Spherical silver powder, method for producing spherical silver powder, device for producing spherical silver powder, and conductive paste

By controlling the reduction and precipitation process of silver powder in the flow path, spherical silver powder with pores is formed, which solves the problem of insufficient low-temperature sintering and printing properties of silver powder in the prior art, and realizes excellent performance of conductive pastes, and is suitable for solar cells. and electronic components.

CN119095682APending Publication Date: 2024-12-06DOWA ELECTRONICS MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036045.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, silver powder is insufficient in low-temperature sintering and printing properties when sintering the conductive paste, and it is difficult to maintain excellent performance at 690 to 740°C.

Method used

By adding complexing agent and formalin to the flow path, the reduction and precipitation process of silver powder is controlled to form spherical silver powder with pores to ensure its dispersion and low-temperature sintering. A combination of laser diffraction method and BET single-point method is used to use the method of combining laser diffraction method and BET single-point method to control particle size and porosity.

Benefits of technology

The spherical silver powder with excellent printing and sintering properties at low temperatures is achieved, and is suitable for conductive pastes, which improves the performance of conductive pastes, especially in electrode applications of solar cells and electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095682A_ABST
    Figure CN119095682A_ABST
Patent Text Reader

Abstract

Provided is a spherical silver powder which, when used in a conductive paste or the like, can impart excellent printability and low-temperature sinterability. A spherical silver powder which has a ratio of a volume-based cumulative 50% diameter (D50) to a BET diameter (DBET) of 0.9-1.2 (inclusive) as determined by a laser diffraction method, and which has pores inside particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to spherical silver powder, a method for producing spherical silver powder, a spherical silver powder producing device and a conductive paste. Background Art

[0002] As a conductive paste used in the internal electrodes of multilayer capacitors, the conductor patterns of circuit boards, and various electronic components including solar cells, a conductive paste produced by adding silver powder and glass powder to an organic binder and kneading them is used. The silver powder for the conductive paste is required to have a moderately small particle size, uniform particle size, and high dispersibility in order to cope with the miniaturization of electronic components, the high density and thinning of conductor patterns, etc.

[0003] As a method for manufacturing silver powder for such a conductive paste, Patent Document 1 proposes a method for manufacturing microparticle silver powder, which is characterized in that an aqueous silver nitrate solution and an ammonia solution are mixed and reacted to obtain an aqueous silver ammonia complex solution, the aqueous solution is flowed into a certain flow path (first flow path), a second flow path is provided to merge with the first flow path in the middle, an organic reducing agent is flowed through the second flow path, and contact mixing is performed at the confluence point of the first flow path and the second flow path.

[0004] In addition, Patent Document 2 proposes a method for producing silver powder, characterized in that a silver solution containing a silver complex and a reducing agent solution are respectively quantitatively and continuously supplied into a flow path, and the silver complex is quantitatively and continuously reduced in a reaction solution formed by mixing the silver solution and the reducing agent solution in the flow path to obtain silver powder, wherein, when the silver solution and the reducing agent solution are mixed, the ratio of the flow rate of the reducing agent solution supplied from a coaxial pipe arranged in the pipe in the same direction as the supply direction of the silver solution to the flow rate of the silver solution in the pipe forming the flow path is set to be 1.5 or more.

[0005] In addition, Patent Document 3 proposes a method for producing spherical silver powder, which comprises mixing an aqueous silver nitrate solution and an ammonia solution and reacting them to obtain an aqueous silver ammonia complex solution, mixing the aqueous silver ammonia complex solution with an aqueous reducing agent solution in the presence of particles serving as seeds and an imide compound, and reducing and precipitating silver particles to produce a spherical silver powder, wherein the aqueous silver ammonia complex solution and the aqueous reducing agent solution are caused to flow into respective flow paths that merge at a confluence point, and at the confluence point, the aqueous silver ammonia complex solution and the aqueous reducing agent solution are contacted and mixed.

[0006] In addition, Patent Document 4 proposes a method for producing silver particles in which ammonia and a reducing agent are added to a silver ion solution to reduce and precipitate silver particles, and a reducing agent is added within 20 seconds after the addition of ammonia to precipitate fine silver particles. However, the silver ion solution to which ammonia is added and the reducing solution are mixed on the outside of a pipeline, and specifically disclosed is only an example of using a hydroquinone solution as a reducing agent.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2005-48236

[0010] Patent Document 2: Japanese Patent Application Publication No. 2015-45064

[0011] Patent Document 3: Japanese Patent Application Publication No. 2010-70793

[0012] Patent Document 4: Japanese Patent Application Publication No. 2008-255378 Summary of the invention

[0013] Problem that the invention aims to solve

[0014] When forming internal electrodes, conductor patterns, etc. using a conductive paste containing silver powder, the silver powder is required to have good printability when made into a conductive paste and to be able to be sintered at low temperatures (690 to 740° C.) and have excellent low-temperature sinterability in order to suppress the degradation of peripheral components caused by heating during the firing of the conductive paste. The silver powder obtained by the production methods of Patent Documents 1 to 4 has room for improvement in these aspects.

[0015] An object of the present invention is to provide spherical silver powder capable of providing a conductive paste having excellent printability and low-temperature sintering properties, and a method and apparatus for producing the same.

[0016] Solutions for solving problems

[0017] The inventors of the present invention have conducted intensive research to solve the above problems and have found that in order to simultaneously obtain excellent low-temperature sintering properties and printability, pores exist in each particle of spherical silver powder, and the cumulative 50% diameter D based on volume based on laser diffraction method is 50 Relative to BET diameter D BET The ratio (D 50 / D BET ) is advantageous to control the dispersibility of such spherical silver powder, thereby completing the present invention. For example, the silver powder obtained by the production methods of the above-mentioned Patent Documents 1 to 4 does not have pores in each particle.

[0018] Here, the BET diameter DBET The specific surface area SSA (unit: m) is determined by the BET single point method. 2 / g) and true density (in g / cm 3 ) is calculated by the following formula.

[0019] D BET =6 / (SSA) / true density

[0020] D 50 , D BET , SSA and true density are values ​​measured by the methods described in the Examples.

[0021] In silver powder, individual particles are usually not completely separated, and sometimes a plurality of particles are aggregated. The particle size measurement based on the laser diffraction method calculates the particle size based on the diffraction pattern of the particles, and thus measures the particle size of the aggregated particles. On the other hand, the BET single point method is a method of measuring the specific surface area using the amount of gas adsorbed on the particles. The BET diameter converted from the specific surface area represents the particle size (particle diameter) of the particles when the measured particles are assumed to be true spheres. Ratio (D 50 / D BET ) close to 1 means that there is little aggregation and the state is close to monodisperse.

[0022] Here, the surface of the silver powder having pores in the particles tends to have unevenness, and it is difficult to compare (D 50 / D BET ) is controlled to a value close to 1.

[0023] The present inventors have found that by allowing a silver-containing solution to flow in a flow path, adding a complexing agent at a complexing agent adding position in the middle of the flow path, adding formalin at a formalin adding position further downstream than the complexing agent adding position, and reducing and precipitating silver powder in the flow path, a particle having pores in the particle and a particle size of (D 50 / D BET ) is 0.9 or more and 1.2 or less, thereby completing the present invention.

[0024] In the manufacturing method of the present invention, a silver-containing solution is made to flow in a flow path, a complexing agent is added to the flow path at a complexing agent adding position in the middle of the flow path, thereby forming a silver complex forming region, and formalin is added to the flow path at a formalin adding position downstream of the complexing agent adding position, thereby forming a reduction precipitation region of silver powder. It is speculated that by continuously forming the silver complex forming region and the reduction precipitation region in this way, and then using formalin as a reducing agent for reduction precipitation, a particle having pores inside and a ratio of (D 50 / D BET ) is 0.9 or more and 1.2 or less and has good dispersibility.

