Silicone release polyester film and method of making same

The silicone release polyester film addresses peeling force variations in ceramic green sheets by using a specialized composition, enhancing peeling control and reducing defects in laminated ceramic capacitors.

CN119095723APending Publication Date: 2024-12-06TOYOBO CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202380036521.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-10
Filing Date
2023-05-08
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing release films for ceramic green sheets in laminated ceramic capacitors face issues with varying peeling forces, leading to cracks, deformation, and defects such as pinholes and thickness fluctuations, especially during the manufacturing process of stacked ceramic capacitors with varying thicknesses.

Method used

A silicone release polyester film with a specific composition and structure, including an aqueous dispersion of silicones with Q units and Si-H groups, a platinum-based catalyst, and a nonionic emulsifier, applied to a polyester film to achieve a controlled peeling force from light to heavy peeling, minimizing sheet deformation and defects.

Benefits of technology

The silicone release polyester film provides effective peeling properties, reducing defects and ensuring high reliability and yield in the production of laminated ceramic capacitors by maintaining sheet integrity and uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005102387400000201
    Figure BDA0005102387400000201
Patent Text Reader

Abstract

Provided are: a silicone release polyester film which is suitable for use as a carrier film or the like in the production of a laminated ceramic capacitor, is suitable for sheet molding from light peeling to heavy peeling, and has excellent peelability and adhesion; a method for producing the silicone release polyester film; and the like. A silicone mold release polyester film having a coating layer formed using a coating composition for mold release on at least one surface of a polyester film, the coating composition for mold release contains an aqueous dispersion (1) of at least one silicone (A) containing an alkenyl group and / or a Q unit represented by SiO4 / 2, an aqueous dispersion (2) of a silicone (B) having a hydrogen atom directly bonded to an Si atom represented by an Si-H group, a crosslinking reaction inhibitor, a platinum-based catalyst, and a nonionic emulsifier, and is characterized in that: the number-average molecular weight of the silicone (A) is 150000 or more; the content of Si atoms contained in the Q unit is from 0.05 mol% to 60 mol% (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a silicone release polyester film, and more particularly to a silicone release polyester film having peelability and adhesion suitable for molding from light peeling to heavy peeling, which can prevent the occurrence of cracks and deformation of the ceramic green sheet used in the manufacture of a laminated ceramic capacitor, and a method for manufacturing the same. Background Art

[0002] As a carrier film for molding resin sheets and ceramic sheets, a release film is used. In particular, in terms of dimensional stability and heat resistance, polyester film is used as the base material of the release film. In recent years, especially with the advancement of miniaturization / high reliability of stacked ceramic capacitors, the thickness of ceramic green sheets manufactured in various places has also ranged from thick to thin. Therefore, various properties suitable for the thickness of the slurry are required for the carrier film. In the manufacture of stacked ceramic capacitors, the rigidity of the ceramic green sheet decreases during the filmization, and cracks will occur when the sheet is peeled off, so light peeling is required. In addition, in a certain thicker raw sheet, the rigidity becomes higher, so floating occurs between the sheet and the release film during the process transportation, causing deformation of the sheet. In this way, for the peeling of ceramic sheets, various peeling forces are sometimes required from light peeling to heavy peeling. In addition, regardless of the thickness of the raw sheet, the slight shrinkage defect during the coating of the ceramic slurry penetrates the sheet, thereby generating pinholes and thickness fluctuations, which will significantly deteriorate the yield of the stacked ceramic capacitor. Therefore, the coating uniformity of the release layer of the release film is required.

[0003] To address these problems, it has been proposed to add a component composed of a silicone resin having a trifunctional siloxane or tetrafunctional siloxane structure (see, for example, Patent Document 1). Specifically, the content of the silicone resin is not mentioned, and an emulsion-type release agent is not mentioned.

[0004] In addition, aqueous coating compositions containing silicone containing Q units and silicone having Si-H groups in a predetermined mol % range are described (for example, see Patent Document 2), but in particular, the optimal molecular weight range of the silicone containing Q units is not described.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 9-1527

[0008] Patent Document 2: Japanese Patent Application Publication No. 2021-11081 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] In view of the above situation, the present invention aims to provide: a silicone release polyester film with excellent peelability and adhesion suitable for sheet molding from light peeling to heavy peeling, which can also be used as a carrier film in the manufacture of laminated ceramic capacitors, and a method for manufacturing the same.

[0011] Solutions for solving problems

[0012] The present inventors have conducted intensive studies to solve the above problems and have found that it is possible to provide a release film having an appropriate release force from light to heavy release even when an emulsion-type silicone is used under certain specific conditions, thereby completing the present invention.

[0013] That is, the present invention provides the following silicone release polyester film (silicone release polyester film). [1]

[0015] A silicone release polyester film having a coating layer formed using a release coating composition on at least one side of the polyester film, wherein the release coating composition comprises: 4 / 2 An aqueous dispersion (1) of one or more silicones (A) having Q units as shown, an aqueous dispersion (2) of silicones (B) having hydrogen atoms directly bonded to Si atoms as shown by Si-H groups, a crosslinking reaction inhibitor, a platinum-based catalyst, and a nonionic emulsifier,

[0016] The number average molecular weight of the above-mentioned silicone A is 150,000 or more,

[0017] The content of Si atoms contained in the Q unit is 0.05 mol % or more and 60 mol % or less. [2]

[0019] The silicone release polyester film according to [1], wherein the content of the silicone (B) is 3 parts by mass or more and 45 parts by mass or less, based on 100 parts by mass of the total content of the silicone (A) and the silicone (B). [3]

[0021] The silicone release polyester film according to [1] or [2], wherein the alkenyl group of the silicone (A) is a vinyl group. [4]

[0023] The silicone release polyester film according to any one of [1] to [3], wherein the release strength after being attached to a polyester pressure-sensitive adhesive tape is 20 g / 25 mm width or more and 400 g / 25 mm width or less. [5]

[0025] The silicone release polyester film according to any one of [1] to [4], which is used for molding ceramic green sheets in the production of laminated ceramic capacitors.

