Hologram recording medium, method of manufacturing same, and optical element including same

A hologram recording medium with a photopolymer layer of specific elemental composition addresses durability issues in high temperature/high humidity environments, maintaining diffraction efficiency and image stability.

CN119095889APending Publication Date: 2024-12-06LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036119.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-10-05
Filing Date
2023-10-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Hologram recording media used in high temperature/high humidity environments, such as mobile devices and vehicle components, suffer from deformation of diffraction gratings, leading to distorted images or failure of intended functions due to insufficient durability against heat and moisture.

Method used

A hologram recording medium comprising a photopolymer layer with specific elemental ratios of carbon, nitrogen, oxygen, fluorine, and silicon, formed by crosslinking a siloxane-based polymer with a (meth)acrylic polyol, and containing a photoreactive monomer and photoinitiator system, which enhances durability and optical recording characteristics.

Benefits of technology

The medium maintains high diffraction efficiency and stability under varying environmental conditions, preventing deformation of diffraction gratings and ensuring reliable image reproduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095889A_ABST
    Figure CN119095889A_ABST
Patent Text Reader

Abstract

The invention relates to a hologram recording medium, a method for manufacturing the same, and an optical element including the same. According to the present invention, since the hologram recording medium satisfies a specific element ratio, it is not only excellent in optical recording characteristics, but also exhibits excellent durability to heat and moisture, and can exhibit appropriate adhesive force to a transparent adhesive and high transparency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Korean Patent Application No. 10-2022-0146069 filed on November 4, 2022, Korean Patent Application No. 10-2022-0146073 filed on November 4, 2022, and Korean Patent Application No. 10-2023-0132803 filed on October 5, 2023, in the Korean Intellectual Property Office, the disclosures of which are incorporated herein by reference in their entirety.

[0003] The present invention relates to a hologram recording medium, a method for preparing the same, and an optical element comprising the same. Background Art

[0004] The hologram recording medium records information by changing the refractive index of a hologram recording layer in the medium through an exposure process, reads the change in the refractive index in the medium thus recorded, and reproduces the information.

[0005] In this regard, the photopolymer composition can be used to prepare a hologram. The photopolymer can easily store the light interference pattern as a hologram by photopolymerization of the photoreactive monomer. Therefore, the photopolymer can be used in various fields, such as smart devices such as mobile devices, wearable display components, vehicle products (e.g., head-up displays), holographic fingerprint recognition systems, optical lenses, reflectors, deflection mirrors, filters, diffusers, diffraction elements, light guides, waveguides, holographic optical elements with projection screen and / or mask functions, optical storage systems and light diffuser plates, optical wavelength multiplexers, reflective, transmissive color filters, etc.

[0006] Specifically, a photopolymer composition for preparing a hologram comprises a polymer matrix, a photoreactive monomer, and a photoinitiator system, and a photopolymer layer prepared from such a composition is irradiated with laser interference light to cause localized photopolymerization of the monomer.

[0007] The refractive index modulation is generated by the local photopolymerization process, and the diffraction grating is generated by such refractive index modulation. The refractive index modulation value (Δn) is affected by the thickness and diffraction efficiency (DE) of the photopolymer layer, and the angular selectivity increases as the thickness decreases.

[0008] Recently, demands for development of materials capable of maintaining a stable hologram at high diffraction efficiency have increased, and various attempts have been made to prepare a photopolymer layer having high diffraction efficiency and a high refractive index modulation value and a thin thickness.

[0009] On the other hand, when the hologram recording medium is used as an optical element in an application such as a mobile device or a vehicle component (e.g., a head-up display), it is placed in a high temperature / high humidity environment. In such a case, when the diffraction grating is deformed, the image becomes distorted, or the originally intended function may not be performed. Therefore, it is necessary to develop a photopolymer layer and a hologram recording medium including the same, in which the diffraction grating of the photopolymer layer is less deformed despite the heat and moisture of the use environment and has excellent reliability. Summary of the invention

[0010] Technical issues

[0011] According to one embodiment of the present invention, there is provided a hologram recording medium.

[0012] According to another embodiment of the present invention, a method for preparing a hologram recording medium is provided.

[0013] According to still another embodiment of the present invention, there is provided an optical element including a hologram recording medium.

[0014] Technical Solution

[0015] Now, a hologram recording medium, a method for producing the same, an optical element including the same, and the like according to a specific embodiment of the present invention will be described.

[0016] Unless otherwise specifically stated, the term "hologram recording medium" as used herein means a medium on which optical information can be recorded in the entire visible light range and ultraviolet range (e.g., 300 nm to 1200 nm) via an exposure process. Therefore, the hologram recording medium herein may mean a medium on which optical information is recorded, or may mean a medium before recording that is capable of recording optical information. The hologram herein may include all visual holograms, such as on-axis (Gabor) holograms, off-axis holograms, full aperture transfer holograms, white light transmission holograms ("rainbow holograms"), Denisyuk holograms, off-axis reflection holograms, edge-illuminated holograms, or holographic stereograms.

[0017] According to one embodiment of the present invention, a hologram recording medium is provided, which includes a photopolymer layer, wherein the photopolymer layer contains: a polymer matrix or a precursor thereof formed by crosslinking a siloxane-based polymer containing a silane functional group and a (meth)acrylic polyol; a photoreactive monomer and a photoinitiator system or a photopolymer obtained therefrom; and a fluorinated compound, wherein the element ratio of carbon is 50 atomic % to 70 atomic %, the element ratio of nitrogen is 0.01 atomic % to 2 atomic %, the element ratio of oxygen is 15 atomic % to 30 atomic %, the element ratio of fluorine is 3 atomic % to 12 atomic %, and the element ratio of silicon is 3 atomic % to 15 atomic %, based on the total amount of carbon atoms, nitrogen atoms, oxygen atoms, fluorine atoms and silicon atoms on the surface of the photopolymer layer determined by photoelectron spectroscopy.

[0018] Since the hologram recording medium of one embodiment includes a photopolymer layer having a specific element ratio, it is excellent not only in optical recording characteristics which are general physical characteristics of hologram recording media, but also has excellent durability against heat and moisture, adhesion to OCA, and transparency.

[0019] Specifically, the element ratio on the surface of the photopolymer layer can be determined using a photoelectron spectroscopy method called X-ray Photoelectron Spectroscopy (XPS) or Electron Spectroscopy for Chemical Analysis (ESCA). According to the photoelectron spectroscopy method described in the test example described later, the elements found on the surface of the sample to be analyzed can be qualitatively analyzed by full spectrum scanning, and then each found element can be narrowly scanned to determine the element ratio. The element ratio of the photopolymer layer in this article can be understood as the element ratio before recording of the photopolymer layer or the element ratio after recording of the photopolymer layer. The element ratio before recording of the photopolymer layer and the element ratio after recording of the photopolymer layer can be the same within the experimental error range, but in some embodiments, they can be different from each other. That is, even if the element ratio before recording of the photopolymer layer and the element ratio after recording are different from each other outside the error range, the desired effect of the hologram recording medium of an embodiment can be exhibited, as long as the element ratio before recording or the element ratio after recording is within the above range. The carbon element ratio on the surface of the photopolymer layer included in the hologram recording medium of one embodiment can be 50 atomic % or greater, 51 atomic % or greater, 52 atomic % or greater, 53 atomic % or greater, or 54 atomic % or greater, and 70 atomic % or less, 69 atomic % or less, or 68 atomic % or less.

[0020] The nitrogen element ratio on the surface of the photopolymer layer can be 0.01 atomic % or greater, 0.05 atomic % or greater, 0.10 atomic % or greater, or 0.20 atomic % or greater, and 2 atomic % or less, 1.8 atomic % or less, 1.6 atomic % or less, 1.4 atomic % or less, or 1.2 atomic % or less.

[0021] The oxygen element ratio on the surface of the photopolymer layer can be 15 atomic % or greater, 16 atomic % or greater, or 17 atomic % or greater, and 30 atomic % or less, 29 atomic % or less, 28 atomic % or less, 27 atomic % or less, or 26 atomic % or less.

[0022] The fluorine element ratio on the surface of the photopolymer layer may be 3 atomic % or more, or 4 atomic % or more, and 12 atomic % or less, 11 atomic % or less, or 10 atomic % or less.

[0023] The silicon element ratio on the surface of the photopolymer layer may be 3 atomic % or more, 4 atomic % or more, 4.5 atomic % or more, and 15 atomic % or less.

[0024] The ratio of carbon, nitrogen, oxygen, fluorine and silicon is the percentage (atomic %) of the total amount of carbon atoms, nitrogen atoms, oxygen atoms, fluorine atoms and silicon atoms on the surface of the photopolymer layer determined by photoelectron spectroscopy.

[0025] Since the photopolymer layer exhibits the above-mentioned element ratio, it has excellent optical recording properties, excellent durability to heat and moisture, and can exhibit appropriate adhesion to OCA (optically clear adhesive) and transparent optical properties. In particular, if the fluorine element ratio is less than the above range, there may be problems of degradation of the optical recording properties, susceptibility of the layer to heat and moisture, and increased haze. If the fluorine element ratio exceeds the above range, there may be problems of degradation of the optical recording properties and degradation of adhesion to OCA. In addition, if the silicon element ratio is less than the above range, there may be problems of susceptibility of the layer to heat and increased haze, and if the silicon element ratio exceeds the above range, there may be a problem of significant degradation of the optical recording properties.

[0026] A hologram recording medium according to an embodiment of the present invention, a method for producing the same, and an optical element including the hologram recording medium will be described in detail below.