[0025] The gist of the present invention is as follows.

[0026] [1] A spherical silver powder having a cumulative 50% diameter D based on volume by laser diffraction method. 50 Relative to BET diameter D BET The ratio is 0.9 or more and 1.2 or less, and the particles have pores inside.

[0027] [2] The spherical silver powder of [1] above, having a true density of 9.0 g / cm 3 Above and 10.0g / cm 3 the following.

[0028] [3] The spherical silver powder according to [1] or [2], wherein D 50 It is not less than 0.2 μm and not more than 3.5 μm.

[0029] [4] The spherical silver powder according to any one of [1] to [3] above, wherein the BET specific surface area is 0.17 m 2 / g or more and 3.23m 2 / g or less.

[0030] [5] The spherical silver powder according to any one of [1] to [4] above, wherein the value obtained by subtracting the contents of carbon, nitrogen and oxygen from the ignition loss is less than 0.10 mass %.

[0031] [6] The spherical silver powder according to any one of [1] to [5] above, wherein the ratio of the oxygen content to the carbon content is 1.5 or more.

[0032] [7] A method for producing spherical silver powder, wherein a silver-containing solution is caused to flow in a flow path, a complexing agent is added to the flow path at a complexing agent addition position in the middle of the flow path, and formalin is added to the flow path at a formalin addition position downstream of the complexing agent addition position, so that the silver powder is reduced and precipitated in the flow path.

[0033] [8] The method for producing spherical silver powder according to [7] above, wherein the time required for the silver-containing solution to flow from the complexing agent addition position to the formalin addition position is 0.1 seconds or more and within 10 seconds.

[0034] [9] The method for producing spherical silver powder as described in [7] or [8] above, wherein a surface treatment agent is added to the flow path between the complexing agent addition position and the formalin addition position, or downstream of the formalin addition position.

[0035]

[10] A method for producing spherical silver powder as described in any one of [7] to [9] above, wherein the formalin is added from multiple directions at the formalin addition position, and the multiple directions each form an angle of greater than 75 degrees and less than 105 degrees relative to the flow path.

[0036]

[11] A device for producing spherical silver powder, which is a device for producing spherical silver powder by adding a complexing agent and formalin to a silver-containing solution to reduce and precipitate silver powder, and which comprises: a tube forming a flow path for the silver-containing solution; a complexing agent adding section connected to the tube; and a formalin adding section connected to the tube on the downstream side of the complexing agent adding section.

[0037]

[12] A conductive paste comprising the spherical silver powder according to any one of [1] to [6] above, an organic binder, and a solvent.

[0038]

[13] The conductive paste according to

[12] , which is used for forming an electrode of a solar cell.

[0039] Effects of the Invention

[0040] According to the present invention, there are provided spherical silver powder which can provide excellent printability and low-temperature sintering properties when used in a conductive paste or the like, and a method and apparatus for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is a perspective view of the appearance of an example of the silver powder production device of the present invention.

[0042] Figure 2 This is a perspective view of the appearance of another example of the silver powder production device of the present invention.

[0043] Figure 3A This is a SEM photograph (10,000 times) of the silver powder of Example 1 (before vacuum drying).

[0044] Figure 3B This is a SEM photograph (10,000 times) of the silver powder of Example 1 (after vacuum drying and crushing treatment).

[0045] Figure 3C This is a FE-SEM photograph (20,000 times) of a cross section of the silver powder of Example 1 (after vacuum drying and crushing treatment).

[0046] Figure 4A This is a SEM photograph (10,000 times) of the silver powder of Example 2 (before vacuum drying).

[0047] Figure 4B This is a SEM photograph (10,000 times) of the silver powder of Example 2 (after vacuum drying and crushing treatment).

[0048] Figure 4C This is a FE-SEM photograph (20,000 times) of a cross section of the silver powder of Example 2 (after vacuum drying and crushing treatment).

[0049] Figure 5A This is a SEM photograph (10,000 times) of the silver powder of Example 3 (before vacuum drying).

[0050] Figure 5B This is a SEM photograph (10,000 times) of the silver powder of Example 3 (after vacuum drying and crushing treatment).

[0051] Figure 5C This is a FE-SEM photograph (20,000 times) of a cross section of the silver powder of Example 3 (after vacuum drying and crushing treatment).

[0052] Fig. 6A This is a SEM photograph (10,000 times) of the silver powder of Example 4 (before vacuum drying).

[0053] Figure 6B This is a SEM photograph (10,000 times) of the silver powder of Example 4 (after vacuum drying and crushing treatment).

[0054] Figure 6C This is a FE-SEM photograph (20,000 times) of a cross section of the silver powder of Example 4 (after vacuum drying and crushing treatment).

[0055] Fig. 7A This is a SEM photograph (10,000 times) of the silver powder of Example 5 (before vacuum drying).

[0056] Figure 7B This is a SEM photograph (10,000 times) of the silver powder of Example 5 (after vacuum drying and crushing treatment).

[0057] Figure 7C This is a FE-SEM photograph (20,000 times) of a cross section of the silver powder of Example 5 (after vacuum drying and crushing treatment).

[0058] Fig. 8A This is a SEM photograph (10,000 times) of the silver powder of Example 6 (before vacuum drying).

[0059] Figure 8B This is a SEM photograph (10,000 times) of the silver powder of Example 6 (after vacuum drying and crushing treatment).

[0060] Figure 8C This is a FE-SEM photograph (20,000 times) of a cross section of the silver powder of Example 6 (after vacuum drying and crushing treatment).

[0061] Fig.9AThis is a SEM photograph (10,000 times) of the silver powder of Example 7 (before vacuum drying).

[0062] Fig. 9B This is a SEM photograph (10,000 times) of the silver powder of Example 7 (after vacuum drying and crushing treatment).

[0063] Fig. 9C This is a FE-SEM photograph (20,000 times) of a cross section of the silver powder of Example 7 (after vacuum drying and crushing treatment).

[0064] Fig. 10A This is a SEM photograph (10,000 times) of the silver powder of Comparative Example 1 (before vacuum drying).

[0065] Fig. 10B This is a SEM photograph (10,000 times) of the silver powder of Comparative Example 1 (after vacuum drying and crushing treatment).

[0066] Fig. 10C This is a FE-SEM photograph (20,000 times) of a cross section of the silver powder of Comparative Example 1 (after vacuum drying and crushing treatment).

[0067] Fig.11A This is a SEM photograph (10,000 times) of the silver powder of Comparative Example 2 (before vacuum drying).

[0068] Fig. 11B This is a SEM photograph (10,000 times) of the silver powder of Comparative Example 2 (after vacuum drying and crushing treatment).

[0069] Fig. 11C This is a FE-SEM photograph (20,000 times) of a cross section of the silver powder of Comparative Example 2 (after vacuum drying and crushing treatment).

[0070] Fig.12 This is a graph showing the heat shrinkage rates of Example 1 and Comparative Examples 1 and 2.

[0071] Fig.13 The diagram shows the shape of an electrode pattern used for EL evaluation of fine line printability.

[0072] Fig.14 These are photographs showing the EL evaluation results of the conductive paste using the silver powder of Example 1.

[0073] Fig.15 These are photographs showing the EL evaluation results of the conductive paste using the silver powder of Example 2.

[0074] Fig.16 These are photographs showing the EL evaluation results of the conductive paste using the silver powder of Example 3.

[0075] Fig.17These are photographs showing the EL evaluation results of the conductive paste using the silver powder of Example 4.