[0026] Furthermore, the present invention provides the following method for producing a silicone release polyester film. [6]

[0028] A method for producing a silicone release polyester film, comprising the following steps: using a release coating composition to form a coating layer on at least one side of a polyester film, wherein the release coating composition comprises: a silicone release coating composition containing an olefinic group and / or SiO 4 / 2 An aqueous dispersion (1) of one or more silicones (A) having Q units as shown, an aqueous dispersion (2) of silicones (B) having hydrogen atoms directly bonded to Si atoms as shown by Si-H groups, a crosslinking reaction inhibitor, a platinum-based catalyst, and a nonionic emulsifier,

[0029] The number average molecular weight of the above-mentioned silicone A is 150,000 or more.

[0030] The content of Si atoms contained in the Q unit is in the range of 0.05 mol % or more and 60 mol % or less. [7]

[0032] The production method according to [6], wherein the content of the organosilicon (B) is 3 parts by mass or more and 45 parts by mass or less, based on 100 parts by mass of the total content of the organosilicon (A) and the organosilicon (B). [8]

[0034] The production method according to [6] or [7], wherein the alkenyl group of the organosilicon (A) is a vinyl group.

[0035] Effects of the Invention

[0036] The silicone release polyester film of the present invention has the above-mentioned structure, so that as a release film for sheet molding, it becomes a release film with a peeling force suitable for sheet molding of a thickness such as ceramic green sheets and moderate peeling properties with little sheet deformation, and can produce sheets with reduced defective rate and high reliability.

[0037] Furthermore, the method for producing the silicone release polyester film of the present invention can efficiently and simply produce the silicone release polyester film having the above-mentioned properties. DETAILED DESCRIPTION

[0038] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to these embodiments.

[0039] <Silicone release polyester film>

[0040] The silicone release polyester film of the present invention is a silicone release polyester film having a coating layer formed using a release coating composition on at least one surface of the polyester film.

[0041] The demoulding coating composition comprises: 4 / 2 An aqueous dispersion (1) of one or more silicones (A) having Q units as shown, an aqueous dispersion (2) of silicones (B) having hydrogen atoms directly bonded to Si atoms as shown by Si-H groups, a crosslinking reaction inhibitor, a platinum-based catalyst, and a nonionic emulsifier,

[0042] The number average molecular weight of the above-mentioned silicone A is 150,000 or more.

[0043] The content of Si atoms contained in the Q unit is 0.05 mol % or more and 60 mol % or less.

[0044] 〔Polyester film〕

[0045] For the polyester film of the present invention, known polyesters can be suitably used, and for example, the following polyesters can be suitably used.

[0046] (Polyester)

[0047] The polyester constituting the polyester film used as the substrate film in the present invention (hereinafter sometimes referred to as "substrate") is not particularly limited, and a film formed by molding a polyester commonly used as a substrate for a release film can be used. Preferably, it is a crystalline linear saturated polyester formed by an aromatic dibasic acid component and a diol component, for example, further suitable are polyethylene terephthalate, polyethylene isophthalate, polyethylene 2,6-naphthalate, polybutylene terephthalate, poly(1,4-cyclohexylene dimethylene terephthalate), polytrimethylene terephthalate or a copolymer with the constituent components of these resins as the main components. Among them, a polyester film formed by polyethylene terephthalate is particularly suitable. In polyethylene terephthalate, the repeating unit of ethylene terephthalate is preferably 90 mol% or more, more preferably 95 mol% or more, and a small amount of other dicarboxylic acid components and diol components may also be copolymerized. For example, from the aspect of cost, it is preferred to produce only from terephthalic acid and ethylene glycol.

[0048] Furthermore, known additives such as antioxidants, light stabilizers, ultraviolet absorbers, crystallizing agents, etc. may be added within the range not impairing the effects of the release film of the present invention. The polyester film is preferably a biaxially oriented polyester film because of its high elastic modulus in both directions.

[0049] The intrinsic viscosity of the polyester film is preferably 0.50 dl / g or more and 0.70 dl / g or less, more preferably 0.52 dl / g or more and 0.65 dl / g or less. When the intrinsic viscosity is 0.50 dl / g or more, a large amount of breakage does not occur during the stretching process, which is preferred. On the contrary, when it is 0.70 dl / g or less, the cutting property when cutting into a predetermined product width is good, and no dimensional defects occur, which is preferred. In addition, the raw material pellets are preferably fully vacuum dried.

[0050] In addition, in this specification, when abbreviated as "polyester film", it means the polyester film which has (laminated) the surface layer A and the surface layer B.

[0051] The method for producing the polyester film of the present invention is not particularly limited, and a conventionally commonly used method can be used. For example, the polyester is melted in an extruder, extruded into a film, cooled on a rotating cooling drum, thereby obtaining an unstretched film, and the unstretched film is biaxially stretched to obtain the film. The biaxially stretched film can be obtained by a method in which a uniaxially stretched film in the longitudinal or transverse direction is biaxially stretched in sequence in the transverse direction or longitudinal direction, or by a method in which an unstretched film is biaxially stretched in the longitudinal and transverse directions simultaneously.

[0052] In the present invention, the stretching temperature during stretching of the polyester film is preferably set to be equal to or higher than the secondary transition point (Tg) of the polyester. The film is preferably stretched by 1 to 8 times, particularly 2 to 6 times, in each of the longitudinal and transverse directions.

[0053] The thickness of the polyester film is preferably 12 μm or more and 100 μm or less, more preferably 16 μm or more and 50 μm or less, and more preferably 19 μm or more and 33 μm or less. If the thickness of the film is 12 μm or more, there is no worry of deformation due to heat during film production, processing, and molding, and it is preferred. On the other hand, if the thickness of the film is 100 μm or less, the amount of film discarded after use does not increase extremely, which is preferred in reducing environmental load.

[0054] The polyester film substrate may be a single layer or a multilayer of two or more layers. For example, the substrate film may be a polyester film having a surface layer A substantially free of particles having a particle size of 1.0 μm or more and a surface layer B containing particles. Preferably, the surface layer A substantially does not contain inorganic particles having a particle size of 1.0 μm or more.

[0055] In this embodiment, particles having a particle size of 1 nm or more and less than 1.0 μm may be present in the surface layer A. Since the surface layer A does not substantially contain particles having a particle size of 1.0 μm or more, such as inorganic particles, the particle shape in the substrate can be transferred to the resin sheet to reduce the occurrence of defects.