[0027] A hologram recording medium according to one embodiment includes a photopolymer layer comprising: a polymer matrix formed by crosslinking a siloxane-based polymer containing a silane functional group and a (meth)acrylic polyol or a precursor thereof; a photoreactive monomer and a photoinitiator system or a photopolymer obtained therefrom; and a fluorinated compound.

[0028] The photopolymer layer may be a photopolymer layer in a state before recording in which optical information can be recorded, or may be a photopolymer layer in a state in which optical information is recorded.

[0029] A photopolymer layer on which optical information is recorded can be prepared by irradiating object light and reference light onto the photopolymer layer before recording. When the object light and reference light are irradiated onto the photopolymer layer before recording, due to the interference field between the object light and the reference light, the photoinitiator system exists in an inactive state in the destructive interference region, and photopolymerization of the photoreactive monomer does not occur, while in the constructive interference region, photopolymerization of the photoreactive monomer occurs due to the activated photoinitiator system. As the photoreactive monomer is continuously consumed in the constructive interference region, a concentration difference occurs between the photoreactive monomers in the destructive interference region and the constructive interference region. Therefore, the photoreactive monomers in the destructive interference region diffuse into the constructive interference region. At this time, the fluorinated compound, which is a plasticizer, moves in the opposite direction to the photoreactive monomer. Since the photoreactive monomer and the photopolymer formed therefrom have a high refractive index compared to the polymer matrix and the fluorinated compound, a spatial change in the refractive index occurs in the photopolymer layer, and a grating is generated by the spatial refractive index modulation occurring in the photopolymer layer. Such a grating surface acts as a reflective surface that reflects incident light due to the difference in refractive index. When light with the wavelength at the time of recording is incident in the direction of the reference light after recording the hologram, it satisfies the Bragg condition and the light is diffracted in the direction of the original object light, which reproduces the holographic optical information.

[0030] Thus, if the photopolymer layer is in a state before recording, the photopolymer layer may comprise the photoreactive monomer, the photoinitiator and the fluorinated compound in a randomly dispersed form within a polymer matrix or a precursor thereof.

[0031] On the other hand, if the optical information is recorded on a photopolymer layer, the photopolymer layer may contain a polymer matrix, a photopolymer distributed to form a grating, and a fluorinated compound.

[0032] The photopolymer layer is formed of a photopolymer composition comprising: a polymer matrix formed by crosslinking a siloxane-based polymer containing a silane functional group and a (meth)acrylic polyol or a precursor thereof; a photoreactive monomer; a photoinitiator system; and a fluorinated compound.

[0033] The polymer matrix is ​​used as a support for the photopolymer layer and is formed by crosslinking a siloxane-based polymer containing a silane functional group (Si-H) and a (meth) acrylic polyol. Specifically, the polymer matrix is ​​formed by crosslinking a (meth) acrylic polyol with a siloxane-based polymer containing a silane functional group. More specifically, the hydroxyl group of the (meth) acrylic polyol can form a crosslink with the silane functional group of the siloxane-based polymer through a hydrosilylation reaction. The hydrosilylation reaction can proceed rapidly even at a relatively low temperature (e.g., a temperature of about 60° C.) under a Pt-based catalyst. Therefore, a hologram recording medium according to an embodiment of the present invention uses a polymer matrix that can be quickly crosslinked even at a relatively low temperature as a support, thereby being able to improve preparation efficiency and productivity.

[0034] The polymer matrix can enhance the mobility of components (e.g., photoreactive monomers or plasticizers, etc.) contained in the photopolymer layer due to the flexible main chain of the siloxane-based polymer. In addition, the siloxane bond having excellent heat resistance and wet heat resistance characteristics can help ensure the reliability of the photopolymer layer recording optical information and the hologram recording medium including the same.

[0035] The polymer matrix can have a relatively low refractive index, which can be used to enhance the refractive index modulation of the photopolymer layer. For example, the upper limit of the refractive index of the polymer matrix can be 1.53 or less, 1.52 or less, 1.51 or less, 1.50 or less, or 1.49 or less. In addition, the lower limit of the refractive index of the polymer matrix can be, for example, 1.40 or greater, 1.41 or greater, 1.42 or greater, 1.43 or greater, 1.44 or greater, 1.45 or greater, or 1.46 or greater. As used herein, "refractive index" can be a value measured at 25°C using an Abbe refractometer.

[0036] The photopolymer layer includes a polymer matrix formed by crosslinking a siloxane-based polymer and a (meth) acrylic polyol containing a silane functional group, but may include a precursor of an uncrosslinked polymer matrix. At this time, the precursor of the polymer matrix may mean a siloxane-based polymer, a (meth) acrylic polyol, and a Pt-based catalyst.

[0037] The siloxane-based polymer may include, for example, a repeating unit represented by the following Chemical Formula 1 and a terminal group represented by the following Chemical Formula 2.

[0038] [Chemical formula 1]

[0039]

[0040] Wherein, in Chemical Formula 1,

[0041] Plural R 1 and R 2 are the same as or different from each other and are each independently hydrogen, halogen, or an alkyl group having 1 to 10 carbon atoms, and

[0042] n is an integer from 1 to 10,000,

[0043] [Chemical formula 2]

[0044]

[0045] Wherein, in Chemical Formula 2,

[0046] Plural R 11 To R 13 are the same as or different from each other and are each independently hydrogen, halogen, or an alkyl group having 1 to 10 carbon atoms, and

[0047] R is selected from at least one repeating unit among the repeating units represented by Chemical Formula 1 and any one terminal group among the terminal groups represented by Chemical Formula 2. 1 , R 2 and R 11 To R 13 At least one of them is hydrogen.

[0048] In Chemical Formula 2, -(O)- means that when Si of the terminal group represented by Chemical Formula 2 is bonded to the repeating unit represented by Chemical Formula 1, it is bonded through oxygen (O) or directly bonded without oxygen (O).

[0049] As used herein, "alkyl" can be a straight chain alkyl, a branched chain alkyl, or a cyclic alkyl. As a non-limiting example, "alkyl" as used herein can be methyl, ethyl, propyl (e.g., n-propyl, isopropyl, etc.), butyl (e.g., n-butyl, isobutyl, tert-butyl, sec-butyl, cyclobutyl, etc.), pentyl (e.g., n-pentyl, isopentyl, neopentyl, tert-pentyl, 1,1-dimethyl-propyl, 1-ethyl-propyl, 1-methyl-butyl, cyclopentyl, etc.), hexyl (e.g., n-hexyl, 1-methylpentyl, 2-methylpentyl, etc.), cyclopentyl, etc.), cyclopentyl, etc.), methyl butyl, propyl, 1-ethyl-propyl, 1-methyl-butyl, cyclopentyl, etc.), methyl butyl, propyl, 1-methyl-butyl, 1-methyl-pentyl, 1-methyl-butyl ... The invention also includes but is not limited to cyclopentyl, 4-methylpentyl, 3,3-dimethylbutyl, 1-ethyl-butyl, 2-ethylbutyl, cyclopentylmethyl, cyclohexyl, etc.), heptyl (for example, n-heptyl, 1-methylhexyl, 4-methylhexyl, 5-methylhexyl, cyclohexylmethyl, etc.), octyl (for example, n-octyl, tert-octyl, 1-methylheptyl, 2-ethylhexyl, 2-propylpentyl, etc.), nonyl (for example, n-nonyl, 2,2-dimethylheptyl, etc.), and the like.

[0050] In one embodiment, R in Chemical Formula 1 and Chemical Formula 2 1 , R 2 and R 11 To R13 is methyl or hydrogen, and R 1 , R 2 and R 11 To R 13 At least two of them may be hydrogen. More specifically, the siloxane-based polymer may be one in which R 1 and R 2 are each independently methyl and hydrogen, and R 11 To R 13 A compound in which each independently is a methyl group or a hydrogen group (for example, a polymethylhydrogensiloxane whose terminal group is a trimethylsilyl group or a dimethylhydrogensilyl group); wherein some R 1 and R 2 are methyl and hydrogen respectively, and the remaining R 1 and R 2 are all methyl groups, and R 11 To R 13 A compound in which each independently is a methyl group or a hydrogen group (for example, a poly(dimethylsiloxane-co-methylhydrogensiloxane) whose terminal group is a trimethylsilyl group or a dimethylhydrogensilyl group); or a compound in which R 1 and R 2 Both are methyl groups. R 11 To R 13 A compound in which at least one of the terminal groups is hydrogen and the others are each independently methyl or hydrogen (for example, a polydimethylsiloxane in which either or both of the terminal groups are dimethylhydrogensilyl groups).

[0051] As an example, the number average molecular weight (Mn) of the siloxane-based compound may be in the range of 200 to 4,000. Specifically, the lower limit of the number average molecular weight of the siloxane-based polymer may be, for example, 200 or more, 250 or more, 300 or more, or 350 or more, and the upper limit thereof may be, for example, 3,500 or less, 3,000 or less, 2,500 or less, 2,000 or less, 1,500 or less, or 1,000 or less. When the number average molecular weight of the siloxane-based polymer satisfies the above range, the following problems can be prevented, so that the hologram recording medium exhibits excellent optical recording characteristics and moisture and heat resistance: during the crosslinking process with (meth) acrylic polyol at room temperature or higher, the siloxane-based polymer volatilizes and the matrix crosslinking degree decreases, or the siloxane-based polymer has poor compatibility with other components of the photopolymer layer, and thus phase separation occurs between the components.

[0052] The number average molecular weight means the number average molecular weight (unit: g / mol) according to polystyrene determined by the GPC method. In the process of determining the number average molecular weight according to polystyrene measured by the GPC method, known analytical devices, detectors such as refractive index detectors and analytical columns can be used, and commonly used temperature, solvent and flow conditions can be used. Specific examples of measurement conditions can include a temperature of 30° C., a tetrahydrofuran solvent, and a flow rate of 1 mL / min.