[0076] Fig.18 These are photographs showing the EL evaluation results of the conductive paste using the silver powder of Example 5.

[0077] Fig.19 The photographs show the EL evaluation results of the conductive paste using the silver powder of Example 6.

[0078] Fig. 20 These are photographs showing the EL evaluation results of the conductive paste using the silver powder of Comparative Example 1.

[0079] Fig.21 These are photographs showing the EL evaluation results of the conductive paste using the silver powder of Comparative Example 2. DETAILED DESCRIPTION

[0080] <Spherical silver powder>

[0081] The cumulative 50% diameter D of the spherical silver powder of the present invention based on the volume basis by the laser diffraction method is 50 Relative to BET diameter D BET The ratio (D 50 / D BET ) is 0.9 or more and 1.2 or less, and the particles have pores inside.

[0082] Here, the spherical shape includes a substantially spherical shape, and is a shape having an average aspect ratio (average ratio of major diameter / minor diameter) of 1.5 or less. The pores inside the particles are closed pores that are not connected to the outside.

[0083] The spherical silver powder has pores inside the particles. The presence of pores inside the particles can be confirmed by observing the cross section of the particles using a field emission scanning electron microscope (FE-SEM).

[0084] In terms of obtaining excellent dispersibility, the ratio (D 50 / D BET ) is preferably 1.20 or less, more preferably 1.15 or less, and still more preferably 1.04 or less. This ratio is usually 0.90 or more, more preferably 0.95 or more.

[0085] From the viewpoint of ease of paste handling when preparing a conductive paste, D 50 The diameter of D is preferably 0.2 μm or more, and more preferably 0.5 μm or more. In addition, from the viewpoints of obtaining appropriate particle activity, low temperature sintering of a wiring pattern formed using a conductive paste, and easy handling of high density, D 50 It is preferably 3.5 μm or less, and more preferably 3.0 μm or less.

[0086] The cumulative 10% diameter D of the spherical silver powder of the present invention based on volume 10 It is preferably 0.1 μm or more and preferably 2.0 μm or less.

[0087] The cumulative 90% diameter D of the spherical silver powder of the present invention based on volume 90 It is preferably 0.5 μm or more and preferably 7.0 μm or less.

[0088] D 10 and D 90 These are values ​​measured by the method described in Examples.

[0089] The BET specific surface area (SSA) is preferably 0.17 m / s from the viewpoints of obtaining appropriate particle activity, being advantageous in low temperature sintering of a wiring pattern formed using a conductive paste, and being easy to cope with high density. 2 / g or more, more preferably 0.20m 2 / g or more. In addition, from the viewpoint of ease of paste handling when the conductive paste is prepared, 3.23 m 2 / g or less, more preferably 2.40m 2 / g or less.

[0090] The true density of silver is 10.49 g / cm 3 However, the spherical silver powder of the present invention has pores inside the particles, and the true density can be 9.0 g / cm 3 Above and 10.0g / cm 3 From the viewpoint of easily coping with the high density of the wiring pattern, the true density is preferably 9.4 g / cm 3 In addition, from the viewpoint of low temperature sintering properties, the true density is preferably 9.9 g / cm 3 the following.

[0091] D BET The specific surface area (m 2 / g) and true density (g / cm 3 ), and the BET diameter (μm) was calculated by the following formula.

[0092] BET diameter = 6 / specific surface area / true density

[0093] D BET The diameter is preferably 0.18 μm or more, more preferably 0.45 μm or more, and is preferably 3.90 μm or less, more preferably 3.20 μm or less.

[0094] From the viewpoint of being easy to handle high-precision patterns, the tap density of the spherical silver powder of the present invention is preferably 2.5 g / cm 3More preferably 4.5 g / cm 3 On the other hand, if the true density of silver and the closest packing of uniform spherical powder are taken into consideration, the upper limit of the tap density is 7.8 g / cm 3 .

[0095] The ignition loss of the spherical silver powder of the present invention is preferably 2.65 mass % or less, and more preferably 1.62 mass % or less. Here, the ignition loss is measured under the same conditions as described in the Examples.

[0096] In addition, the carbon content of the spherical silver powder of the present invention is preferably 1.00 mass% or less, more preferably 0.50 mass% or less, the nitrogen content is preferably 0.15 mass% or less, more preferably 0.12 mass% or less, and the oxygen content is preferably 1.50 mass% or less, more preferably 1.00 mass% or less. From the viewpoint of low temperature sintering performance, the oxygen content is preferably 0.20 mass% or more, more preferably 0.30 mass% or more. The contents of carbon, nitrogen and oxygen are values ​​measured by the method of the examples.

[0097] From the viewpoint of low temperature sintering properties, the ratio of oxygen content to carbon content (O / C) is preferably 1.5 or more, preferably 3.5 or less, and more preferably 1.7 or more and 3.0 or less. In particular, when the spherical silver powder of the present invention is used in a conductive paste containing glass powder, the oxygen contained in the silver particles contributes to the generation of heat, thereby promoting the softening of the glass, which is advantageous in low temperature sintering.

[0098] Furthermore, the value obtained by subtracting the total content of carbon, nitrogen and oxygen from the ignition loss of the spherical silver powder of the present invention is preferably less than 0.10 mass %, more preferably 0.09 mass % or less. Within this range, the problem of thermal expansion when forming components such as electrodes using the spherical silver powder of the present invention can be easily avoided.

[0099] <Method for producing spherical silver powder>

[0100] The method for producing spherical silver powder of the present invention comprises: making a silver-containing solution flow in a flow path, adding a complexing agent at a complexing agent adding position in the middle of the flow path, adding formalin at a formalin adding position downstream of the complexing agent adding position, and reducing and precipitating the silver powder in the flow path. In the production method of the present invention, by continuously supplying the silver-containing solution, the complexing agent, and formalin and quantitatively mixing them, the formation rate of the silver complex and the reduction and precipitation rate of the silver powder can be kept constant, thereby quantitatively and continuously obtaining a predetermined spherical silver powder.

[0101] The silver-containing solution is a solution that reacts with a complexing agent to form a silver complex, and a solution containing a silver salt can be used. For example, aqueous solutions of silver nitrate, silver chloride, silver formate, silver oxalate, silver sulfate, etc. can be enumerated, and from the viewpoints of being easy to obtain, preferably an aqueous silver nitrate solution.

[0102] From an economic point of view, the silver concentration of the silver-containing solution is preferably 0.01 mol / L or more, more preferably 0.05 mol / L or more. From the viewpoint of ensuring the interparticle distance of the particles after reduction precipitation and inhibiting aggregation, the silver concentration is preferably 0.5 mol / L or less, more preferably 0.3 mol / L or less.

[0103] From the perspective of productivity and the formation of monodisperse particles, the flow rate of the silver-containing solution is preferably 0.45 m / sec or more, more preferably 0.65 m / sec or more. In addition, from the perspective of suppressing aggregation and forming monodisperse particles, it is preferably 3.20 m / sec or less, more preferably 2.70 m / sec or less.

[0104] In the production method of the present invention, a silver-containing solution is made to flow in a flow channel, and a complexing agent is added to a complexing agent adding position in the middle of the flow channel, thereby forming a silver complex.

[0105] Examples of the complexing agent include ammonia, ammonium salts, citric acid, acetic acid, and the like, and ammonia is preferred. Ammonia may be added in the form of aqueous ammonia.