[0056] In one embodiment, the surface layer A does not contain particles having a particle diameter of less than 1.0 μm, and thus can more effectively suppress the transfer of particle shapes in the substrate to the resin sheet to cause problems.

[0057] In one embodiment, the polyester film substrate is preferably a laminated film having a surface layer A substantially free of inorganic particles on at least one surface. This can more effectively prevent the particle shape in the substrate from being transferred to the resin sheet and causing problems.

[0058] For example, it is preferable that the surface layer A substantially does not contain particles having a particle size of less than 1.0 μm and substantially does not contain particles having a particle size of 1.0 μm or more.

[0059] Here, in the present invention, "substantially free of particles" means, for example, in the case of inorganic particles smaller than 1.0 μm, when the inorganic elements are quantitatively analyzed by fluorescent X-ray analysis, the content is 50 ppm or less, preferably 10 ppm or less, and most preferably below the detection limit. This is because even if particles are not actively added to the film, there are cases where contamination components from foreign matter, dirt attached to production lines and devices in the raw resin or film manufacturing process are peeled off and mixed into the film. In addition, "substantially free of particles with a particle size of 1.0 μm or more" means that particles with a particle size of 1.0 μm or more are not actively included.

[0060] In the case of a laminated polyester film having a multilayer structure of two or more layers, it is preferred that a surface layer B which may contain inorganic particles and the like is provided on the opposite side of a surface layer A which does not substantially contain inorganic particles.

[0061] As a laminated structure, when the layer on one side of the release layer is set as the A layer, the layer on the opposite side is set as the B layer, and the core layer other than these is set as the C layer, the layer structure in the thickness direction can cite a laminated structure such as release layer / A / B or release layer / A / C / B. Of course, the C layer can be a multilayer structure. In addition, the surface layer B may not contain inorganic particles. In this case, in order to impart the slippage for winding the film into a roll, it is preferred that a coating layer containing at least inorganic particles and a binder is provided on the surface layer B.

[0062] In the polyester film substrate of the present invention, from the viewpoint of the slipperiness of the film and the ease of air removal, the surface layer B on the opposite side of the surface to which the release layer is applied preferably contains inorganic particles, and silica particles and / or calcium carbonate particles are particularly preferably used. The content of the inorganic particles contained in the surface layer B is preferably 5000 ppm or more and 15000 ppm or less based on the total amount of the inorganic particles.

[0063] At this time, the regional surface average roughness (Sa) of the film of surface layer B is preferably in the range of more than 1nm and less than 40nm. More preferably, the range is more than 5nm and less than 35nm. When the total amount of silicon dioxide particles and / or calcium carbonate particles is more than 5000ppm and Sa is more than 1nm, when the film is rolled into a roll, air can be released evenly, and the winding form is good and the planarity is good, thus, it becomes suitable for manufacturing ultra-thin layer ceramic green sheets. In addition, when the total amount of silicon dioxide particles and / or calcium carbonate particles is less than 15000ppm and Sa is less than 40nm, it is not easy to produce the aggregation of lubricants, and no coarse protrusions are produced, so the quality of ultra-thin layer ceramic green sheets is stable and preferred during manufacturing.

[0064] As the particles contained in the above-mentioned B layer, inactive inorganic particles and / or heat-resistant organic particles can also be used in addition to silicon dioxide and / or calcium carbonate, but from the viewpoint of transparency and cost, silicon dioxide particles and / or calcium carbonate particles are more preferably used. In addition, as inorganic particles that can be used in addition, aluminum oxide-silicon dioxide composite oxide particles, hydroxyapatite particles, etc. can be cited. In addition, as heat-resistant organic particles, cross-linked polyacrylic acid particles, cross-linked polystyrene particles, benzoguanamine particles, etc. can be cited. In addition, when using silicon dioxide particles, porous colloidal silica is preferred, and when using calcium carbonate particles, from the viewpoint of preventing the lubricant from falling off, it is preferred that light calcium carbonate surface-treated with a high molecular compound of a polyacrylic acid system is used.

[0065] The average particle size of the inorganic particles added to the surface layer B is preferably 0.1 μm or more and 2.0 μm or less, and particularly preferably 0.3 μm or more and 1.0 μm or less. If the average particle size of the inorganic particles is 0.1 μm or more, the slip property of the release film is good and thus it is preferred. In addition, if the average particle size is 2.0 μm or less, there is no concern about adversely affecting the smoothness of the release layer surface, and therefore, there is no concern about the generation of pinholes in the ceramic green sheet and thus it is preferred.

[0066] In addition, in order to improve the adhesion of a release layer to be applied later, or to prevent static electricity, a coating layer may be provided on the surface of the surface layer A and / or the surface layer B before stretching or after uniaxial stretching in the film-making process, or a corona treatment may be performed.

[0067] In addition, the peeling force of the silicone release polyester film of the present invention after being attached to the polyester adhesive tape can be set to 20g / 25mm width or more and 400g / 25mm width or less. The lower limit of the above-mentioned peeling force can be set to, for example, 30g / 25mm width or more, 40g / 25mm width or more, 50g / 25mm width or more, 70g / 25mm width or more, 100g / 25mm width or more, 120g / 25mm width or more, 150g / 25mm width or more, 180g / 25mm width or more. In addition, the upper limit of the above-mentioned peeling force can be set to, for example, 380g / 25mm width or less, 350g / 25mm width or less, 330g / 25mm width or less, 300g / 25mm width or less, 280g / 25mm width or less, 250g / 25mm width or less, 230g / 25mm width or less, 200g / 25mm width or less. The peel strength is preferably 20 g / 25 mm or more and 400 g / 25 mm or less. The silicone release polyester film of the present invention has the above-mentioned structure, and therefore, for example, by introducing silicone resin (Q unit resin) into the silicone main agent (silicone A), it has a release film with a moderate hardness and a good adhesion as a sheet-forming release film even when a small amount of crosslinking agent is used. By adjusting the amount of crosslinking agent added, the peeling force from light peeling to heavy peeling can be controlled, and its industrial value is extremely high.