[0053] The silane functional group (Si-H) equivalent of the siloxane-based polymer may be, for example, in the range of 30 g / equivalent to 200 g / equivalent. More specifically, the silane functional group (Si-H) equivalent of the siloxane-based polymer may be 50 g / equivalent or greater, 60 g / equivalent or greater, 70 g / equivalent or greater, 80 g / equivalent or greater, or 90 g / equivalent or greater, and 180 g / equivalent or less, or 150 g / equivalent or less.

[0054] As used herein, "equivalent weight of a certain functional group" briefly refers to the number of gram equivalents (also referred to as equivalent weight) expressed in units of g / equivalent, and means a value obtained by dividing the molecular weight (weight average molecular weight, number average molecular weight, etc.) of a molecule or polymer containing the functional group by the number of the functional group. Therefore, as the equivalent value is smaller, the density of the functional group is higher, and as the equivalent value is larger, the density of the functional group is smaller.

[0055] When the silane functional group equivalent of the siloxane-based polymer satisfies the above range, the polymer matrix has an appropriate cross-linking density and thus fully serves as a support, and the mobility of the components contained in the photopolymer layer is improved, which allows the initial refractive index modulation value to be maintained at an excellent level even over time without the problem of boundary surface collapse of the diffraction grating generated after recording, thereby minimizing the reduction in the recording characteristics of the optical information.

[0056] (Meth) acrylic polyol may refer to a polymer in which one or more, specifically two or more, hydroxyl groups are bonded to the main chain or side chain of a (meth) acrylate-based polymer. Unless otherwise specifically stated, "(meth) acrylic" as used herein refers to acrylic and / or methacrylic, which is a term covering all acrylics, methacrylics, or mixtures of acrylics and methacrylics.

[0057] The (meth) acrylic polyol is a homopolymer of a (meth) acrylate-based monomer having a hydroxyl group, a copolymer of two or more types of (meth) acrylate-based monomers having a hydroxyl group, or a copolymer of a (meth) acrylate-based monomer having a hydroxyl group and a (meth) acrylate-based monomer not having a hydroxyl group. Unless otherwise specified, "copolymer" as used herein is a term covering all random copolymers, block copolymers, and graft copolymers.

[0058] The (meth)acrylate-based monomer having a hydroxyl group may include, for example, hydroxyalkyl (meth)acrylate, hydroxyaryl (meth)acrylate, etc., the alkyl group is an alkyl group having 1 to 30 carbon atoms, and the aryl group may be an aryl group having 6 to 30 carbon atoms. In addition, the (meth)acrylate-based monomer not having a hydroxyl group may include, for example, a (meth)acrylate-based monomer, a (meth)acrylate-based monomer, etc., the alkyl group may be an alkyl group having 1 to 30 carbon atoms, and the aryl group may be an aryl group having 6 to 30 carbon atoms.

[0059] As an example, the weight average molecular weight (Mw) of (meth) acrylic polyol can be in the range of 150,000 to 1,000,000. The weight average molecular weight means the weight average molecular weight according to polystyrene measured by the GPC method as described above. For example, the lower limit of the weight average molecular weight can be 150,000 or more, 200,000 or more, or 250,000 or more, and its upper limit can be, for example, 900,000 or less, 850,000 or less, 800,000 or less, 750,000 or less, 700,000 or less, 650,000 or less, 600,000 or less, 550,000 or less, 500,000 or less, or 450,000 or less. When the weight average molecular weight of the (meth)acrylic polyol satisfies the above range, the polymer matrix fully exerts its function as a support, and therefore the recording characteristics of optical information are less reduced even after the use time has passed, and sufficient flexibility is given to the polymer matrix, thereby being able to improve the mobility of components contained in the photopolymer layer (for example, photoreactive monomers or plasticizers, etc.) and minimize the reduction in the recording characteristics of optical information.

[0060] In order to adjust the crosslinking density of the (meth)acrylic polyol through the siloxane-based polymer to a level conducive to ensuring the function of the hologram recording medium, the hydroxyl equivalent of the (meth)acrylic polyol may be adjusted to an appropriate level.

[0061] Specifically, the hydroxyl (-OH) equivalent of the (meth) acrylic polyol may be, for example, in the range of 500 g / equivalent to 3000 g / equivalent. More specifically, the lower limit of the hydroxyl (-OH) equivalent of the (meth) acrylic polyol may be 600 g / equivalent or more, 700 g / equivalent or more, 800 g / equivalent or more, 900 g / equivalent or more, 1000 g / equivalent or more, 1100 g / equivalent or more, 1200 g / equivalent or more, 1300 g / equivalent or more, 1400 g / equivalent or more, 1500 g / equivalent or more, 1600 g / equivalent or more, 1700 g / equivalent or more, or 1750 g / equivalent or more. In addition, the upper limit of the hydroxyl (—OH) equivalent of the (meth)acrylic polyol may be 2900 g / equivalent or less, 2800 g / equivalent or less, 2700 g / equivalent or less, 2600 g / equivalent or less, 2500 g / equivalent or less, 2400 g / equivalent or less, 2300 g / equivalent or less, 2200 g / equivalent or less, 2100 g / equivalent or less, 2000 g / equivalent or less, or 1900 g / equivalent or less.

[0062] When the hydroxyl (-OH) equivalent of the (meth) acrylic polyol satisfies the above range, the polymer matrix has an appropriate cross-linking density and thus fully serves as a support, and the mobility of the components contained in the photopolymer layer is improved, which allows the initial refractive index modulation value to be maintained at an excellent level even over time without the problem of boundary surface collapse of the diffraction grating generated after recording, thereby minimizing the reduction in the recording characteristics of the optical information.

[0063] For example, the glass transition temperature (Tg) of the (meth) acrylic polyol may be in the range of -60°C to -10°C. Specifically, the lower limit of the glass transition temperature may be, for example, -55°C or higher, -50°C or higher, -45°C or higher, -40°C or higher, -35°C or higher, -30°C or higher, or -25°C or higher, and the upper limit thereof may be, for example, -15°C or lower, -20°C or lower, -25°C or lower, -30°C or lower, or -35°C or lower. If the above glass transition temperature range is met, the glass transition temperature may be reduced without significantly reducing the modulus of the polymer matrix, thereby increasing the mobility (fluidity) of other components in the photopolymer composition, and also improving the formability of the photopolymer composition. The glass transition temperature may be measured using known methods such as DSC (Differential Scanning Calorimetry) or DMA (dynamic mechanical analysis).

[0064] The refractive index of the (meth) acrylic polyol may be, for example, 1.40 or more and less than 1.50. Specifically, the lower limit of the refractive index of the (meth) acrylic polyol may be, for example, 1.41 or more, 1.42 or more, 1.43 or more, 1.44 or more, 1.45 or more, or 1.46 or more, and the upper limit thereof may be, for example, 1.49 or less, 1.48 or less, 1.47 or less, 1.46 or less, or 1.45 or less. When the (meth) acrylic polyol has a refractive index within the above range, it may contribute to improving the refractive index modulation. The refractive index of the (meth) acrylic polyol is a theoretical refractive index and may be calculated using the refractive index of the monomer used to prepare the (meth) acrylic polyol (value measured at 25° C. using an Abbe refractometer) and the fraction (molar ratio) of each monomer.

[0065] The (meth)acrylic polyol and the siloxane-based polymer may be included such that a molar ratio (SiH / OH) of a silane functional group (Si—H) of the siloxane-based polymer to a hydroxyl group (—OH) of the (meth)acrylic polyol is 1.5 to 4.

[0066] The molar ratio of the silane functional groups of the siloxane-based polymer to the hydroxyl groups of the (meth)acrylic polyol (hereinafter referred to as SiH / OH molar ratio) can be calculated based on the molar number of the functional groups determined by the weight of each polymer and the corresponding functional group equivalent of each polymer.

[0067] Specifically, the silane functional group equivalent of the siloxane-based polymer is a value obtained by dividing the molecular weight (e.g., number average molecular weight) of the siloxane-based polymer by the number of silane functional groups per molecule, and the hydroxyl equivalent of the (meth)acrylic polyol is a value obtained by dividing the molecular weight (e.g., weight average molecular weight) of the (meth)acrylic polyol by the number of hydroxyl functional groups per molecule. Therefore, if the weight of the siloxane-based polymer is divided by the silane functional group equivalent of the siloxane-based polymer, the number of moles of the silane functional group can be determined, and if the weight of the (meth)acrylic polyol is divided by the hydroxyl equivalent of the (meth)acrylic polyol, the number of moles of the hydroxyl group can be determined. More specifically, looking at Example 3 described below, if the weight of the siloxane-based polymer used in Example 3 (2.6 g) is divided by the silane functional group equivalent of the siloxane-based polymer used in Example 3 (103 g / equivalent), the number of moles of silane functional groups (0.0252 mol) is calculated, and if the weight of the (meth)acrylic polyol used in Example 3 (22.4 g) is divided by the hydroxyl equivalent of the (meth)acrylic polyol used in Example 3 (1802 g / equivalent), the number of moles of hydroxyl groups (0.0124 mol) is calculated. If the number of moles of silane functional groups (0.0252 mol) is divided by the number of moles of hydroxyl groups (0.0124 mol), the SiH / OH molar ratio is determined to be calculated as 2.