[0106] For example, when adding ammonia water as a complexing agent, a silver ammonia complex is formed. The silver ammonia complex can be easily reduced by formalin, so it is preferred. The amount of ammonia water added is preferably an amount in which substantially no silver ions that do not form a silver ammonia complex remain in the liquid, and relative to 1 mole of silver, the amount of ammonia can be set to be more than 2.6 moles and less than 11.2 moles, preferably more than 3.1 moles and less than 10.4 moles.

[0107] From an economical viewpoint, the concentration of aqueous ammonia is preferably 3.1 mol / L or more, more preferably 3.7 mol / L, and is preferably 16.2 mol / L or less, more preferably 15.1 mol / L or less.

[0108] The flow rate of the ammonia water is preferably 0.40 m / sec or more, more preferably 0.60 m / sec or more, and is preferably 3.20 m / sec or less, more preferably 2.70 m / sec or less.

[0109] When other complexing agents are used, the above-mentioned concentration and flow rate may also be used.

[0110] In the production method of the present invention, formalin is added to the flow path at a formalin addition position downstream of the complexing agent addition position to reduce and precipitate the silver powder. By using formalin as a reducing agent, silver powder having pores inside the particles can be obtained.

[0111] The concentration of formalin (formaldehyde aqueous solution) is preferably 3.9 mol / L or more, more preferably 4.7 mol / L or more, and is preferably 14.5 mol / L or less, more preferably 12.8 mol / L or less.

[0112] The amount of formalin is preferably an amount that substantially does not generate unreacted silver ions, and the amount of formalin (formaldehyde) can be 3.1 mol to 10.6 mol, preferably 3.7 mol to 9.3 mol, per 1 mol of silver.

[0113] In the manufacture method of the present invention, in order to add formalin when forming silver complex solution, the silver-containing solution flows to the time (elapsed time) required for formalin addition position from the complexing agent addition position and is preferably more than 0.1 second, more preferably more than 0.5 second. In addition, if the reaction other than the complexing agent and the silver ion, the stability of the silver complex becomes high, and reduction reaction is likely to be difficult to carry out, so in order to prevent the reaction other than the complexing agent and the silver ion from starting, the elapsed time is preferably within 10.0 seconds, more preferably below 5.0 seconds. It is believed that if the elapsed time is as long as to exceed 10.0 seconds, the generation status of the by-product during the period from the addition of the complexing agent to the addition of formalin and the reduction reaction changes, and the value obtained by deducting the total of the content of carbon, nitrogen and oxygen by the loss on ignition increases. And then, it is believed that the oxygen content contained in the silver particles is reduced relative to the ratio of carbon content.

[0114] In the manufacturing method of the present invention, a surface treatment agent can be added to the flow path between the complexing agent addition position and the formalin addition position or downstream of the formalin addition position. The addition of the surface treatment agent is advantageous in suppressing the aggregation of the silver powder precipitated by reduction. The addition is preferably performed at a time between the complexing agent addition position and the formalin addition position.

[0115] Examples of the surface treatment agent include fatty acids, fatty acid salts, surfactants, organic metals, chelate forming agents, protective colloids, etc. The surface treatment agent can be used in an amount of 0.03 mass % or more and 1.00 mass % or less relative to the silver in the silver-containing solution. The surface treatment agent can be used in the form of an emulsion, a solution, etc.

[0116] (1) Fatty acids

[0117] Examples of the fatty acid include propionic acid, caprylic acid, lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, acrylic acid, oleic acid, linoleic acid, arachidonic acid, and ricinoleic acid.

[0118] (2) Fatty acid salts

[0119] Examples of the fatty acid salt include metal salts of the fatty acid described in (1) above, and examples of the metal include lithium, sodium, potassium, barium, magnesium, calcium, aluminum, iron, cobalt, manganese, lead, zinc, tin, strontium, zirconium, silver, and copper.

[0120] (3) Surfactants

[0121] Examples of the surfactant include anionic surfactants such as alkylbenzene sulfonates and polyoxyethylene alkyl ether phosphates, cationic surfactants such as aliphatic quaternary ammonium salts, amphoteric surfactants such as imidazoline betaine, and nonionic surfactants such as polyoxyethylene alkyl ethers and polyoxyethylene fatty acid esters.

[0122] (4) Organic metals

[0123] Examples of the organic metal include tributoxyzirconium acetylacetonate, magnesium citrate, diethyl zinc, dibutyl tin oxide, dimethyl zinc, tetra-n-butoxy zirconium, triethyl indium, triethyl gallium, trimethyl indium, trimethyl gallium, monobutyl tin oxide, tetraisocyanate silane, tetramethylsilane, tetramethoxysilane, monomethyl triisocyanate silane, silane coupling agents, titanate-based coupling agents, and aluminum-based coupling agents.

[0124] (5) Chelate Forming Agent

[0125] Examples of the chelate forming agent include imidazole, oxazole, thiazole, selenazole, pyrazole, isoxazole, isothiazole, 1H-1,2,3-triazole, 2H-1,2,3-triazole, 1H-1,2,4-triazole, 4H-1,2,4-triazole, 1,2,3-oxadiazole, 1,2,4-oxadiazole, 1,2,5-oxadiazole, 1,3,4-oxadiazole, 1,2,3-thiadiazole, 1,2,4-thiadiazole, 1,2,5 -thiadiazole, 1,3,4-thiadiazole, 1H-1,2,3,4-tetrazole, 1,2,3,4-oxatriazole, 1,2,3,4-thiatriazole, 2H-1,2,3,4-tetrazole, 1,2,3,5-oxatriazole, 1,2,3,5-thiatriazole, indazole, benzimidazole, benzotriazole, etc., and salts of these chelate formers, polycarboxylic acids represented by dicarboxylic acids such as succinic acid, malonic acid, glutaric acid, and adipic acid, etc.

[0126] (6) Protective colloid

[0127] Examples of the protective colloid include peptides, gelatin, albumin, gum arabic, ovalbumin, gelatin, and glue.

[0128] As the surface treatment agent, from the viewpoint of the ease of modifying the silver particle surface, (1) fatty acids are preferred, and among them, stearic acid is preferred. (1) The fatty acid is preferably in the form of an emulsion, and examples thereof include stearic acid emulsions.

[0129] In the production method of the present invention, from the viewpoint of the reactivity of the reduction reaction, the temperature of the liquid flowing in the flow path is preferably 5°C or higher, more preferably 15°C or higher, and in terms of operation, is preferably 60°C or lower, more preferably 50°C or lower.

[0130] In the production method of the present invention, a mixer may be used to impart a spiral rotation in the axial direction of the flow path to mix the liquids.

[0131] In the manufacturing method of the present invention, spherical silver powder can be obtained by releasing the liquid containing the silver powder precipitated by reduction (hereinafter also referred to as "silver powder containing liquid") to the outside of the flow path and recovering it. From the viewpoint of being able to predict the end of the reduction reaction, the time from the addition of formalin to the release of the silver powder containing liquid to the outside of the flow path is preferably 1 second or more, more preferably 2 seconds or more, and from the viewpoint of suppressing retention in the piping, it is preferably 10 seconds or less, more preferably 5 seconds or less.

[0132] In the manufacturing method of the present invention, since formalin is added to the flow path at the formalin addition position downstream of the complexing agent addition position, a reduction reaction occurs in the flow path to generate silver nuclei, and the particles grow into silver particles in the flow path. When a reduction reaction occurs outside the flow path as in Patent Document 4, the surface unevenness may become larger, so it is preferred to perform a reduction reaction in the flow path and grow the particles as in the present invention.

[0133] By controlling the flow rate after adding formalin, the shape of the silver powder can be controlled. For example, making the flow rate after adding formalin slower than the flow rate of the silver complex solution before adding it is beneficial to reduce the aggregation of the silver powders.