[0068] In the present invention, the above-mentioned adhesive tape peel strength refers to the strength obtained as follows: a polyester adhesive tape (manufactured by Nitto Denko Corporation, No. 31B) is attached to the surface of the coating layer (release layer) of a release film, and the result is crimped with a 5 kg crimping roller and left for more than 30 minutes, and then the peel strength between the release layer and the adhesive tape is measured with a peel strength tester (peeling angle 180 degrees, peeling speed 300 mm / min, unit: g / 25 mm width).

[0069] [Mold release coating composition]

[0070] The mold release coating composition of the present invention comprises: 4 / 2 An aqueous dispersion (1) of one or more silicones (A) having Q units as shown, an aqueous dispersion (2) of silicones (B) having hydrogen atoms directly bonded to Si atoms as shown by Si-H groups, a crosslinking reaction inhibitor, a platinum-based catalyst, and a nonionic emulsifier.

[0071] (containing alkenyl and / or SiO 4 / 2 One or more silicones (A) of the Q unit shown

[0072] As the alkenyl group and / or SiO 4 / 2The organosilicon (A) of the Q unit (hereinafter, sometimes simply referred to as "Q unit") shown is exemplified by an organopolysiloxane (hereinafter, sometimes referred to as "organosilicon (A)") having the following general formula (I).

[0073] R 1 a R 2 b SiO (4-a-b) / 2 ···(I)

[0074] (In formula (I), R 1 is an alkenyl group having 2 to 8 carbon atoms, R 2 It is a monovalent saturated hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group, and a is an integer of 0 to 3 and b is an integer of 0 to 3, and satisfies a+b≤3.

[0075] As R 1 Examples of the alkenyl group having 2 to 8 carbon atoms include vinyl, allyl, butenyl, pentenyl, hexenyl, etc. Among them, vinyl is particularly preferred. 2 Examples of the alkyl group include methyl, ethyl, propyl, and butyl. Examples of the aryl group include phenyl and tolyl. Among them, in terms of light peelability, R 2 50 mol % or more of the substituents are methyl groups.

[0076] The organosilicon (A) containing alkenyl groups and / or Q units must contain Q units. Among them, when the organosilicon (A) containing alkenyl groups and / or Q units contains multiple types, it is sufficient as long as any one of them contains Q units. The Q unit is contained in the organosilicon-based release layer, thereby increasing the coating hardness of the silicone-based release layer, which can suppress the viscosity loss when peeling off the sheet, and thus is related to easy peeling. In addition, when the organosilicon containing Q units is contained in the above-mentioned alkenyl-containing organosilicon, the wettability is also improved, so pinhole defects during sheet coating can be suppressed. The content of Si atoms contained in the Q unit is 0.05 mol% or more and 60 mol%, preferably 0.1 mol% or more and 55 mol% or less, and more preferably 1.0 mol% or more and 50 mol% or less, relative to all Si atoms in the organosilicon (A) containing alkenyl groups and / or Q units. When the content of Si atoms in the Q unit is less than 0.05 mol%, sufficient coating hardness cannot be achieved and light peeling is not involved. If it exceeds 60 mol%, excessive wettability is imparted and the film is strongly adhered to the sheet, resulting in cohesive failure of the sheet surface (excessive heavy peeling).

[0077] In addition, the number average molecular weight of the organosilicon (A) containing alkenyl groups and / or Q units is 150,000 or more, for example, preferably 180,000 or more, 200,000 or more, 220,000 or more, etc. In addition, the number average molecular weight of the organosilicon (A) containing alkenyl groups and / or Q units can be, for example, 1,000,000 or less, 900,000 or less, 800,000 or less, 700,000 or less, 600,000 or less, 500,000 or less, 400,000 or less, etc. If it is less than 150,000, when the amount of the crosslinking agent decreases, the crosslinking formation of the release coating becomes insufficient, and the viscosity loss during the peeling of the sheet cannot be suppressed, so excessive re-peeling occurs, and the amount of silicone transferred to the adherend also increases.

[0078] The organosilicon (A) containing alkenyl groups and / or Q units in the present invention can be produced by a known method. In addition, the organosilicon (A) containing alkenyl groups and / or Q units in the present invention is preferably contained in the composition in the form of a water dispersion (water dispersion (1)).

[0079] When the above-mentioned organosilicon (A) containing an alkenyl group and / or a Q unit is formed into an aqueous dispersion (aqueous dispersion (1)), the mass % of the above-mentioned organosilicon (A) containing an alkenyl group and / or a Q unit in the above-mentioned aqueous dispersion (1) can be set to, for example, 1 mass % to 50 mass %, or 3 mass % to 40 mass %, 5 mass % to 30 mass %, 10 mass % to 20 mass %, etc.

[0080] (Organic silicon (B) having a hydrogen atom directly bonded to a Si atom represented by a Si—H group)

[0081] As the organosilicon (B) having a hydrogen atom directly bonded to a Si atom represented by a Si—H group (hereinafter sometimes referred to as “organosilicon (B)” or “Si—H group-containing organosilicon (B)”) in the present invention, an organohydrogenpolysiloxane having a structure represented by the following general formula (II) is exemplified.

[0082] R 3 c H d SiO (4-c-d) / 2 ···(II)

[0083] (In formula (II), R 3 It is a monovalent saturated hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group, and c is 0 to 2, d is 1 to 3, and an integer satisfying c+d≤3.

[0084] As R 3Examples of the alkyl groups include methyl, ethyl, propyl, and butyl groups, and examples of the aryl groups include phenyl and tolyl groups. 3 50 mol % or more of the substituents are methyl groups.

[0085] From the viewpoint of curing characteristics, the Si—H group-containing silicone (B) preferably has at least 3, preferably 5 or more hydrogen atoms bonded to Si atoms in one silicone molecule.

[0086] The Si-H group-containing silicone (B) can be produced by a known method. In addition, the Si-H group-containing silicone (B) in the present invention is preferably contained in the composition in the form of a water dispersion (water dispersion (2)).

[0087] When the Si—H group-containing silicone (B) is formed into a water dispersion (water dispersion (2)), the mass % of the Si—H group-containing silicone (B) in the water dispersion (2) can be, for example, 1 mass % to 50 mass %, 3 mass % to 40 mass %, 5 mass % to 30 mass %, 10 mass % to 20 mass %, etc.