[0068] The lower limit of the SiH / OH molar ratio may be, for example, 1.6 or more, 1.7 or more, 1.8 or more, 1.9 or more, or 2.0 or more, and the upper limit thereof may be, for example, 3.9 or less, 3.8 or less, 3.7 or less, 3.6 or less, or 3.5 or less. When the SiH / OH molar ratio range is satisfied, the polymer matrix is ​​cross-linked at an appropriate cross-linking density, thereby improving the mobility of recording components (e.g., photoreactive monomers and plasticizers, etc.) and ensuring excellent optical recording properties, and even if the photopolymer layer is placed in a high temperature / high humidity environment after recording, it can inhibit the migration or deformation of the components in the photopolymer layer and can inhibit the penetration of moisture into the photopolymer layer, thereby exhibiting excellent moisture and heat resistance, etc., and exhibiting transparent optical properties.

[0069] The catalyst based on Pt can be, for example, a Karstedt catalyst, etc. Based on 100 parts by weight of (meth) acrylic polyol, the catalyst based on Pt can be included in an amount of 0.01 to 2 parts by weight. Specifically, based on 100 parts by weight of (meth) acrylic polyol, the catalyst based on Pt can be included in an amount of, for example, 0.01 parts by weight or more, 0.02 parts by weight or more, 0.03 parts by weight or more, 0.04 parts by weight or more, 0.05 parts by weight or more, or 0.06 parts by weight or more, and 1.5 parts by weight or less, 1.0 parts by weight or less, 0.5 parts by weight or less, 0.3 parts by weight or less, 0.2 parts by weight or less, 0.15 parts by weight or less, 0.14 parts by weight or less, 0.13 parts by weight or less, or 0.12 parts by weight or less. When using the catalyst based on Pt in the above amount, the polymer matrix can be crosslinked with an appropriate crosslinking density, thereby showing desired optical recording properties.

[0070] In one example, when the molar ratio of the silane functional group of the siloxane-based polymer used as a cross-linking agent to the hydroxyl group of the (meth)acrylic polyol which is the main component forming the polymer matrix is ​​as high as 1.5 to 4, and the content of the Pt-based catalyst is adjusted to 0.01 to 0.30 parts by weight based on 100 parts by weight of the (meth)acrylic polyol, the polymer matrix has an appropriate cross-linking density so that it can provide a photopolymer layer exhibiting transparent optical properties.

[0071] In addition to the Pt-based catalyst, the precursor of the polymer matrix may optionally also contain a rhodium-based catalyst, an iridium-based catalyst, a rhenium-based catalyst, a molybdenum-based catalyst, an iron-based catalyst, a nickel-based catalyst, an alkali metal or alkaline earth metal-based catalyst, a Lewis acid-based or carbene-based non-metal catalyst.

[0072] On the other hand, in a hologram recording medium of one embodiment, optical information can be recorded by irradiating object light and reference light onto a photopolymer layer. Due to the interference field between the object light and the reference light, photopolymerization of the photoreactive monomer does not occur in the destructive interference region, while photopolymerization of the photoreactive monomer occurs in the constructive interference region. As the photoreactive monomer is continuously consumed in the constructive interference region, a concentration difference occurs between the photoreactive monomers in the destructive interference region and the constructive interference region, and therefore, the photoreactive monomers in the destructive interference region diffuse into the constructive interference region. A diffraction grating is generated by the refractive index modulation thus generated.

[0073] Therefore, the photoreactive monomer may include a compound having a higher refractive index than the polymer matrix to achieve the above-mentioned refractive index modulation. However, all photoreactive monomers are not limited to those having a higher refractive index than the polymer matrix, and at least a portion of the photoreactive monomers may have a higher refractive index than the polymer matrix to achieve a high refractive index modulation value. In one example, the photoreactive monomer may include a monomer having a refractive index of 1.50 or greater, 1.51 or greater, 1.52 or greater, 1.53 or greater, 1.54 or greater, 1.55 or greater, 1.56 or greater, 1.57 or greater, 1.58 or greater, 1.59 or greater, or 1.60 or greater and 1.70 or less.

[0074] The photoreactive monomer may include at least one monomer selected from a monofunctional monomer having one photoreactive functional group and a multifunctional monomer having two or more photoreactive functional groups. The photoreactive functional group may be, for example, a (meth)acryloyl group, a vinyl group, a thiol group, etc. More specifically, the photoreactive functional group may be a (meth)acryloyl group.

[0075] The monofunctional monomer may include, for example, at least one selected from the group consisting of benzyl (meth)acrylate (M1182 with a refractive index of 1.5140, Miwon Specialty Chemical), benzyl 2-phenylacrylate, phenoxybenzyl (meth)acrylate (M1122 with a refractive index of 1.565, Miwon Specialty Chemical), phenol (ethylene oxide) (meth)acrylate (phenol (EO) (meth)acrylate; M140 with a refractive index of 1.516, Miwon Specialty Chemical), phenol (ethylene oxide) 2 (meth)acrylate (phenol (EO) 2 (meth)acrylate; M142 with a refractive index of 1.510, Miwon Specialty Chemical), o-phenylphenol (ethylene oxide) (meth)acrylate (o-phenylphenol (EO) (meth)acrylate; M1142 with a refractive index of 1.577, Miwon Specialty Chemical), phenylthioethyl (meth)acrylate (M1162 with a refractive index of 1.560, Miwon Specialty Chemical), Specialty Chemical), and biphenyl methyl (meth)acrylate.

[0076] The multifunctional monomer may include, for example, at least one selected from the following: bisphenol A (ethylene oxide) 2~10 Di(meth)acrylate (bisphenol A (EO) 2~10(Meth)acrylates; M240 with a refractive index of 1.537, M241 with a refractive index of 1.529, M244 with a refractive index of 1.545, M245 with a refractive index of 1.537, M249 with a refractive index of 1.542, M2100 with a refractive index of 1.516, M2101 with a refractive index of 1.512, Miwon Specialty Chemical), bisphenol A epoxy di(meth)acrylate (PE210 with a refractive index of 1.557, PE2120A with a refractive index of 1.533, PE2120B with a refractive index of 1.534, PE2020C with a refractive index of 1.539, PE2120S with a refractive index of 1.556, Miwon Specialty Chemical), Chemical), bisphenol fluorene di(meth)acrylate (HR6022 with a refractive index of 1.600, HR6040 with a refractive index of 1.600, HR6042 with a refractive index of 1.600, Miwon Specialty Chemical), modified bisphenol fluorene di(meth)acrylate (HR6060 with a refractive index of 1.584, HR6100 with a refractive index of 1.562, HR6200 with a refractive index of 1.530, Miwon Specialty Chemical), tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate (M370 with a refractive index of 1.508, Miwon Specialty Chemical), phenol novolac epoxy (meth)acrylate (SC6300 with a refractive index of 1.525, Miwon Specialty Chemical), Chemical), and cresol novolac epoxy (meth)acrylate (SC6400 with a refractive index of 1.522, SC6400C with a refractive index of 1.522, Miwon Specialty Chemical).

[0077] Based on 100 parts by weight of the polymer matrix, the photopolymer layer may contain the photoreactive monomer in an amount of 50 to 300 parts by weight. For example, the lower limit of the content of the photoreactive monomer may be 50 parts by weight or more, 70 parts by weight or more, 100 parts by weight or more, or 110 parts by weight or more, and the upper limit thereof may be 300 parts by weight or less, 290 parts by weight or less, 280 parts by weight or less, or 270 parts by weight or less. When the above range is met, a photopolymer layer may be provided that exhibits excellent optical recording properties, heat resistance and moisture-heat resistance, high transparency, and has appropriate adhesion to OCA.

[0078] The content of the polymer matrix herein means the total content (weight) of the (meth) acrylic polyol and the siloxane-based polymer forming the matrix. In other words, the content of the polymer matrix means both the content of the polymer matrix formed by crosslinking the (meth) acrylic polyol and the siloxane-based polymer and the content of the partially uncrosslinked polymer matrix precursor.

[0079] The photopolymer layer comprises a photoinitiator system. The photoinitiator system may mean a photoinitiator, or a combination of a photosensitizer and a co-initiator that enables polymerization initiated by light.

[0080] The photopolymer layer may comprise a photosensitizer and a coinitiator as the photoinitiator system.

[0081] As the photosensitizer, a photosensitizing dye may be used. Specifically, the photosensitizing dye may include, for example, at least one selected from the following: a silicon rhodamine compound, anthra(9,1-bc)naphtho(3,2,1-kl)acridine (ceramidonine), derivatives, new methylene blue, thioerythrosine triethylammonium, 6-acetylamino-2-methylceramidonin, eosin, erythrosine, rose red, thionine, basic yellow, chlorinated pinacol cyanol, rhodamine 6G, baking cyanine, ethyl violet, Victoria blue R, azure blue, quinaldine red, crystal violet, brilliant green, basic orange G, darrow red, pyronin Y, basic red 29, pyranose I (pyran Iodide), Safranin O, Cyanine, Methylene Blue, Azure A, and BODIPY.

[0082] In one example, the photosensitizing dye may include a silicon rhodamine compound represented by Chemical Formula 3 below.

[0083] [Chemical formula 3]

[0084]

[0085] Among them, in chemical formula 3,

[0086] R 21 To R 29 are each independently hydrogen, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted aryloxy group having 6 to 30 carbon atoms,

[0087] d and e are each independently an integer from 0 to 3,

[0088] f is an integer from 0 to 5, and

[0089] An - It is an anion.

[0090] As used herein, "substituted or unsubstituted" means that hydrogen or carbon is replaced by another element, wherein hydrogen may be replaced by halogen, hydroxyl, alkyl having 1 to 10 carbon atoms, or alkoxy having 1 to 10 carbon atoms, and carbon (-CH2-) may be replaced by -O- or -CO-.