[0134] The silver powder-containing liquid discharged to the outside of the flow channel was filtered and washed with water to obtain a block-like filter cake containing silver powder and water and having almost no fluidity.

[0135] The filter cake is dried using a forced circulation air dryer, a vacuum dryer, an airflow dryer, or the like to obtain the spherical silver powder of the present invention. Drying can be accelerated by replacing the water in the filter cake with a lower alcohol or the like.

[0136] The filter cake may be subjected to dry crushing treatment, surface smoothing treatment, etc. The surface smoothing treatment may be performed by mechanically colliding particles with each other using a high-speed stirrer.

[0137] Then, aggregates of silver powder having a particle size larger than a predetermined size may be removed by classification treatment.

[0138] Furthermore, the cake may be dried, crushed, and classified using an integrated device capable of drying, crushing, and classifying (DryMysta and MICRON dryers manufactured by HosokawaMicron Corporation, etc.).

[0139] <Silver powder manufacturing device>

[0140] In the manufacturing method of the present invention, a spherical silver powder manufacturing device can be used, which has a pipe forming a flow path of a silver-containing solution, a complexing agent adding part connected to the pipe, and a formalin adding part connected to the pipe at the downstream side of the complexing agent adding part. The structures of the complexing agent adding part and the formalin adding part are not particularly limited.

[0141] The complexing agent adding part or the formalin adding part may be a Y-shaped pipeline or a T-shaped pipeline respectively, or may be a structure in which a second tube is connected in the middle of the tube forming the flow path of the silver-containing solution so that the flow path of the silver-containing solution merges with the flow path of the second tube.

[0142] Alternatively, the complexing agent adding part or the formalin adding part may be coaxial twin-axis pipelines respectively. Figure 1 This is a schematic diagram of an example of a silver powder production apparatus in which a complexing agent adding section and a formalin adding section are coaxial twin-axis pipelines.

[0143] Figure 1 In the present invention, a silver powder manufacturing device 1 has a tube 2 for circulating a silver-containing solution, a complexing agent supply tube 3 for supplying a complexing agent, and a formalin supply tube 4 for supplying formalin. The tube 2 is formed in a straight line, and the complexing agent supply tube 3 and the formalin supply tube 4 are respectively formed in a substantially L-shaped shape. In the silver powder manufacturing device 1, the complexing agent supply tube 3 is arranged inside the tube 2 in such a manner that one side of the L-shaped complexing agent supply tube 3 is coaxial with the tube 2, and the formalin supply tube 4 is arranged inside the tube 2 on the downstream side of the arrangement portion in such a manner that one side of the L-shaped formalin supply tube 4 is coaxial with the tube 2. The complexing agent and formalin are respectively supplied to the downstream side of the flow path of the tube 2 from the complexing agent supply tube 3 and the formalin supply tube 4. The silver powder manufacturing device 1 is provided with a surface treatment agent supply tube 5 for supplying a surface treatment agent on the downstream side of the portion of the tube 2 where the formalin supply tube 4 is arranged. The surface treatment agent supply pipe 5 for supplying the surface treatment agent may be disposed upstream of the portion where the formalin supply pipe 4 is disposed, for example, between the complexing agent supply pipe 3 and the formalin supply pipe 4 .

[0144] The silver powder manufacturing device may have the following structure: the tube for circulating the silver-containing solution is provided with a slit having an opening radially outward along the inner circumference of the tube, and is connected with a formalin supply pipe for supplying formalin to the slit. There are preferably at least two formalin supply pipes. By using a device having such a structure, formalin can enter the tube from the slit approximately vertically (for example, more than 75 degrees and less than 105 degrees) from the outer circumference of the tube as a whole.

[0145] Figure 2 This is a schematic diagram of an example of a silver powder production apparatus including a formalin adding section for supplying formalin into a tube through a slit.

[0146] Figure 2 In the present invention, the silver powder manufacturing device 1 has a tube 2 for circulating a silver-containing solution, a complexing agent supplying tube 3 for supplying a complexing agent, and a formalin adding member 10 for supplying formalin. Formalin supplying tubes 14a and 14b are eccentrically connected to the formalin adding member 10. Formalin supplied from the formalin supplying tubes 14a and 14b enters the tube from the slit provided in the tube 2 and from the outer periphery of the tube as a whole. Figure 2 The silver powder production apparatus 1 includes a surface treatment agent supply pipe 5 for supplying a surface treatment agent on the upstream side of the formalin adding means 10 of the pipe 2, but the surface treatment agent supply pipe 5 may be arranged on the downstream side.

[0147] <Conductive paste>

[0148] The spherical silver powder of the present invention can provide a conductive paste having excellent printability and low-temperature sintering properties, and is suitable as a conductive paste used for internal electrodes of multilayer capacitors, conductor patterns of circuit boards, electrodes of various electronic components including solar cells, circuits, and the like.

[0149] The conductive paste of the present invention may contain the spherical silver powder of the present invention, an organic binder, and a solvent.

[0150] The organic binder is not particularly limited, and examples thereof include silicone resins, epoxy resins, acrylic resins, polyester resins, polyimide resins, polyurethane resins, phenoxy resins, cellulose resins (ethyl cellulose, hydroxypropyl cellulose, etc.), etc. They may be used alone or in combination of two or more in any ratio.

[0151] The solvent is not particularly limited, and examples thereof include alcohol solvents such as terpineol, butyl carbitol, Texanol, ethylene glycol, diethylene glycol, and glycerol; ester solvents such as butyl carbitol acetate and ethyl acetate; hydrocarbon solvents such as toluene, xylene, and cyclohexane, etc. These may be used alone or in combination of two or more in any ratio.

[0152] The content of the spherical silver powder of the present invention in the conductive paste can be 80% by mass or more, preferably 85% by mass or more, and can be 95% by mass or less, preferably 90% by mass or less.

[0153] The content of the organic binder in the conductive paste can be 0.1% by mass or more, preferably 0.2% by mass or more, and can be 0.4% by mass or less, preferably 0.3% by mass or less.

[0154] The content of the solvent in the conductive paste can be 6% by mass or more, preferably 7% by mass or more, and can be 20% by mass or less, preferably 15% by mass or less.

[0155] The conductive paste may contain glass powder, a dispersant, a surfactant, a viscosity modifier, a lubricant, etc. as optional components. The conductive paste used in the manufacture of the electrode of the solar cell preferably contains glass powder, for example, glass powders of Pb-Te-Bi system, Pb-Si-B system, etc. are mentioned.

[0156] The method for producing the conductive paste is not particularly limited, and examples thereof include a method of mixing the spherical silver powder of the present invention, an organic binder, a solvent, and optional components as appropriate. The mixing method is not particularly limited, and examples thereof include a self-rotating revolution mixer, an ultrasonic disperser, a disperser, a three-roll mill, a ball mill, a bead mill, a biaxial kneader, and the like.

[0157] The conductive paste of the present invention can be applied on a substrate by printing such as screen printing, offset printing, photolithography, or dipping to form a coating film. The coating film can also be formed into a predetermined pattern by photolithography using a resist.

[0158] The conductive film can be formed by firing the coating film. The firing can be performed in air atmosphere or in a non-oxidizing atmosphere such as nitrogen.

[0159] The spherical silver powder of the present invention has excellent low-temperature sintering properties, and the sintering temperature of the coating film can be set to 600° C. to 800° C., preferably 690° C. to 760° C. The sintering time can be set to 20 seconds to 1 hour, preferably 40 seconds or more, preferably 20 minutes or less, and more preferably 2 minutes or less.

[0160] The conductive paste of the present invention can be suitably used for forming internal electrodes of multilayer capacitors, conductor patterns of circuit boards, and electrodes and circuits of various electronic components including solar cells.