[0088] In addition, the content of the Si-H group-containing organosilicon (B) is determined by adding the olefin group and / or SiO 4 / 2 When the total content of the organosilicon (A) and the Si-H group-containing organosilicon (B) of the Q unit shown is 100 parts by mass, it is preferably 1 part by mass or more and 60 parts by mass or less, more preferably 2 parts by mass or more and 50 parts by mass or less, and more preferably 3 parts by mass or more and 45 parts by mass or less. When the content is less than 1 part by mass, the curing reaction is not easy to proceed, so sufficient coating hardness may not be obtained. When the content exceeds 60 parts by mass, Si-H is excessively precipitated on the surface and strongly adheres to the green sheet, so as a result, heavy peeling may occur.

[0089] (Silicone content)

[0090] In the mold release coating composition of the present invention, based on the solid content mass of the above composition, it is preferred that the composition contains alkenyl groups and / or SiO 4 / 2The total amount of the solid content of the organosilicon (A) and the solid content of the Si-H group-containing organosilicon (B) in the Q unit shown is 70% by mass or more. In addition, the more preferred content of each organosilicon solid component is 80% by mass or more and 97% by mass or less. Here, the organosilicon solid component refers to the amount excluding the aqueous solvent, and the solid content mass of the composition refers to the total amount of the solid content of each additive. If the total amount of the above-mentioned organosilicon solid component is less than the lower limit, the area covered by the organosilicon on the surface of the film formed with the coating film becomes smaller, the peeling force becomes heavier, and sometimes the peeling force becomes uneven.

[0091] (Water-based solvent)

[0092] As the aqueous solvent for forming each of the silicone aqueous dispersions of the present invention, water is preferably used. By using an aqueous solvent, the silicone release layer can be formed in the release film production process without using explosion-proof equipment and organic solvent recovery equipment required for organic solvents.

[0093] (Nonionic emulsifier)

[0094] Each aqueous dispersion is prepared using a nonionic emulsifier to improve the stability and shear resistance of the aqueous dispersion. It should be noted that after in-depth research, the inventors determined that in order to prevent the aggregation of each aqueous dispersion and not affect the curing reaction of silicone, the emulsifier must be a nonionic emulsifier. Cationic emulsifiers affect the curing reaction of silicone and exist locally in the coating film, such as seeping out on the surface and affecting the demoulding property, resulting in heavy peeling. In addition, the details are unclear, but when a cationic emulsifier is used, the silicone-based aqueous dispersions become easy to aggregate with each other.

[0095] As nonionic emulsifiers, HLB values ​​preferably range from 6 to 18, and examples thereof include at least one selected from alkylene oxide adducts such as alkylene oxide adducts of higher alcohols and higher fatty acids, esters of alkylene oxide adducts of higher fatty acids and alcohols, alkylene oxide adducts of alkanolamides, alkylene oxide adducts of sorbitan esters, and alkylene oxide adducts of higher fatty acid glycerides. These may be used alone or in combination of two or more. Here, the HLB value is a value calculated according to Griffin's calculation formula.

[0096] As alkylene oxide, for example, ethylene oxide, propylene oxide, and butylene oxide can be mentioned, and one of these can be used or multiple can be used. When using multiple types, regardless of block or random addition forms, the HLB value is preferably in the range of 6 or more and 18 or less, and more preferably in the range of 10 or more and 15 or less. Among these nonionic emulsifiers, for example, polyoxyethylene lauryl ether, polyoxyethylene tridecyl ether, etc. can be preferably mentioned. If a nonionic emulsifier whose HLB value deviates from the above range is used as an emulsifier for an organic silicone aqueous dispersion, the emulsification dispersion power and the stability of the aqueous dispersion are sometimes reduced. The nonionic emulsifier is preferably used in a range of 0.1% by mass or more and 20% by mass or less relative to the total solid content, more preferably in a range of 0.2% by mass or more and 15% by mass or less, and more preferably in a range of 0.5% by mass or more and 10% by mass or less. If it is lower than this range, there is a tendency to be poor at emulsification, and if it is higher than it, it sometimes causes heavy peeling.

[0097] (Platinum catalyst)

[0098] In the release coating composition constituting the coating layer of the present invention, a platinum-based catalyst is required to perform an addition reaction between the at least one organosilicon (A) containing an alkenyl group and / or a Q unit and the Si—H group-containing organosilicon (B).

[0099] As the platinum catalyst, known ones can be used, for example, platinum chloride and chloroplatinic acid. For the above platinum catalyst, in consideration of the dispersibility of the organosilicon, 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (Karstedt catalyst) can be used to disperse the organosilicon at the same time when emulsifying it, thereby ensuring uniform dispersibility. They can be used alone or in combination of two or more.

[0100] The amount of platinum-based catalyst is preferably contained in a range of 10 ppm or more and 800 ppm or less relative to the total amount of 100 parts by mass of the aqueous dispersion (1) of one or more silicones (A) containing alkenyl groups and / or Q units, and the aqueous dispersion (2) of the silicones (B) containing Si-H groups. By setting the above range, the curing of silicone can be fully carried out. In addition, the generation of silicone aggregates can be suppressed, and a release polyester film with excellent surface properties can be obtained. If the mass ratio of the platinum element exceeds the upper limit, the addition reaction of the alkenyl group and the Si-H group is accelerated, and there is a tendency to generate silicone aggregates. From the above viewpoint, the amount of platinum-based catalyst is more preferably 600 ppm or less, further preferably 500 ppm or less, particularly preferably 200 ppm or less, and very preferably 150 ppm or less. In addition, if the mass ratio of the platinum element is lower than the lower limit, the addition reaction does not proceed, and there is a tendency to cause poor curing of silicone. From the above viewpoint, the amount of platinum catalyst is more preferably 15 ppm or more, further preferably 20 ppm or more, particularly preferably 25 ppm or more, and most preferably 40 ppm or more.