[0091] In chemical formula 3, R 21 To R 28 Each of them may be independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms. Specifically, in Chemical Formula 3, R 21 To R 28 may be each independently an alkyl group having 1 to 6 carbon atoms. More specifically, in Chemical Formula 3, R 21 To R 28 It may be methyl.

[0092] In Chemical Formula 3, d and e may each independently be an integer from 0 to 2, an integer from 0 to 1, or 0.

[0093] In Chemical Formula 3, f may be an integer of 0 to 5, an integer of 0 to 4, an integer of 0 to 3, an integer of 0 to 2, or an integer of 1 to 2.

[0094] In chemical formula 3, R 29 It may be a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms. Specifically, in Chemical Formula 3, R 29 It may be an alkoxy group having 1 to 6 carbon atoms. More specifically, in Chemical Formula 3, R 29 It may be a methoxy group.

[0095] In Chemical Formula 3, the anion (An - ) may be a halide anion, a cyanide anion, a sulfonate anion, an alkoxy anion having 1 to 30 carbon atoms, a substituted or unsubstituted alkyl sulfonate anion having 1 to 30 carbon atoms, a substituted or unsubstituted aromatic sulfonate anion having 6 to 30 carbon atoms, or a substituted or unsubstituted aromatic borate anion having 6 to 30 carbon atoms.

[0096] Specifically, in Chemical Formula 3, the anion (An -) may be a substituted or unsubstituted alkylsulfonate anion having 1 to 30 carbon atoms, a substituted or unsubstituted aromatic sulfonate anion having 6 to 30 carbon atoms, or a substituted or unsubstituted aromatic borate anion having 6 to 30 carbon atoms.

[0097] More specifically, in Chemical Formula 3, the anion (An - ) may be an alkylsulfonate anion having 2 to 15 carbon atoms in which at least one hydrogen is replaced by fluorine or not, an alkylsulfonate anion having 6 to 30 carbon atoms in which at least one carbon is replaced by -O- or -CO- or not, a phenylsulfonate anion substituted or unsubstituted by methyl, or a substituted or unsubstituted tetraarylborate anion. In one example, in Chemical Formula 3, anion (An - ) may be a dodecylsulfonate anion, a perfluorobutylsulfonate anion, a phenylsulfonate anion, a methylphenylsulfonate anion, or tetraphenylborate anion.

[0098] Based on 100 parts by weight of the polymer matrix, the photopolymer layer may contain a photosensitizing dye in an amount of 0.01 to 10 parts by weight. Specifically, the lower limit of the content of the photosensitizing dye may be, for example, 0.02 parts by weight or more, 0.03 parts by weight or more, or 0.05 parts by weight or more, and the upper limit may be, for example, 5 parts by weight or less. When the above range is met, it is beneficial to exhibit an appropriate polymerization reaction rate and ensure desired optical recording characteristics.

[0099] The coinitiator may be an electron donor, an electron acceptor, or a mixture thereof.

[0100] In one example, the photopolymer composition may include an electron donor as a coinitiator. The electron donor may include, for example, a borate anion represented by the following Chemical Formula 4.

[0101] [Chemical formula 4]

[0102] BX 1 X 2 X 3 X 4

[0103] Wherein, in chemical formula 4, X 1 To X 4 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an alkylaryl group having 7 to 30 carbon atoms, or an allyl group, provided that X 1 To X 4At least one of the groups is not an aryl group.

[0104] When an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an alkylaryl group having 7 to 30 carbon atoms, or an allyl group is substituted, it may be substituted with at least one selected from halogen, a vinyl group, a haloalkyl group having 1 to 5 carbon atoms, and an alkoxy group having 1 to 5 carbon atoms.

[0105] Specifically, X 1 To X 3 may be each independently phenyl, methylphenyl, naphthyl, or methylnaphthyl substituted or unsubstituted by at least one substituent selected from halogen, vinyl, trifluoromethyl, and methoxy, and X 4 The straight chain alkyl group may have 1 to 12 carbon atoms.

[0106] More specifically, the borate anion represented by Chemical Formula 4 may be, for example, at least one selected from the borate anions represented by the following Chemical Formulas 4-1 and 4-2.

[0107] [Chemical formula 4-1]

[0108]

[0109] Among them, in chemical formula 4-1,

[0110] Each R 102 are independently methyl or halogen,

[0111] Each R 103 are independently hydrogen, methyl, or halogen, provided that if the adjacent R 102 If R is methyl, 103 is a halogen, and

[0112] X 4 ' is a straight chain alkyl group having 1 to 12 carbon atoms,

[0113] [Chemical formula 4-2]

[0114]

[0115] Among them, in chemical formula 4-2,

[0116] Each R 106 are independently hydrogen, methyl, or halogen, and

[0117] X 4 " is a straight chain alkyl group having 1 to 12 carbon atoms.

[0118] In Chemical Formula 4-2, each R 106may independently be hydrogen, methyl, or halogen, provided that at least one of them may be halogen.

[0119] When the borate anions represented by the following Chemical Formulas 4-1 and 4-2 are used as electron donors, excellent heat resistance can be ensured even before recording.

[0120] In Chemical Formulas 4-1 and 4-2, the halogen may be fluorine or chlorine, of which chlorine can ensure more excellent heat resistance.

[0121] The cation bonded to the borate anion does not absorb light, and may be at least one cation selected from an alkali metal cation, a quaternary ammonium cation, and a nitrogen-containing heterocyclic cation.

[0122] The alkali metal cation may be, for example, at least one selected from the group consisting of lithium, sodium, potassium, rubidium, and cesium.

[0123] The quaternary ammonium cation may be an ammonium cation in which nitrogen (N) is substituted with four substituents, or a cyclic ammonium cation in which two substituents substituted on nitrogen are linked to each other, or a mixture thereof.

[0124] Specifically, the quaternary ammonium cation may be a cation represented by the following Chemical Formula 4-3.

[0125] [Chemical formula 4-3]

[0126] NY 1 Y 2 Y 3 Y 4

[0127] Among them, in chemical formula 4-3, Y 1 To Y 4 The two substituents in may not be bonded to each other or may be bonded to each other to form an aliphatic ring having 4 to 10 carbon atoms, and

[0128] Y that does not form an aliphatic ring 1 To Y 4 each independently is an alkyl group having 1 to 40 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 6 to 40 carbon atoms, or an alkyl group having 2 to 40 carbon atoms connected by an ester bond (e.g., -CH2CH2-O-CO-CH2CH2CH3, etc.),

[0129] The condition is that Y is not included 1 To Y 4 The case where all are methyl groups or two or more substituents are alkyl groups having 16 or more carbon atoms.

[0130] In chemical formula 4-3, if Y 1 To Y 4If all are methyl groups, or two or more substituents are alkyl groups having 16 or more carbon atoms, the electron donor may not be well dissolved in the photopolymer composition and thus may not exhibit desired optical recording characteristics.

[0131] Specifically, in Y 1 To Y 4 In the above formula (A), two substituents may be linked to each other to form a piperidine or a pyrrolidine.

[0132] In Y 1 To Y 4 In the above, the substituents not forming an aliphatic ring may each independently be a linear alkyl group having 1 to 32 carbon atoms, a phenyl group, a benzyl group, or -CH2CH2-O-CO-CH2CH2CH3. More specifically, in Y 1 To Y 4 In the above, the substituents not forming an aliphatic ring may each independently be a methyl group, a butyl group, a hexadecyl group, a hexadecyl group, a phenyl group, or a benzyl group.

[0133] The nitrogen-containing heterocyclic cation may be a heteroaromatic ring cation containing one or more nitrogen. Examples of such heteroaromatic ring cations include pyrrole cations, pyrazolium cations, imidazolium cations, or pyridinium cations, and their hydrogen may be substituted or unsubstituted.

[0134] In one example, the nitrogen-containing heterocyclic cation may be a cation represented by the following Chemical Formula 4-4.

[0135] [Chemical formula 4-4]

[0136]

[0137] In the chemical formula 4-4, R 107 , R 109 and R 110 each independently represents hydrogen, an alkyl group having 1 to 40 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 6 to 40 carbon atoms, or an alkyl group having 2 to 40 carbon atoms connected by an ester bond (e.g., -CH2CH2-O-CO-CH2CH2CH3, etc.), and

[0138] R 108 and R 111 Each is independently an alkyl group having 1 to 40 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 6 to 40 carbon atoms, or an alkyl group having 2 to 40 carbon atoms connected by an ester bond (e.g., -CH2CH2-O-CO-CH2CH2CH3, etc.).

[0139] Specifically, R 107 , R109 and R 110 may each independently be hydrogen or an aryl group having 6 to 30 carbon atoms. More specifically, R 107 , R 109 and R 110 Each may independently be hydrogen or phenyl.

[0140] Specifically, R 108 and R 111 It may be a linear alkyl group having 1 to 40 carbon atoms or an aryl alkyl group having 6 to 40 carbon atoms. More specifically, R 108 and R 111 It may be hexadecyl or benzyl.

[0141] The cation bonded to the borate anion may include, for example, at least one selected from the group consisting of a tetrabutylammonium cation, a hexadecyldimethylbenzylam ...benzylammonium cation, a hexadecylbenzylammonium cation, a hexadecylbenzylammonium cation, a Cationic, hexadecylbenzylpyrrolidine Cation, 1-hexadecyl-3-benzylimidazole Cation and 1,3-dihexadecyl-2-phenylimidazole cation.

[0142] However, the cations bonded to the borate anion are not limited to the above cations, and even if they exhibit poor solubility when contained alone, some of the above cations may be replaced with other cations known in the art as long as they can exhibit sufficient solubility when mixed with the above cations. As a non-limiting example, some of the above cations may be replaced with 1,2-dicyclohexyl-4,4,5,5-tetramethylbiguanide. etc. as an alternative.

