the sample is placed in isopropanol for 5 minutes to remove the acetone residue.

[0077] S10: Based on S9, 15nm HfO was prepared by plasma enhanced atomic layer deposition (PEALD) 2 As the dielectric layer unit, the process temperature is 300 ° C, tetrakis (ethylmethylamino) hafnium (TEMAHf) and deionized water (H 2 O) as the precursor, and high-purity nitrogen (99.999%) as the protection and cleaning gas (the volume flow rate was set to 200cm 3 / min), and the reaction chamber pressure was set to 1000 Pa. In each ALD cycle, TEMAHf and H 2 The carrier gas volume flow rate of O was 120 cm 3 / min and 150cm 3 / min, the pulse times are 1.5s and 0.3s respectively, and the purge time is 4.0s.

[0078] S11: Based on S10, on the surface of the dielectric layer unit, a photolithography process is first used to define the pattern of the first right lateral electrode layer 42, and then a 150nm TaN film is prepared as the first left lateral electrode layer 62 by magnetron sputtering. The sputtering gas is Ar-N 2 Mixed gas, Ar partial pressure is 3.4×10 -1 Pa,N 2 The partial pressure is 0.2×10 -1 Pa. The back vacuum of the system during coating is 6×10 -4 Pa, and the working gas pressure is 0.4 Pa. After sputtering, the stripping process is used to soak the sample in acetone until the metal in the undefined area falls off, and then the sample is placed in isopropanol for 5 minutes to remove the acetone residue.

[0079] S12: Based on S11, photolithography and etching processes are used to etch out the shapes of the right longitudinal metal layer 41 and the left longitudinal metal layer 61. Finally, metal Al is filled in the hole by electroplating to a height of 100 μm to prepare the right longitudinal metal layer 41 and the left longitudinal metal layer 61. At this point, the process flow ends.

[0080] It is easy to understand that in the two preparation process embodiments of the present invention, each right lateral electrode layer and left lateral electrode layer 44 cannot cover the entire dielectric layer unit, but is prepared on the right part and the left part of the dielectric layer unit respectively.

[0081] It can be seen that the back via capacitor structure provided by the present invention is compatible with the back process of chip manufacturing, can effectively optimize the manufacturing process, improve production efficiency, ensure device performance and consistency, and at the same time save chip area, improve integration and reduce costs.

[0082] The above contents are further detailed descriptions of the invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.

Claims

1. A semiconductor RF chip back-through hole large-capacitance capacitor structure, It is characterized in that The capacitor structure comprises, from bottom to top, a substrate layer (1) and an epitaxial layer (2); A plurality of back through holes (3) penetrating the substrate layer (1) and the epitaxial layer (2) are provided between the substrate layer (1) and the epitaxial layer (2), and a back through hole capacitor structure is provided inside the back through hole (3); The back through-hole capacitor structure comprises a right electrode (4), a dielectric layer (5), a left electrode (6) and a front metal layer (7); The right electrode (4) and the left electrode (6) are both multi-layer structures, and the two intersect each other to form interdigitated electrodes; The dielectric layer (5) is filled between the right electrode (4) and the left electrode (6) that cross each other, and the dielectric layer (5) is filled between the electrodes; the right electrode (4) is connected to the front metal layer (7) located on the front of the chip, and the left electrode (6) is grounded.

2. A semiconductor radio frequency chip back side through hole large-capacitance capacitor structure according to claim 1, It is characterized in that The right electrode (4) is a multi-layer structure, comprising a right longitudinal metal layer (41) arranged on the side wall of the back through hole (3) and a plurality of right transverse electrode layers connected to the left side of the right longitudinal metal layer (41); the top of the right longitudinal metal layer (41) and / or the top of the uppermost right transverse electrode layer are connected to the front metal layer (7); The left electrode (6) is a multi-layer structure, comprising a left longitudinal metal layer (61) arranged on the side wall of the back through hole (3) and a plurality of left transverse electrode layers connected to the right side of the left longitudinal metal layer (61), and the left longitudinal metal layer (61) and / or the left transverse electrode layer are grounded.

3. A semiconductor radio frequency chip back side through hole large capacity capacitor structure according to claim 2, It is characterized in that The difference in number between the left lateral electrode layer and the right lateral electrode layer is 1.