[0101] (Cross-linking Reaction Inhibitor)

[0102] In order to suppress the activity of the platinum catalyst at room temperature, it is preferred that a crosslinking reaction inhibitor is contained in the aqueous coating composition. The above-mentioned crosslinking reaction inhibitor is preferably a crosslinking reaction inhibitor with an alkenyl group. As a crosslinking reaction inhibitor with an alkenyl group, as long as there is an alkenyl group, there is no particular limitation, specifically, examples 1-ethynyl-1-cyclohexanol, 4-ethyl-1-octyne-3-ol, 3-methyl-1-dodecyne-3-ol, 3,7,11-trimethyl-1-dodecyne-3-ol, 1,1-diphenyl-2-propyne-3-ol, 3-ethyl-6-ethyl-1-nonyne-3-ol, 3-methyl-1-pentadecane-3-ol, 2,5-dimethyl-3-hexyne-2,5-diol, 3-phenyl-1-butyne-3-ol. They can be used alone, in addition, two or more kinds can also be combined and used. In the present invention, an aqueous emulsion coating composition is used, and therefore, the crosslinking reaction inhibitor having an olefin group and a hydroxyl group as exemplified is preferably used in terms of the balance between affinity solubility for water and coordination ability for platinum and boiling point.

[0103] The content of the cross-linking reaction inhibitor is preferably 5 ppm or more and 1000 ppm or less, more preferably 10 ppm or more and 700 ppm or less, and further preferably 20 ppm or more and 500 ppm or less, relative to the mass of the aqueous coating composition used in the formation of the release layer. When the content of the cross-linking reaction inhibitor is above the lower limit, the pot life becomes longer, the addition curing reaction of the organosilicon at room temperature is not easy to proceed, and there is a tendency that it becomes difficult to produce organosilicon aggregates. In addition, if the content of the cross-linking reaction inhibitor is below the upper limit, the organosilicon becomes difficult to migrate to the object material after the object material is peeled off, and the amount of the reaction inhibitor volatilized during the heat treatment is reduced, so it is not easy to cause contamination inside the oven.

[0104] (Other ingredients)

[0105] The mold release coating composition of the present invention may further contain, for example, an adhesiveness-imparting agent to a substrate, a colorant, an ultraviolet absorber, particles, an antistatic agent, and the like, within a range not impairing the subject matter of the present invention.

[0106] (Preparation of Silicone Aqueous Dispersion)

[0107] When preparing each of the organosilicon aqueous dispersions of the present invention, a method of emulsifying the above-mentioned organosilicon component, aqueous solvent and emulsifier can be cited. These components can be emulsified by a known method, for example, a method of mechanically emulsifying the pre-prepared organosilicon, emulsifier and other components as required in an aqueous medium using a stirring device such as a homogenizer, a vacuum emulsifier, a super planetary mixer, etc.

[0108] The particle size of the aqueous dispersion can be adjusted by adjusting the size of the stirring blade, the stirring speed and the stirring time. The average particle size of each silicone aqueous dispersion of the present invention is preferably 200 nm or less, more preferably 100 nm or more and 200 nm or less.

[0109] 〔Coating layer〕

[0110] In the present invention, a coating layer (release layer) is formed on at least one surface of a polyester film using the release coating composition of the present invention. The coating layer (release layer) of the present invention is formed as follows: the release coating composition is applied to the polyester film and then dried to form a coating layer.

[0111] In the present invention, the coating layer thickness is preferably 5 nm or more and 70 nm or less in terms of thickness after drying. If the coating layer thickness does not reach the lower limit, the demoulding property may become insufficient. If it exceeds the upper limit, the peel strength increases. In addition, the coating liquid must be made into a high concentration or the coating amount must be increased, so there is a tendency to become difficult to coat.

[0112] When applying the demoulding coating composition of the present invention on a polyester film, an aqueous coating liquid comprising the above-mentioned composition is prepared, and the mass of the above-mentioned coating liquid is used as a benchmark, and the solid content concentration of the aqueous coating liquid is preferably below 20% by mass, more preferably above 1% by mass and below 10% by mass. If the solid content concentration in the aqueous coating liquid does not reach the lower limit, the coating property of the polyester film is sometimes insufficient. In addition, if the solid content concentration exceeds the upper limit, the stability of the coating liquid and the appearance of the coating layer are sometimes deteriorated. As an aqueous solvent for adjusting the solid content concentration, water is preferably used.

[0113] The aqueous coating liquid may be applied to the polyester film at any stage, but is preferably applied during the production process of the polyester film, and more preferably applied to the polyester film before the orientation crystallization is completed.

[0114] Here, the polyester film before the crystal orientation is completed includes: unstretched film; uniaxially oriented film oriented in any one of the longitudinal direction (hereinafter, sometimes referred to as the film continuous film forming direction, length direction, MD direction) or transverse direction (hereinafter, sometimes referred to as the direction orthogonal to the longitudinal direction, width direction, TD direction); further oriented by low-ratio stretching in both longitudinal and transverse directions (finally, biaxially stretched film before the orientation crystallization is completed by re-stretching in the longitudinal direction or transverse direction); etc. Among them, it is preferred to apply the aqueous coating liquid of the above-mentioned composition on the unstretched film or the uniaxially stretched film oriented in one direction, and directly perform longitudinal stretching and / or transverse stretching and heat setting, so-called online coating. The coating layer can be dried by the stretching process or heat setting treatment after coating, and a drying process can be further applied as needed. In addition, when the composition is cured with a catalyst to obtain a cured coating, it can be cured by a stretching process or heat setting treatment, but a curing process can be further applied as needed.

[0115] When the aqueous coating liquid is applied to a polyester film, for example, as a pretreatment for improving coating properties, it is preferred to subject the film surface to a physical treatment such as corona surface treatment, flame treatment, or plasma treatment, or to use the above-mentioned emulsifier together with the composition as a wetting agent.

[0116] As the coating method, any known coating method can be applied, for example, roll coating, gravure coating, roll brush coating, spray coating, air knife coating, impregnation, curtain coating, etc. can be used alone or in combination.

[0117] <Method for producing silicone release polyester film>

[0118] The method for producing the silicone release polyester film of the present invention comprises the following steps:

[0119] A coating layer is formed on at least one side of a polyester film using a release coating composition, wherein the release coating composition comprises: a polyol containing an olefin group and / or SiO 4 / 2 An aqueous dispersion (1) of one or more silicones (A) having Q units as shown, an aqueous dispersion (2) of silicones (B) having hydrogen atoms directly bonded to Si atoms as shown by Si-H groups, a crosslinking reaction inhibitor, a platinum-based catalyst, and a nonionic emulsifier,

[0120] The number average molecular weight of the above-mentioned silicone A is 150,000 or more,

[0121] The content of Si atoms contained in the Q unit is in the range of 0.05 mol % or more and 60 mol % or less.