[0143] In one example, the photopolymer layer may include an electron acceptor as a co-initiator. The electron acceptor may include, for example: Salt, such as Salt and iodine salt; a triazine compound such as tris(trihalomethyl)triazine, substituted bis(trihalomethyl)triazine, etc.; or a mixture thereof.

[0144] In one example, the electron acceptor may include iodine (4-(Octyloxy)phenyl)(phenyl)iodide Salts, or 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine as a triazine compound. Examples of electron acceptors include commercially available H-Nu 254 (Spectra Group) or 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine (TCI America).

[0145] The photopolymer layer may contain the coinitiator in a range of 0.05 to 10 parts by weight based on 100 parts by weight of the polymer matrix. Specifically, the lower limit of the content of the coinitiator may be, for example, 0.1 parts by weight or more, 0.5 parts by weight or more, 1 part by weight or more, 1.5 parts by weight or more, or 2 parts by weight or more, and the upper limit thereof may be, for example, 5 parts by weight or less. When the above range is met, it is beneficial to exhibit an appropriate polymerization reaction rate and ensure desired optical recording characteristics.

[0146] The photoinitiator system may contain an additional photoinitiator to remove the color of the photosensitive dye and react all unreacted photoreactive monomers after the light irradiation for recording. The photoinitiator may include, for example, imidazole derivatives, bisimidazole derivatives, N-arylglycine derivatives, organic azide compounds, titanocene, aluminate complexes, organic peroxides, N-alkoxypyridines, salts, thioxanthone derivatives, amine derivatives, diazonium salts, Salt, iodine Salts, sulfonates, imide sulfonates / salts, dialkyl-4-hydroxy Salt, arylsulfonic acid p-nitrobenzyl ester, silanol-aluminum complex, (η6-phenyl)(η5-cyclopentadienyl) iron (II), benzoin toluenesulfonate / salt, 2,5-dinitrobenzyl toluenesulfonate / salt, N-toluenesulfonylphthalimide, or a mixture thereof. More specifically, the photoinitiator may include 1,3-di(tert-butyldioxycarbonyl)benzophenone, 3,3',4,4"-tetra(tert-butyldioxycarbonyl)benzophenone, 3-phenyl-5-isobutylenesulfonate, 1,3-di(tert-butyldioxycarbonyl)benzophenone, 1,3',4,4"-tetra ... oxazolidinone, 2-mercaptobenzimidazole, bis(2,4,5-triphenyl)imidazole, 2,2-dimethoxy-1,2-diphenylethane-1-one (product name: Irgacure 651 / manufacturer: BASF), 1-hydroxy-cyclohexyl-phenyl-ketone (product name: Irgacure 184 / manufacturer: BASF), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 (product name: Irgacure 369 / manufacturer: BASF), bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium (product name: Irgacure 784 / manufacturer: BASF), Ebecryl P-115 (manufacturer: SK Entis), Cyracure UVI-6970, Cyracure UVI-6974, Cyracure UVI-6990 (manufacturer: Dow Chemical Co., USA), Irgacure 264, Irgacure 250 (manufacturer: BASF), CIT-1682 (manufacturer: Nippon Soda), or a mixture thereof, but not limited thereto.

[0147] Based on 100 parts by weight of the polymer matrix, the photopolymer layer may contain a photoinitiator in a range of 0.05 parts by weight to 10 parts by weight. Specifically, the lower limit of the content of the photoinitiator may be, for example, 0.1 parts by weight or more, 0.5 parts by weight or more, 1 part by weight or more, 1.5 parts by weight or more, or 2 parts by weight or more, and the upper limit thereof may be, for example, 5 parts by weight or less. If the above range is met, after recording optical information on the photopolymer layer, the reaction of the photoreactive monomer is effectively terminated, and the color of the photosensitive dye is decolorized, thereby providing a transparent hologram recording medium.

[0148] The photopolymer layer may contain a fluorinated compound as a plasticizer. The plasticizer can more easily achieve refractive index modulation when recording a hologram recording medium. More specifically, the plasticizer reduces the glass transition temperature of the polymer matrix, improves the mobility of the photoreactive monomer, and has low refractive index and non-reactive properties. Therefore, when the photoreactive monomer that is uniformly distributed in the polymer matrix but not photopolymerized moves, it can move in the opposite direction of the plasticizer and contribute to refractive index modulation. In addition, the plasticizer can also help improve the formability of the photopolymer composition.

[0149] The fluorinated compound may have a low refractive index of 1.45 or less to perform the above-mentioned plasticizer function. Specifically, the upper limit of the refractive index may be, for example, 1.44 or less, 1.43 or less, 1.42 or less, 1.41 or less, 1.40 or less, 1.40 or less, 1.39 or less, 1.38 or less, or 1.37 or less, and the lower limit of the refractive index may be, for example, 1.30 or more, 1.31 or more, 1.32 or more, 1.33 or more, 1.34 or more, or 1.35 or more. Due to the use of a fluorinated compound having a lower refractive index than the above-mentioned photoreactive monomer, the refractive index of the polymer matrix can be further reduced, and the refractive index modulation of the photoreactive monomer can be made greater.

[0150] The fluorinated compound may include, for example, two or more difluoromethylene groups and at least one functional group selected from an ether group, an ester group, and an amide group. More specifically, the fluorinated compound may be, for example, a compound containing a repeating unit represented by the following Chemical Formula 5.

[0151] [Chemical formula 5]

[0152]

[0153] Among them, in chemical formula 5,

[0154] Plural R 31 To R 34 are each independently hydrogen or fluorine, provided that R 31 To R 34 At least one of is fluorine, and m is an integer from 2 to 12.

[0155] More specifically, the fluorinated compound may be a compound containing 1 to 3 units represented by the following Chemical Formula 5-1.

[0156] [Chemical formula 5-1]

[0157]

[0158] Among them, in chemical formula 5-1,

[0159] R 41 To R 44 and R 53 To R 56 are each independently hydrogen or fluorine, and R 45 To R 52 For fluorine.

[0160] In one example, in Chemical Formula 5-1, R 41 , R 42 , R 55 and R 56 is hydrogen, and R43 To R 54 For fluorine.

[0161] The fluorinated compound containing the (repeating) unit represented by chemical formula 5 and 5-1 is not particularly limited, but can be capped with a capping agent widely used in the relevant technical field. In one example, the end of the fluorinated compound containing the (repeating) unit represented by chemical formula 5 and 5-1 can be an alkyl group or an alkyl group substituted with at least one alkoxy group. As a non-limiting example, 2-methoxyethoxymethyl chloride is used as a capping agent, and therefore, the end of the fluorinated compound containing the (repeating) unit represented by chemical formula 5 and 5-1 can be 2-methoxyethoxymethyl.

[0162] The weight average molecular weight of the fluorinated compound can be 300 or more. Specifically, the lower limit of the weight average molecular weight of the fluorinated compound can be, for example, 350 or more, 400 or more, 450 or more, 500 or more, or 550 or more, and its upper limit can be, for example, 1000 or less, 900 or less, 800 or less, 700 or less, or 600 or less. Considering refractive index modulation, compatibility with other components, outflow problems of fluorinated compounds, etc., it is preferred to meet the above weight average molecular weight range. At this time, the weight average molecular weight means the weight average molecular weight according to polystyrene measured by the GPC method as described above.

[0163] Based on 100 parts by weight of the polymer matrix, the photopolymer layer may contain 20 to 200 parts by weight of the fluorinated compound. Specifically, the lower limit of the content of the fluorinated compound may be, for example, 25 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, 60 parts by weight or more, or 70 parts by weight or more, and the upper limit thereof may be, for example, 190 parts by weight or less, 180 parts by weight or less, 170 parts by weight or less, 160 parts by weight or less, or 155 parts by weight or less. When the above range is met, it can show a large refractive index modulation value after recording due to the fluorinated compound having a sufficiently low refractive index, without deteriorating the compatibility with the components contained in the photopolymer layer, some fluorinated compounds flowing out to the surface of the photopolymer layer, or deteriorating the haze, so this is conducive to ensuring excellent optical recording characteristics.

[0164] The major component of photopolymer layer can be said to be polymer matrix, photoreactive monomer and fluorinated compound.Therefore, the element ratio on the surface of photopolymer layer can be controlled by the mixing ratio of polymer matrix, photoreactive monomer and fluorinated compound.Based on the gross weight of polymer matrix, photoreactive monomer and fluorinated compound, photopolymer layer can comprise 17 wt % to 38 wt % of polymer matrix, 36 wt % to 58 wt % of photoreactive monomer and 17 wt % to 38 wt % of fluorinated compound, to meet the above-mentioned element ratio.

[0165] More specifically, the polymer matrix can be included in an amount of, for example, 17 wt % or more, 18 wt % or more, 19 wt % or more, or 20 wt % or more and 38 wt % or less, 37 wt % or less, or 36 wt % or less. The photoreactive monomer can be included in an amount of, for example, 36 wt % or more, 37 wt % or more, or 38 wt % or more and 58 wt % or less, 55 wt % or less, or 53 wt % or less. The fluorinated compound can be included in an amount of, for example, 17 wt % or more, 18 wt % or more, 19 wt % or more, or 20 wt % or more and 38 wt % or less, 35 wt % or less, 33 wt % or less, or 32 wt % or less. Within this range, a photopolymer layer satisfying the above-mentioned element ratio can be provided.

[0166] The photopolymer layer may also contain additives, such as surfactants or defoamers.

[0167] The photopolymer layer may include a silicone-based surfactant, a fluorine-based surfactant, or a mixture thereof as a surfactant.