4. The semiconductor radio frequency chip back side through hole large-capacitance capacitor structure according to claim 2, It is characterized in that The material of the right longitudinal metal layer (41) and the left longitudinal metal layer (61) is any one or more of titanium nitride, tantalum nitride, titanium, tungsten, aluminum, and gold, and the height is 50-200 μm; the material of the right transverse electrode layer and the left transverse electrode layer is any one or more of titanium nitride, tantalum nitride, titanium, tungsten, aluminum, and gold, and the thickness is 100-1000nm, the longitudinal distance between adjacent right transverse electrode layers and left transverse electrode layers is 10nm-1000nm, and the length of the transverse intersection part is 30-40 μm.

5. The semiconductor radio frequency chip back side through hole large-capacitance capacitor structure according to claim 2, It is characterized in that The number of the right lateral electrode layers is three, and the number of the left lateral electrode layers is two.

6. The semiconductor radio frequency chip back side through hole large capacity capacitor structure according to claim 2, It is characterized in that The material of the substrate layer (1) is one of silicon carbide, silicon, sapphire, and gallium nitride, and the thickness after thinning is 50-200 μm; the material of the epitaxial layer (2) is a group III nitride, and the thickness is 1-5 μm, and the group III nitride is a multi-component compound composed of one or two or more of gallium nitride, aluminum nitride, and indium nitride; the material of the dielectric layer (5) is any one or more of silicon dioxide, aluminum oxide, hafnium oxide, tantalum pentoxide, and zirconium oxide.

7. The method for preparing a semiconductor radio frequency chip back side through hole large-capacitance capacitor structure according to any one of claims 1 to 6, comprising the following steps: S1: using a back through hole etching process to etch the substrate layer (1) and the epitaxial layer (2), wherein the etching depth penetrates the substrate layer (1) and the epitaxial layer (2) until they contact the front metal layer (7), thereby forming a back through hole (3); S2: In the back through hole (3), a right lateral electrode layer, a dielectric layer unit, a left lateral electrode layer, a dielectric layer unit, a right lateral electrode layer, a dielectric layer unit, ..., a dielectric layer unit, a right lateral electrode layer or a left lateral electrode layer are sequentially prepared on the surface of the front metal layer (7), holes are etched again and filled with metal, each right lateral electrode layer is connected to obtain a right electrode (4), each left lateral electrode layer is connected to obtain a left electrode (6), each right lateral electrode layer and each left lateral electrode layer form an interdigitated electrode structure, and each dielectric layer unit is filled between the electrodes to form a dielectric layer (5).

8. The semiconductor radio frequency chip back side through hole large capacity capacitor structure according to claim 7, It is characterized in that The right side lateral electrode layer, dielectric layer unit, left side lateral electrode layer, dielectric layer unit, right side lateral electrode layer, dielectric layer unit, ..., dielectric layer unit, right side lateral electrode layer or left side lateral electrode layer are sequentially prepared on the surface of the front metal layer (7), and the implementation method is as follows: S21: preparing a right lateral electrode layer on a portion of the surface of the front metal layer (7); S22: preparing a dielectric layer unit on another part of the surface of the front metal layer (7) and on the surface of the right lateral electrode layer obtained in S21; S23: preparing a left lateral electrode layer on a part of the surface of the dielectric layer unit obtained in S22; S24: preparing a dielectric layer unit on another part of the surface of the dielectric layer unit obtained in S22 and on the surface of the left lateral electrode layer obtained in S23; S25: preparing a right lateral electrode layer on a portion of the surface of the dielectric layer unit obtained in S24; S26: preparing a dielectric layer unit on another part of the surface of the dielectric layer unit obtained in S24 and on the surface of the right lateral electrode layer obtained in S25; S27: Repeat S23 to S26, and end with preparing the left lateral electrode layer or preparing the right lateral electrode layer.

9. The semiconductor radio frequency chip back side through hole large capacity capacitor structure according to claim 7, It is characterized in that The holes are etched again and filled with metal, and the right side lateral electrode layers are connected to obtain the right side electrode (4), and the left side lateral electrode layers are connected to obtain the left side electrode (6), and the implementation method is as follows: Photolithography and etching processes are used to etch the shape of connection holes on the right side of each right lateral electrode layer and on the left side of each left lateral electrode layer, and then metal is filled in the holes by electroplating to prepare a right longitudinal metal layer (41) and a left longitudinal metal layer (61).

10. A semiconductor radio frequency chip back side through hole large-capacitance capacitor structure according to claim 7, 8 or 9, It is characterized in that The right lateral electrode layer and the left lateral electrode layer are both prepared by photolithography-stripping process, and the dielectric layer units are both prepared by plasma enhanced chemical vapor deposition method or plasma enhanced atomic layer deposition method.