[0122] The method for producing the silicone release polyester film of the present invention can efficiently and simply produce a silicone release polyester film having the above-mentioned properties. It should be noted that the production method shown here is an example, and the present invention is not limited thereto.

[0123] In the above-mentioned production method, the description concerning the above-mentioned silicone release polyester film and the like in this specification can be appropriately applied to each structure.

[0124] As the step of forming a coating layer using the aqueous release coating composition in the above production method, any known method can be appropriately used as long as it is a method of forming a coating layer on a film using the aqueous release coating composition.

[0125] Example

[0126] The present invention is specifically described according to the examples, but the present invention is not limited to the following examples. It should be noted that the physical properties and characteristics in the examples are measured or evaluated by the following methods. In addition, when expressing "parts", it means "parts by mass".

[0127] Each measurement / evaluation in the examples was performed as follows.

[0128] (1) Adhesive tape peelability

[0129] The peel strength of the adhesive tape is the strength obtained by laminating a polyester adhesive tape (manufactured by Nitto Denko Corporation, No. 31B) on the surface of the coating layer (release layer) of the release film, pressing it with a 5 kg pressing roller, leaving it for more than 30 minutes, and then measuring the peel strength between the release layer and the adhesive tape with a peel strength tester (peeling angle 180 degrees, peeling speed 300 mm / min, unit: g / 25 mm width). The peel strength of the silicone release polyester film of the present invention is preferably 20 g / 25 mm or more and 400 g / 25 mm or less.

[0130] (2) Residual bonding rate

[0131] Determine the peel strength after making polyester adhesive tape (made by Nitto Denko, No.31B) adhere to the cold-rolled stainless steel plate (SUS304) specified in JIS G4305, as the basic bonding force (f0). In addition, with a 5kg crimping roller, the above-mentioned polyester adhesive tape is crimped to the release layer surface of the demoulding polyester film, and the adhesive tape is peeled off after maintaining for 30 seconds, and the peel strength after the peeled adhesive tape is adhered to the above-mentioned stainless steel plate is measured as the residual bonding force (f). By the basic bonding force (f0) and residual bonding force (f) obtained, the following formula is used to obtain the residual bonding rate. It should be noted that the peeling angle is set to 180 degrees and the peeling speed is set to 300mm / minute.

[0132] Residual bonding rate (%) = (f) / (f0)×100

[0133] The residual adhesion rate is preferably 90% or more, indicating that the silicone crosslinking density is high. If it is less than 90%, it indicates that the crosslinking is insufficient.

[0134] [Examples 1 to 3, Comparative Examples 1 to 4]

[0135] A molten polyethylene terephthalate ([η]=0.64dl / g, Tg=78°C) containing 0.1% by mass of calcium carbonate particles with an average particle size of 0.7μm was extruded from a die and cooled on a cooling drum according to a conventional method to form an unstretched film. Subsequently, the film was stretched to 3.6 times in the longitudinal direction and then mixed with the components in a manner to obtain a solid content ratio as shown in Table 1 to prepare an aqueous coating solution (aqueous dispersion with a solid content concentration of 3% by mass). The obtained aqueous coating solution was evenly applied to the surface of the film using a roll coater.

[0136] Next, the coated film was dried at 115°C for about 5 seconds and stretched to 4.5 times in the transverse direction at 145°C, and further heat-set at 230°C for about 5 seconds to obtain a 25 μm biaxially stretched polyester film having a coating layer shown in Table 1.

[0137] (Aqueous dispersion of organosilicon (1-a) containing alkenyl groups and Q units)

[0138] A raw material containing 95% by mass of silicone (1) and 5% by mass of polyoxyethylene tridecyl ether (manufactured by Takemoto Oil & Fats Co., Ltd., trade name "NEW KALGEN D-1208") as a surfactant was mechanically emulsified in an aqueous medium using an emulsifier capable of stirring the entire container (manufactured by NPLabo Co., Ltd., device name "Super Planetary Mixer") to obtain an aqueous dispersion of silicone (1-a) having a solid content of 20% by mass. The stirring speed and stirring time during emulsification were adjusted to adjust the emulsion particle size to an average particle size of 200 nm.

[0139] It should be noted that the composition of the organosilicon (1-a) is as follows: comprising R 1 For vinyl, R 2 6.00 mol% of structural units in which only one vinyl group is bonded to silicon directly bonded to a methyl group or a vinyl group, 60.00 mol% of structural units consisting of Q units in which a=b=0 in the formula (I), and 60.00 mol% of structural units consisting of R in the formula (I) 2 The structural unit having a methyl group, a=0, b=2 (a=0, b=3 at both ends) was 34.00 mol%, and the number average molecular weight was adjusted to 240,000 (1-a).

[0140] R 1 a R 2 b SiO (4-a-b) / 2 ···(I)

[0141] (In formula (I), R 1 is an alkenyl group having 2 to 8 carbon atoms, R 2 It is a monovalent saturated hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group, and a is an integer of 0 to 3 and b is an integer of 0 to 3, and satisfies a+b≤3.

[0142] (Aqueous dispersion of alkenyl-containing organosilicon (1-b) not containing Q unit)

[0143] A raw material containing 95% by mass of silicone (1-b) and 5% by mass of polyoxyethylene tridecyl ether (manufactured by Takemoto Oil & Fats Co., Ltd., trade name "NEW KALGEN D-1208") as a surfactant was mechanically emulsified in an aqueous medium using an emulsifier capable of stirring the entire container (manufactured by NPLabo Co., Ltd., device name "Super Planetary Mixer") to obtain an aqueous dispersion of silicone (1-b) having a solid content of 20% by mass. In addition, the stirring speed and stirring time during emulsification were adjusted to adjust the emulsion particle size to an average particle size of 200 nm.