[0168] As silicone-based surfactants, for example, BYK-077, BYK-085, BYK-300, BYK-301, BYK-302, BYK-306, BYK-307, BYK-310, BYK-320, BYK-322, BYK-323, BYK-325, BYK-330, BYK-331, BYK-333, BYK-334, BYK-335, BYK-336, BYK-337, BYK-338, BYK-339, BYK-340, BYK-341, BYK-342, BYK-343, BYK-344, BYK-345, BYK-346, BYK-347, BYK-348, BYK-349, BYK-350, BYK-351, BYK-352, BYK-353, BYK-354, BYK-355, BYK-356, BYK-357, BYK-358, BYK-359, BYK-360, BYK-361, BYK-362, BYK-363, BYK-364, BYK-365, BYK-366, BYK-367, BYK-368, BYK-369, BYK-369 YK-335, BYK-341v344, BYK-345v346, BYK-348, BYK-354, BYK355, BYK-356, BYK-358, B YK-361, BYK-370, BYK-371, BYK-375, BYK-380, BYK-390, BYK-3550 (manufactured by BYKChemie), etc. As fluorine-based surfactants, F-114, F-177, F-410, F-411, F-450, F-493, F-494, F-443, F-444, F-445, F-446, F-470, F-471, F-472SF, F-474, F-475, F-477, F-478, F-479, F-480SF, F-482, F-483, F-484, F-486, F-487, F-172D, MCF-350SF, TF-1025SF, TF-1117SF, TF-1026SF, TF-1128, TF-1127, TF1129, TF-1126, TF-1130, TF-1116SF, TF-1131, TF1132, TF1027SF, TF-1441, TF-1442 (manufactured by Dai Nippon Ink & Chemicals), etc.

[0169] If the photopolymer layer contains a surfactant, the surfactant may be contained in an amount of 0.01 parts by weight or more, 0.02 parts by weight or more, 0.03 parts by weight or more, or 0.05 parts by weight or more, and 5 parts by weight or less, or 3 parts by weight or less, based on 100 parts by weight of the polymer matrix. When the above range is satisfied, it can impart excellent adhesion and release properties to the photopolymer layer, and thus maintain excellent optical recording properties.

[0170] The photopolymer layer may contain a silicone-based reactive additive as a defoaming agent. As the silicone-based reactive additive, for example, a commercially available product such as Tego Rad 2500 may be used. The content of the defoaming agent may be appropriately adjusted to a level that does not hinder the function of the hologram recording medium.

[0171] The photopolymer layer may be formed of a photopolymer composition including a solvent.

[0172] The solvent may be an organic solvent, and examples thereof may be at least one organic solvent selected from ketones, alcohols, acetates, and ethers, but are not limited thereto. Specific examples of such organic solvents include at least one selected from the following: ketones such as methyl ethyl ketone, methyl isobutyl ketone, acetylacetone, or isobutyl ketone; alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, or tert-butanol; acetates such as ethyl acetate, isopropyl acetate, or polyethylene glycol monomethyl ether acetate; and ethers such as tetrahydrofuran or propylene glycol monomethyl ether.

[0173] The organic solvent may be added at a point in time when the respective components included in the photopolymer composition are mixed, or may be contained in the photopolymer composition when the respective components are added in a state of being dispersed or mixed in the organic solvent.

[0174] Photopolymer composition can include solvent so that solid content concentration is 1 wt % to 90 wt %. Specifically, photopolymer composition can include solvent so that solid concentration is 20 wt % or more, 25 wt % or more, or 30 wt % or more, and 50 wt % or less, 45 wt % or less, or 40 wt % or less. Within this range, photopolymer composition shows suitable fluidity and can form a coating layer without defects (such as stripes). Defects will not occur during drying and curing process, and therefore a photopolymer layer showing desired physical properties and surface characteristics can be formed.

[0175] The hologram recording medium of one embodiment has excellent refractive index modulation, diffraction efficiency, and driving reliability despite having a thin thickness of the photopolymer layer.

[0176] The thickness of the photopolymer layer may be, for example, in the range of 5.0 μm to 40.0 μm. Specifically, the lower limit of the thickness of the photopolymer layer may be, for example, 6 μm or more, 7 μm or more, 8 μm or more, or 9 μm or more. In addition, the upper limit of the thickness may be, for example, 35 μm or less, 30 μm or less, 29 μm or less, 28 μm or less, 27 μm or less, 26 μm or less, 25 μm or less, 24 μm or less, 23 μm or less, 22 μm or less, 21 μm or less, 20 μm or less, 19 μm or less, or 18 μm or less.

[0177] The hologram recording medium according to one embodiment of the present invention may further include a substrate on at least one surface of the photopolymer layer. The type of substrate is not particularly limited, and those known in the relevant technical field may be used. For example, a substrate such as glass, PET (polyethylene terephthalate), TAC (triacetyl cellulose), PC (polycarbonate) or COP (cycloolefin polymer) may be used.

[0178] A hologram recording medium according to one embodiment of the present invention can have a high diffraction efficiency. In one example, the hologram recording medium can have a diffraction efficiency of 80% or more when recording a notch filter hologram. Wherein, the thickness of the photopolymer layer can be, for example, 5μm to 30μm. Specifically, when recording a notch filter hologram, the diffraction efficiency can be 85% or more, 90% or more, 91% or more, 92% or more, 93% or more, 94% or more, 95% or more, or 96% or more. In this way, a hologram recording medium according to one embodiment of the present invention can achieve excellent diffraction efficiency even if it includes a photopolymer layer of a thin thickness. The diffraction efficiency can be measured by the method described in the test example described below.

[0179] A hologram recording medium of one embodiment includes a photopolymer layer satisfying a specific element ratio, and thus can exhibit resistance to heat and / or moisture.

[0180] In one example, the hologram recording medium of one embodiment may have a diffraction efficiency variation value (ΔDE) of 10% or less, which is calculated by the following Equation 2.

[0181] [Equation 2]

[0182] ΔDE(%)={(|DE0-DE1|) / DE0}×100

[0183] Wherein, in Equation 2, DE0 is the diffraction efficiency measured on the hologram recording medium in which the notch filter hologram is recorded after the hologram recording medium before recording is stored in a dark room under constant temperature and humidity conditions of 20°C to 25°C and 40RH% to 50RH%, and DE1 is the diffraction efficiency measured on the hologram recording medium in which the notch filter hologram is recorded after the hologram recording medium before recording is stored in a dark room under high temperature conditions of 60°C to 70°C and 40RH% to 50RH%.

[0184] The diffraction efficiency change value is an indicator that can evaluate the thermal durability (heat resistance) of the hologram recording medium before recording. As the thermal durability is higher, the diffraction efficiency change value (ΔDE) calculated by Equation 2 can be smaller. For a more specific measurement method of the diffraction efficiency change value (ΔDE) calculated by Equation 2, refer to the method described in the test example described later. The diffraction efficiency change value may be 9% or less, 8% or less, 7% or less, 6% or less, 5% or less, 4% or less, 3% or less, or 2% or less.

[0185] The hologram recording medium of one embodiment can show excellent durability not only to heat but also in a high temperature and high humidity environment. Specifically, in the hologram recording medium of one embodiment, the degree of displacement (Δλ) of the wavelength showing the maximum reflectivity before and after being placed at a temperature of 60°C and a relative humidity of 90% can appear in the range of -10nm to 10nm.

[0186] The degree of displacement (Δλ) of the wavelength showing the maximum reflectivity is an indicator that can evaluate the durability (wet heat resistance) of the hologram recording medium to heat and moisture after recording, and as the durability to heat and moisture is higher, the value of the wavelength displacement degree can be smaller. For a more specific measurement method of the degree of displacement (Δλ) of the wavelength showing the maximum reflectivity, refer to the method described in the test example described later. The degree of displacement (Δλ) of the wavelength showing the maximum reflectivity before and after being placed under high temperature and high humidity conditions can be -10nm to 10nm, -9nm to 9nm, -8nm to 8nm, -7nm to 7nm, -6nm to 6nm, -5nm to 5nm, -4nm to 4nm, -3nm to 3nm, or -2nm to 2nm.

[0187] The hologram recording medium of one embodiment can show appropriate adhesion to an optically clear adhesive (OCA). Specifically, the adhesion of the photopolymer layer to the OCA can be 1000gf / 25mm or greater. For the method of measuring the adhesion, refer to the method described in the test example described later. The adhesion of the photopolymer layer to the OCA can be 1010gf / 25mm or greater, 1030gf / 25mm or greater, or 1100gf / 25mm or greater. The upper limit of the adhesion of the photopolymer layer to the OCA is not particularly limited, but can be 3000gf / 25mm or less.

[0188] On the other hand, since the hologram recording medium uses a mixture of a component having a low refractive index and a component having a high refractive index to record optical properties, it tends to have opaque properties due to their compatibility. However, since the hologram recording medium of one embodiment includes a photopolymer layer satisfying a specific element ratio, it exhibits highly transparent optical properties.

[0189] In one example, the haze of the hologram recording medium may be 3% or less. The upper limit of the haze may be, for example, 2.5% or less, 2.0% or less, 1.9% or less, 1.8% or less, 1.7% or less, 1.6% or less, 1.5% or less, 1.4% or less, 1.3% or less, 1.2% or less, 1.1% or less, 1.0% or less, or 0.9% or less. The lower limit of the haze is not particularly limited and may be 0% or more. The haze may be measured, for example, by the method described in the test example described later.

[0190] The hologram recording medium of still another embodiment exhibits excellent optical recording characteristics, resistance to moist heat, and highly transparent optical characteristics, and is therefore expected to provide various optical elements even in an environment with high heat or high humidity.