[0161] Example

[0162] Hereinafter, examples of the present invention will be described, but the present invention is not limited to the examples.

[0163] [Evaluation of Silver Powder]

[0164] The evaluation of the silver powder in the examples and comparative examples was carried out as follows.

[0165] <True Density>

[0166] The true density was measured by the constant volume expansion method ("gas pycnometer method" in the Japanese Pharmacopoeia) using a dry-type automatic density meter (manufactured by Micromeritics, device name: AccuPyc II 1340). In the measurement of the true density, the measurement was carried out in such a form that the silver particles with a density not connected to the outside contained closed pores inside.

[0167] <BET Specific Surface Area>

[0168] The BET specific surface area was measured using a fully automatic specific surface area measuring device (manufactured by Mountech, device name: Macsorb HM-model 1210). The silver powder was placed in the device, and after degassing by flowing a He-N2 mixed gas (30% nitrogen) at 60 °C for 10 minutes, the measurement was carried out by the BET single-point method.

[0169] <D 10 、D 50 、D 90 >

[0170] D 10 、D 50 、D 90 The particle size distribution was measured by the wet sample measurement method of laser diffraction using a Microtrac particle size distribution measuring device (manufactured by Microtrac BEL Co., Ltd., device name: MT-3300EXII). At the time of measurement, 0.1 g of the sample (silver powder) was added to 40 mL of isopropyl alcohol (IPA) for dispersion. The dispersion was carried out using an ultrasonic homogenizer (manufactured by Nippon Seiki Co., Ltd., device name: US-150T; 19.5 kHz, tip diameter 18 mm). The dispersion time was set to 2 minutes. The dispersed sample was supplied to the above device, and the particle size distribution was obtained using the attached analysis software.

[0171] <Ignition Loss (Ig-Loss) of Silver Powder>

[0172] Regarding the ignition loss, 2 g of the sample (silver powder) was weighed and placed in a magnetic crucible. After burning for 30 minutes as a sufficient time to reach a constant weight at 800 °C, the sample was cooled, weighed, and the mass (w) after heating was obtained. The ignition loss (%) was calculated by the following formula.

[0173] Ignition loss (%) = (2 - w) / 2 × 100

[0174] The unknown components are values ​​obtained by subtracting the measured values ​​of the contents of carbon, nitrogen and oxygen measured by the following measuring method of "Contents of Carbon, Nitrogen and Oxygen" from the ignition loss.

[0175] <Contents of Carbon, Nitrogen and Oxygen>

[0176] The contents of carbon, nitrogen and oxygen were measured as follows.

[0177] The carbon content was measured by infrared absorption method using a carbon and sulfur analyzer (manufactured by Horiba, Ltd., device name: EMIA-810) to measure CO and CO2 generated when the sample (silver powder) was heated to 1350°C in an oxygen flow to melt, and converted from the measured value. The amount of the sample (silver powder) used in the measurement was determined by preliminary measurement and comparison with the strength of the standard sample, and the amount was set to fall within the range of the standard curve.

[0178] The nitrogen content was determined by using an oxygen, nitrogen, and hydrogen simultaneous analyzer (manufactured by LECO, device name: ONH836) with a pulse furnace power of 4,000 W in a helium or argon atmosphere and by a heat conduction method in 0.20 g of a sample (silver powder).

[0179] The oxygen content in 0.05 g of the sample (silver powder) was measured by infrared absorption method in a helium or argon atmosphere using an oxygen, nitrogen, and hydrogen simultaneous analyzer (manufactured by LECO, device name: ONH836) with the power of the pulse furnace set to 4,000 W.

[0180] <Tap density>

[0181] The tap density (TAP) is the value obtained using a tap density measuring device (manufactured by Shibayama Scientific Co., Ltd., device name: Casa Specific Gravity Measuring Device SS-DA-2). The tap density is measured as follows. 30 g of silver powder is weighed and placed in a 20 mL test tube, and tapped 1000 times with a drop of 20 mm. Then, the sample volume (cm 3 ). Tap density (g / cm 3 ) is obtained by the following formula.

[0182] Tap density (g / cm 3 )=30(g) / volume of sample after impact(cm 3 )

[0183] [Production of silver powder]

[0184] The silver powders of Examples and Comparative Examples were prepared as follows.

[0185] <Example 1>

[0186] use Figure 1 The apparatus shown produces silver powder.

[0187] A silver nitrate aqueous solution with a silver concentration of 0.13 mol / L was introduced into a tube 2 (inner diameter 20 mm) at a liquid temperature of 25.7° C. at a flow rate of 21.5 L / min, and about 1 second later, a 9.4% by mass ammonia aqueous solution was introduced from a complexing agent supply tube 3 (inner diameter 6 mm) which was a coaxial double tube at a flow rate of 2.3 L / min to generate a silver ammonia complex in the tube 2. The amount of the silver nitrate aqueous solution was such that the silver concentration in the total liquid volume after adding the complexing agent / formalin / surface treatment agent became 0.1 mol / L.

[0188] About 2.23 seconds after the addition of the ammonia solution, formalin (17.4 mass % formaldehyde aqueous solution) was introduced at a flow rate of 2.5 L / min from the formalin supply pipe 4 (inner diameter 6 mm, outer diameter 8 mm) as a coaxial double-layer tube to precipitate the silver powder. The flow rate of the silver complex solution before the formalin addition immediately before the formalin addition position was 1.50 m / s, and the flow rate of the formalin was 1.50 m / s.

[0189] About 1 second after the addition of formalin, the surface treatment agent (0.17 mass % SELOSOL aqueous solution. SELOSOL 920 (manufactured by Chukyo Oil Co., Ltd., containing 15.5 mass % stearic acid)) was introduced from the surface treatment agent supply pipe 5 at a flow rate of 2.5 L / min. The amount of stearic acid added relative to silver (target value) was 0.18 mass %. A slurry containing silver powder was thus obtained. In the above, the distance from the ammonia solution addition position to the formalin addition position was set to 1.8 m, and the distance from the formalin addition position to the surface treatment agent addition position was set to 1.6 m.

[0190] The slurry containing silver powder is discharged from tube 2. The obtained slurry containing silver powder is subjected to solid-liquid separation, and the obtained solid is washed with pure water to remove impurities in the solid. The end point of the washing can be judged by the conductivity of the water after washing. The water is washed until the conductivity reaches 0.5 mS / m or less, and then it is dried and crushed to obtain 310 g of silver powder. The time from the addition of the surface treatment agent to the discharge is 1 to 2 seconds. Other production conditions and evaluation results are shown in Tables 1 and 2.

[0191] The SEM photograph (10000 times) of the silver powder of Example 1 is shown in Figure 3A (before vacuum drying) and Figure 3B (after vacuum drying and crushing). And, Figure 3C The field emission scanning electron microscope (FE-SEM) (20,000 times) of the particle cross section of the silver powder (after vacuum drying and crushing) is shown in FIG. Figure 3C It can be seen that there are pores inside the particles.

[0192] <Example 2>

[0193] In the preparation of the silver powder of Example 2, the setting position of the surface treatment agent supply pipe 5 was changed to set the surface treatment agent supply pipe 5 between the complexing agent supply pipe 3 and the formalin supply pipe 4, and the surface treatment agent was added before adding formalin. The distance from the surface treatment agent addition position before adding formalin to the formalin addition position was set to 17.5 cm. Other preparation conditions are shown in Table 1, and the silver powder of Example 2 was prepared in the same manner as in Example 1. The evaluation results are shown in Table 2.