[0144] It should be noted that the composition of the organosilicon (1-b) is as follows: comprising R 1 For vinyl, R 2 The structural units are methyl, vinyl directly bonded to silicon with only one vinyl group bonded, vinyl bonded to terminal silicon atoms, silicon atoms with vinyl bonds repeated three times, and dimethylsiloxane (vinyl groups at both ends). The number average molecular weight is adjusted to 40,000 according to the number of repetitions of the latter structural units.

[0145] (Aqueous dispersion of organosilicon (2) having Si—H groups)

[0146] A raw material containing 97% by mass of Si-H group-containing silicone (2) and 3% by mass of polyoxyethylene tridecyl ether (manufactured by Takemoto Oil & Fats Co., Ltd., trade name "NEW KALGEN D-1208") as a surfactant was mechanically emulsified in an aqueous medium using an emulsifying device capable of stirring the entire container (manufactured by NPLabo Co., Ltd., device name "Super Planetary Mixer") to obtain an aqueous dispersion (2) having a solid content of 10% by mass of Si-H group-containing silicone (2). In addition, the stirring speed and stirring time during emulsification were adjusted to adjust the emulsion particle size to an average particle size of 160 nm.

[0147] R 3 c H d SiO (4-c-d) / 2 ···(II)

[0148] (In formula (II), R 3 It is a monovalent saturated hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group, and c is 0 to 2, d is 1 to 3, and an integer satisfying c+d≤3.

[0149] In addition, the Si-H-containing organic silicon composition is as follows: comprising R 3 The structure unit is a methyl group, c=d=1, i.e., only one hydrogen group is bonded to the silicon to which the hydrogen group is directly bonded, the hydrogen atom is not bonded to the terminal silicon atom, the number of repetitions of the structural unit having the silicon atom to which the hydrogen group is directly bonded is 30, and a structural unit of dimethylsiloxane (methyl groups at both ends), and the number average molecular weight is adjusted to 5000 according to the number of repetitions of the latter structural unit.

[0150] (Silicone coating liquid adjustment)

[0151] As an aqueous coating composition (mold release coating composition), an aqueous dispersion of silicone (1-a) or an aqueous dispersion of silicone (1-b) and an aqueous dispersion of silicone having a Si-H group (2) were mixed in a solid component mixing ratio as shown in Table 1, and 40 ppm of the following platinum-based catalyst was mixed with respect to the total coating liquid mass of silicone (1-a) and silicone (2), and 200 ppm of the following cross-linking reaction inhibitor was mixed with respect to the coating mass. The coating liquid was diluted with water to have a solid content concentration of 40 nm in a dry coating film thickness to prepare a coating liquid.

[0152] · Platinum-based catalyst: platinum-based catalyst emulsion (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "CAT-PM-10A")

[0153] · Cross-linking reaction inhibitor: 1-ethynylcyclohexanol (manufactured by Alfa Lancaster)

[0154] The above formulation and the above results are shown in Table 1. In addition, the numerical value of each silicone represents the mass part of the solid content.

[0155] [Table 1]

[0156]

[0157] As can be seen from Table 1, the films of the embodiments of the present invention have excellent peelability and residual adhesion. This is because, by using a specific structure containing very high molecular weight silicone, a film with excellent peelability and residual adhesion is obtained. On the other hand, in Comparative Example 1, insufficient crosslinking results in heavy peeling. In addition, in Comparative Example 2, the SiH residues in silicone (2) increase, the transfer increases, and the residual adhesion rate decreases. In addition, in Comparative Example 3, insufficient crosslinking results, the transfer of the main agent increases, and the residual adhesion rate decreases. In addition, in Comparative Example 4, the SiH residues in silicone (2) increase, the transfer increases, and the residual adhesion rate decreases.

Claims

1. A silicone release polyester film, comprising a coating layer formed using a release coating composition on at least one side of the polyester film, wherein the release coating composition comprises: 4 / 2 An aqueous dispersion (1) of one or more silicones (A) having Q units as shown, an aqueous dispersion (2) of silicones (B) having hydrogen atoms directly bonded to Si atoms as shown by Si-H groups, a crosslinking reaction inhibitor, a platinum-based catalyst, and a nonionic emulsifier, The number average molecular weight of the organosilicon A is greater than 150,000. The content of Si atoms contained in the Q unit is 0.05 mol % or more and 60 mol % or less.

2. The silicone release polyester film according to claim 1, wherein When the total content of the silicone (A) and the silicone (B) is 100 parts by mass, the content of the silicone (B) is 3 parts by mass or more and 45 parts by mass or less.

3. The silicone release polyester film according to claim 1, wherein: The alkenyl group of the organosilicon (A) is a vinyl group. 4 . The silicone release polyester film according to claim 1 , wherein the release force of the silicone release polyester film after being attached to a polyester adhesive tape is 20 g / 25 mm width or more and 400 g / 25 mm width or less. 5 . The silicone release polyester film according to claim 1 , which is used for molding ceramic green sheets in the production of laminated ceramic capacitors.

6. A method for producing a silicone release polyester film, comprising the steps of: forming a coating layer on at least one side of a polyester film using a release coating composition, wherein the release coating composition comprises: a polyol containing an olefin group and / or SiO 4 / 2 An aqueous dispersion (1) of one or more silicones (A) having Q units as shown, an aqueous dispersion (2) of silicones (B) having hydrogen atoms directly bonded to Si atoms as shown by Si-H groups, a crosslinking reaction inhibitor, a platinum-based catalyst, and a nonionic emulsifier, The number average molecular weight of the organosilicon A is greater than 150,000. The content of Si atoms contained in the Q unit is in the range of 0.05 mol % or more and 60 mol % or less.

7. The manufacturing method according to claim 6, wherein: When the total content of the silicone (A) and the silicone (B) is 100 parts by mass, the content of the silicone (B) is 3 parts by mass or more and 45 parts by mass or less.

8. The manufacturing method according to claim 6 or 7, wherein: The alkenyl group of the organosilicon (A) is a vinyl group.

Citation Information

Patent Citations

  • Release film for manufacturing ceramic sheet

    JP1997001527A

  • Mold releasing film

    JP2005313601A

  • Silicone release polyester film

    JP2013208810A

  • Silicone release polyester film

    JP2014083697A

  • Coating composition for release and silicone-releasable polyester film consisting of the same

    JP2014156560A