[0194] The SEM photograph (10000 times) of the silver powder of Example 2 is shown in Figure 4A (before vacuum drying) and Figure 4B (After vacuum drying and crushing). In addition, Figure 4C The FE-SEM image (20,000 times) of the particle cross section of the silver powder of Example 2 (after vacuum drying and crushing treatment) is shown in FIG. Figure 4C It can be seen that there are pores inside the particles.

[0195] <Examples 3 to 6>

[0196] In the preparation of the silver powders of Examples 3 to 6, Figure 2 The silver powder manufacturing device shown. A slit (slit width 0.44mm) with an opening toward the radial outside is provided along the inner circumference of tube 2 (tube inner diameter 20.6mm), and a device having a formalin addition component 10 (recorded as a slit in Table 1) that eccentrically connects the supply pipes 14a and 14b of formalin to the slit is used to add formalin into the tube from the entire circumference of tube 2. A surface treatment agent supply pipe 5 is provided between the formalin addition component 10 and the complexing agent supply pipe 3, and a surface treatment agent is added before adding formalin. In the formalin addition component 10 of Example 5, a tube 2 with a tube inner diameter of 21.4mm is used. In Examples 5 and 6, a mixer that imparts rotation to the flow is configured at the introduction position of the silver nitrate aqueous solution to carry out liquid mixing. It should be noted that the distance from the ammonia solution addition position to the formalin addition position is set to 2.1m, and the distance from the surface treatment agent addition position before the formalin addition to the formalin addition position is set to 17.5cm. The other production conditions are shown in Table 1, and the silver powders of Examples 3 to 6 were produced in the same manner as in Example 1. Table 2 shows the evaluation results.

[0197] The SEM photographs (10000 times) of the silver powders of Examples 3 to 6 are shown in Figures 5A to 8A (before vacuum drying) and Figure 5B to Figure 8B (after vacuum drying and crushing). And, Figure 5C to Figure 8C FE-SEM images (20,000 times) of the particle cross-sections of the silver powders of Examples 3 to 6 (after vacuum drying and crushing) are shown in FIG. Figure 5C to Figure 8C It can be seen that the silver powders of Examples 3 to 6 have pores inside the particles.

[0198] <Example 7>

[0199] The silver powder of Example 7 was prepared in the same manner as in Example 1 except that the preparation conditions were changed to those shown in Table 1. The evaluation results are shown in Table 2. The SEM photograph (magnification 10,000) of the silver powder of Example 7 is shown in Table 2. Fig.9A (before vacuum drying) and Fig. 9B (After vacuum drying and crushing). In addition, Fig. 9C The FE-SEM image (20,000 times) of the particle cross section of the silver powder (after vacuum drying and crushing treatment) of Example 7 is shown in FIG. Fig. 9C It can be seen that there are pores inside the particles.

[0200] <Comparative Example 1>

[0201] In the preparation of the silver powder of Comparative Example 1, Figure 1 The silver powder manufacturing device shown in the figure (where the complexing agent supply pipe 3 is not provided) is preliminarily mixed with an aqueous silver nitrate solution and an aqueous ammonia solution in a tank (not shown) to prepare an aqueous silver ammonia complex solution with a silver concentration of 0.12 mol / L and an ammonia concentration of 0.51 mol / L. About 5 minutes after the preparation, Figure 1 Into a silver powder manufacturing device (which does not include a complexing agent supply pipe 3), a silver ammonia complex aqueous solution was introduced at a liquid temperature of 30.4° C. and a flow rate of 25.6 L / min into a tube (inner diameter 20 mm) to replace the silver-containing solution.

[0202] About 4 seconds after the introduction of the silver ammine complex aqueous solution, formalin (18.5 mass % aqueous solution) was introduced from the inner tube of the coaxial double tube (inner diameter 6 mm, outer diameter 8 mm) at a flow rate of 2.5 L / min to precipitate silver powder.

[0203] Next, a surface treatment agent (0.17 mass % SELOSOL aqueous solution. SELOSOL 920 (manufactured by Chukyo Yushi Co., Ltd., containing 15.5 mass % of stearic acid)) was supplied from a supply tube (inner tube 6 mm) connected to the pipe.

[0204] The silver-containing paste was discharged from the tube and treated in the same manner as in Example 1. Other production conditions and evaluation results are shown in Tables 1 and 2. A SEM photograph (10,000 times) of the silver powder of Comparative Example 1 is shown in Fig. 10A (before vacuum drying) and Fig. 10B (After vacuum drying and crushing). In addition, Fig. 10C : A FE-SEM photograph (20,000 times) of a particle cross section of the silver powder of Comparative Example 1 (after vacuum drying and crushing treatment) is shown.

[0205] <Comparative Example 2>

[0206] The silver powder of Comparative Example 2 was prepared in the same manner as in Comparative Example 1, except that the surface treatment agent was added before adding formalin.

[0207] The SEM photograph (10000 times) of the silver powder of Comparative Example 2 is shown in Fig.11A (before vacuum drying) and Fig. 11B (After vacuum drying and crushing). In addition, Fig. 11C : A FE-SEM photograph (20,000 times) of a particle cross section of the silver powder of Comparative Example 2 (after vacuum drying and crushing treatment) is shown.

[0208] [Table 1]

[0209]

[0210] [Table 2]

[0211]

[0212] [Thermomechanical Analysis (TMA)]

[0213] Using the silver powder of the embodiment and the comparative example, a load of 50 kgf was applied for 1 minute by a pellet forming machine to make roughly cylindrical (5 mm in diameter) particles, and the particles were placed in a thermomechanical analysis (TMA) device (manufactured by Rigaku Corporation, device name: TMA8311), and heated from room temperature to 900°C at a heating rate of 10°C / min in an atmospheric atmosphere. The heat shrinkage rate was calculated by the following formula based on the length a of the particle at room temperature and the length b of the particle at the most contracted time, c, relative to the difference (ab). The temperatures at which the heat shrinkage rate reached 10%, 20%, 50%, and 90% were obtained, and the thermal expansion was evaluated.

[0214] Thermal shrinkage = c × 100 / (ab)

[0215] Table 3 shows the temperatures at which the heat shrinkage rates of the silver powders of Examples 1 to 4, Examples 6 to 7, and Comparative Examples 1 to 2 reach 10%, 20%, 50%, and 90%.

[0216] [Table 3]

[0217] (℃)

[0218] Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 Example 4 Example 6 Example 7 10% shrinkage temperature 418 415 350 399 367 363 378 317 20% shrinkage temperature 444 435 387 428 398 395 409 354 50% shrinkage temperature 506 489 455 489 461 457 469 429 90% shrinkage temperature 624 597 552 591 555 551 568 529

[0219] The results of the measurement of the heat shrinkage ratios of Example 1 and Comparative Examples 1 and 2 are shown in the graph. Fig.12 The vertical axis of the graph represents the ratio of the amount of change (contraction) in the length of the pellet to the difference between the length of the pellet at room temperature and the length of the pellet at the most contracted state.

[0220] [Preparation of conductive paste]

[0221] Conductive pastes were prepared as follows using the silver powders of Examples 1 to 6 and Comparative Examples 1 and 2.

[0222] The silver powders of the examples and comparative examples were subjected to the following treatments to obtain conductive pastes at the composition ratios shown in Table 4. After stirring and mixing at 1400 rpm for 30 seconds using a propeller-free self-rotating and revolving stirring and degassing device (AR310 manufactured by THINKY), the mixture was kneaded using a three-roll mill (80S manufactured by EXAKT) to pass through the roll gap from 100 μm to 20 μm.

[0223] [Table 4]

[0224] quality% Ethyl cellulose 0.10 Hydroxypropyl Cellulose 0.10 wax* 0.07 Triethylene glycol butyl methyl ether 1.83 Terpineol 1.20 Texano 1.28 Butyl Carbitol Acetate 1.18 Tributyl citrate 1.34 Dimethicone 100cs** 0.40 Triethanolamine 0.26 castor oil 0.07 Oleic acid 0.69 Pb-Te-Bi glass powder 1.99 Silver powder of examples and comparative examples 89.48 total 100.00

[0225] *NAMLON206r manufactured by Kusumoto Chemicals Co., Ltd.

[0226] **KF96-100 manufactured by Shin-Etsu Chemical Co., Ltd.

[0227] [Evaluation of Printability (Thin Line Printability)]

[0228] The thin line evaluation (EL) is performed by forming a conductive pattern. The conductive pattern is formed as follows. First, a screen printer (Microtec, MT-320TV) is used on a silicon substrate for solar cells (100Ω / □) to form a 154mm solid pattern on the back of the substrate using aluminum paste (Rutech, 28D22G-2). Next, the conductive paste prepared using the silver powder of the embodiment and the comparative example is filtered through 500 mesh and then filtered on the surface of the substrate. Fig.13 The pattern shown is printed (coated) with electrodes (finger electrodes) with a line width of 14μm-26μm and electrodes (busbar electrodes) with a width of 1mm at a scraper speed of 350mm / sec. After hot air drying at 200°C for 10 minutes, a high-speed sintering furnace IR furnace (manufactured by Nippon Insulator Co., Ltd., high-speed sintering test 4-chamber furnace) is used to perform sintering at a peak temperature of 750°C and an in-and-out time of 41 seconds to obtain a conductive pattern.

[0229] After obtaining the conductive pattern, an EL / PL evaluation device (PVX330+POPLI-3C manufactured by ITES Co., Ltd.) was used to check whether the electrode was broken. It should be noted that in the EL / PL evaluation device, a current was passed through the busbar electrode to perform EL (electroluminescence) evaluation. If there is a break in the electrode (finger electrode) between the busbar electrodes, the position where the break occurs does not emit light and appears black. Figures 14 to 21The EL evaluation results of the conductive paste using the silver powder of Examples 1 to 6 and Comparative Examples 1 to 2 are shown. In the conductive paste using the silver powder of the comparative example, the results show that the thinner the line width, the more black parts that do not emit light due to broken lines, which shows that the conductive paste using the silver powder of the example can perform fine line printing. Even when the peak temperature during firing is set to 690°C and 710°C, the example has less broken lines, and light emission with a thinner line width is obtained, which enables fine line printing.

[0230] [Measurement of volume resistivity]

[0231] Conductive films were prepared and the volume resistivity was measured for the conductive pastes using the silver powders of Examples 1 to 6 and Comparative Examples 1 and 2. The conductive films were prepared as follows.

[0232] The sample for volume resistivity evaluation was made by screen printing a conductive paste. The printer used was MT-320 manufactured by Micro-tec Co., Ltd., the mask was manufactured by MURAKAMI CO., LTD. (250 mesh, emulsion thickness 10 μm), and a serrated design with a line width of 0.5 mm and a length of 128 mm was used. During printing, the scraper speed was 40 mm / s and the printing pressure was 0.18 MPa. The printed object used a substrate processed into a 1-inch square Si substrate for solar cells.

[0233] The printed sample was placed in a hot air dryer (LC-114 manufactured by ESPEC) set at 200°C and allowed to stand for 5 minutes to dry. After drying, it was fired in a high-speed firing test furnace (solar cell firing furnace manufactured by NGK) at a peak temperature of 690°C, 710°C, and 740°C for a 1-inch substrate to obtain a conductive film.

[0234] In the evaluation of volume resistivity, the line resistance of the obtained conductive film was measured with a digital multimeter (7451A manufactured by ADVANTEST), and the average value of the cross-sectional area of ​​the conductive film was measured with a laser microscope (VK-X1000 manufactured by KEYENCE). The line resistance (Ω) was multiplied by the average value of the cross-sectional area and divided by the length of the conductive film to obtain the volume resistivity (μΩ·cm). The results are shown in Table 5.

[0235] [Table 5]

[0236] (μΩcm)

[0237] Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 740℃ firing 4.85 4.20 3.23 3.23 3.49 3.37 2.72 3.61 710℃ sintering 4.67 4.10 3.17 3.17 3.37 2.46 3.58 3.52 690℃ firing 4.49 3.83 3.01 3.01 3.20 3.04 3.24 3.36

[0238] The conductive films produced at any sintering temperature in Examples all showed low volume resistivity, and it was found that the conductive paste using the silver powder of Examples had excellent low-temperature sintering properties.

[0239] Industrial Applicability

[0240] According to the present invention, there are provided spherical silver powder which can provide excellent printability and low-temperature sintering properties when used in a conductive paste or the like, and a method and apparatus for producing the same.

[0241] Description of Reference Numerals

[0242] 1 Silver powder manufacturing device

[0243] 2 tubes

[0244] 3 Complexing agent supply pipe

[0245] 4 Formalin supply tube

[0246] 5 Surface treatment agent supply pipe

[0247] 10 Formalin Additive

[0248] 14a Formalin supply tube

[0249] 14b Formalin supply tube

Claims

1. A spherical silver powder having a cumulative 50% diameter D based on volume by laser diffraction method. 50 Relative to BET diameter D BET The ratio is D 50 / D BET It is 0.9 or more and 1.2 or less, and has pores inside the particles.

2. The spherical silver powder according to claim 1, having a true density of 9.0 g / cm 3 Above and 10.0g / cm 3 the following.

3. The spherical silver powder according to claim 1, wherein The D 50 It is not less than 0.2 μm and not more than 3.5 μm.

4. The spherical silver powder according to claim 1, wherein the BET specific surface area is 0.17 m 2 / g or more and 3.23m 2 / g or less.

5. The spherical silver powder according to claim 1, wherein The value obtained by subtracting the contents of carbon, nitrogen and oxygen from the loss on ignition is less than 0.10 mass %.

6. The spherical silver powder according to claim 1, wherein The ratio of the oxygen content to the carbon content is 1.5 or more.

7. A method for producing spherical silver powder, wherein: The silver-containing solution is allowed to flow in a flow path, a complexing agent is added to the flow path at a complexing agent adding position in the middle of the flow path, and formalin is added to the flow path at a formalin adding position downstream of the complexing agent adding position, so that silver powder is reduced and precipitated in the flow path.

8. The method for producing spherical silver powder according to claim 7, wherein: The time required for the silver-containing solution to flow from the complexing agent addition position to the formalin addition position is 0.1 seconds or more and within 10 seconds.

9. The method for producing spherical silver powder according to claim 7, wherein: A surface treatment agent is added to the flow path between the complexing agent addition position and the formalin addition position or on the downstream side of the formalin addition position.

10. The method for producing spherical silver powder according to any one of claims 7 to 9, wherein: The formalin is added from a plurality of directions at the formalin adding position, and the plurality of directions respectively form an angle of not less than 75 degrees and not more than 105 degrees with respect to the flow path.

11. A device for producing spherical silver powder, which is a device for producing spherical silver powder by adding a complexing agent and formalin to a silver-containing solution to reduce and precipitate silver powder, and which comprises: a tube forming a flow path for the silver-containing solution; a complexing agent adding section connected to the tube; and a formalin adding section connected to the tube on the downstream side of the complexing agent adding section. 12 . A conductive paste comprising the spherical silver powder according to claim 1 , an organic binder, and a solvent. 13 . The conductive paste according to claim 12 , which is used to form an electrode of a solar cell.