[0191] The hologram recording medium of one embodiment is not limited thereto but may be a medium on which a reflection hologram or a transmission hologram is recorded.

[0192] On the other hand, according to another embodiment of the present invention, a method for preparing a hologram recording medium is provided, which includes the following steps: applying a photopolymer composition to form a photopolymer layer, wherein the photopolymer composition includes a polymer matrix or a precursor thereof formed by crosslinking a siloxane-based polymer containing a silane functional group and a (meth)acrylic polyol, a fluorinated compound, a photoreactive monomer, and a photoinitiator system; and irradiating a predetermined area of ​​the photopolymer layer with coherent laser light and selectively polymerizing the photoreactive monomer contained in the photopolymer layer to record optical information, wherein based on the total amount of carbon atoms, nitrogen atoms, oxygen atoms, fluorine atoms and silicon atoms on the surface of the photopolymer layer determined by photoelectron spectroscopy, the element ratio of carbon is 50 atomic % to 70 atomic %, the element ratio of nitrogen is 0.01 atomic % to 2 atomic %, the element ratio of oxygen is 15 atomic % to 30 atomic %, the element ratio of fluorine is 3 atomic % to 12 atomic %, and the element ratio of silicon is 3 atomic % to 15 atomic %.

[0193] The photopolymer layer having the specific element ratio may be the photopolymer layer included in the hologram recording medium of the above-mentioned embodiment, and the photopolymer layer has been previously described in detail, and thus a detailed description thereof is omitted here.

[0194] In the step of forming the photopolymer layer, a photopolymer composition including the above-mentioned configuration may be first prepared. When preparing the photopolymer composition, in order to mix the components, a known mixer, a stirrer, a mixer, etc. may be used without particular limitation. In addition, such a mixing process may be performed at a temperature ranging from 0° C. to 100° C., a temperature ranging from 10° C. to 80° C., or a temperature ranging from 20° C. to 60° C.

[0195] In the step of forming the photopolymer layer, the prepared photopolymer composition may be applied to form a coating layer formed of the photopolymer composition. The coating layer may be dried at a temperature of 50° C. or higher, 55° C. or higher, 60° C. or higher, 65° C. or higher, or 70° C. or higher and 120° C. or lower, 110° C. or lower, 100° C. or lower, or 90° C. or lower. Through this process, a hydrosilylation reaction between the hydroxyl group of the (meth) acrylic polyol remaining unreacted and the silane functional group of the siloxane-based polymer may be caused, thereby achieving a desired crosslinking density while maintaining high transparency.

[0196] In the photopolymer layer prepared by the step of forming the photopolymer layer, the fluorinated compound, the photoreactive monomer and the photoinitiator system and additives added as needed may be uniformly dispersed in a cross-linked polymer matrix.

[0197] Subsequently, in the step of recording optical information, if coherent laser light is irradiated onto the photopolymer layer, polymerization of the photoreactive monomer occurs in the region where constructive interference occurs to form a photopolymer, and polymerization of the photoreactive monomer does not occur or is suppressed in the region where destructive interference occurs, so that the photoreactive monomer exists. In addition, when the unreacted photoreactive monomer causes refractive index modulation while diffusing toward the photopolymer side where the concentration of the photoreactive monomer is lower, a diffraction grating is generated by the refractive index modulation. Thus, a hologram (i.e., optical information) is recorded on the photopolymer layer having the diffraction grating.

[0198] The method for preparing a hologram recording medium according to still another embodiment of the present invention may further include a photobleaching step by irradiating light onto the entire photopolymer layer on which the optical information is recorded, after the step of recording the optical information.

[0199] In the photobleaching step, ultraviolet rays are irradiated onto the photopolymer layer on which the optical information is recorded to terminate the reaction of the photoreactive monomers remaining in the photopolymer layer, thereby removing the color of the photosensitizing dye. In one example, in the photobleaching step, ultraviolet rays (UVA) in the range of 320 nm to 400 nm are irradiated to terminate the reaction of the photoreactive monomers and remove the color of the photosensitizing dye.

[0200] On the other hand, according to another embodiment of the present invention, there is provided an optical element including a hologram recording medium.

[0201] Specific examples of optical elements may include smart devices such as mobile devices, components of wearable displays, vehicle products (such as head-up displays), holographic fingerprint recognition systems, optical lenses, reflectors, deflection mirrors, filters, diffuser screens, diffraction elements, light guides, waveguides, holographic optical elements with projection screen and / or mask functions, media for optical storage systems and light diffuser plates, optical wavelength multiplexers, reflective and transmissive color filters, etc.

[0202] An example of an optical element including a hologram recording medium may include a hologram display device. The hologram display device includes a light source unit, an input unit, an optical system, and a display unit.

[0203] Specifically, the light source unit is a portion that irradiates a laser beam for providing, recording, and reproducing three-dimensional image information of an object in the input unit and the display unit.

[0204] The input unit is a part that pre-inputs three-dimensional image information of the object to be recorded on the display unit, specifically, the three-dimensional information of the object such as the intensity and phase of light in each space can be input into the electrically addressed liquid crystal SLM, where the input light beam can be used.

[0205] The optical system may include a reflector, a polarizer, a beam splitter, a beam gate, a lens, etc. The optical system may be allocated into an input beam for sending a laser beam emitted from a light source unit to an input unit, a recording beam for sending a laser beam to a display unit, a reference beam, an erasing beam, a reading beam, etc.

[0206] The display unit can receive the three-dimensional image information of the object from the input unit, record it on the hologram plate including the optically addressed SLM, and reproduce the three-dimensional image of the object. At this time, the three-dimensional image information of the object can be recorded by the interference of the input light beam and the reference light beam. The three-dimensional image information of the object recorded on the hologram plate can be reproduced as a three-dimensional image through the diffraction pattern generated by the read light beam. The erase light beam can be used to quickly remove the formed diffraction pattern. On the other hand, the hologram plate can be moved between the position of the input three-dimensional image and the position of the reproduced three-dimensional image.

[0207] Beneficial Effects

[0208] Since the hologram recording medium according to one embodiment of the present invention satisfies a specific element ratio, it is not only excellent in optical recording characteristics but also exhibits excellent durability against heat and moisture and can exhibit appropriate adhesion to a transparent adhesive and high transparency. BRIEF DESCRIPTION OF THE DRAWINGS

[0209] Figure 1 The recording device setup for hologram recording is schematically shown. Specifically, Figure 1The following process is schematically shown: laser light of a predetermined wavelength is radiated from a light source 10 and is irradiated onto a PP (hologram recording medium) 80 located on one surface of a reflector 70 via reflectors 20 and 20', an aperture 30, a spatial filter 40, an aperture 30', a collimating lens 50 and a PBS (Polarized Beam Splitter) 60. DETAILED DESCRIPTION

[0210] Hereinafter, the action and effect of the present invention will be described in more detail with reference to specific embodiments of the present invention. However, these embodiments are presented for illustrative purposes only, and the scope of the present invention is not limited thereby in any way.

[0211] In the following Preparation Examples, Examples, Comparative Examples and the like, unless otherwise specified, the content of a raw material and the like means the content based on the solid content.

[0212] Preparation Example 1: Preparation of (meth)acrylic polyol

[0213] 132g butyl acrylate, 420g ethyl acrylate and 48g hydroxybutyl acrylate are added to a 2L jacket reactor and diluted with 1200g ethyl acetate. The reaction temperature is set to 60°C to 70°C, and the mixture is stirred for about 30 minutes to 1 hour. 0.42g n-dodecyl mercaptan (n-DDM) is further added and stirred for about 30 minutes. Then, 0.24g AIBN is added as a polymerization initiator, and polymerization is carried out at the reaction temperature for 4 hours or more, and maintained until the residual acrylate content becomes less than 1%. Thus, a copolymer based on (meth) acrylate in which hydroxyl groups are located in the side chains (weight average molecular weight of about 300,000, OH equivalent of about 1802g / equivalent) is prepared.

[0214] Preparation Example 2: Preparation of fluorinated compounds

[0215] 20.51 g of 2,2'-{oxybis[(1,1,2,2-tetrafluoroethane-2,1-diyl)oxy]}bis(2,2-difluoroethane-1-ol) was added to a 1000 mL flask and dissolved in 500 g of tetrahydrofuran, and 4.40 g of sodium hydride (60% dispersion in mineral oil) was carefully added several times while stirring at 0°C. After stirring at 0°C for 20 minutes, 12.50 mL of 2-methoxyethoxymethyl chloride was slowly added dropwise. When all reactants were determined to be consumed by 1H NMR, 29 g of a liquid product with a purity of 95% or more was obtained using dichloromethane treatment, with a yield of 98%. The weight average molecular weight of the prepared fluorinated compound was 586, and the refractive index measured with an Abbe refractometer was 1.361.

[0216] Example 1: Preparation of hologram recording medium

[0217] (1) Preparation of photopolymer composition

[0218] First, trimethylsilyl-terminated poly(methylhydrogensiloxane) (Sigma-Aldrich, number average molecular weight: about 390, SiH equivalent: about 103 g / equivalent) as a siloxane-based polymer was mixed with the (meth)acrylic polyol prepared in Preparation Example 1. The content of the (meth)acrylic polyol was 17.95 g, and the siloxane-based polymer was added so that the SiH / OH molar ratio was 2. In Example 1, 2.05 g of the siloxane-based polymer was added.

[0219] Then, 50 g of HR 6042 (Miwon Specialty Chemical, refractive index 1.60) as a photoreactive monomer, 0.2 g of a compound represented by the following chemical formula a as a photosensitizing dye, 0.8 g of hexadecyldimethylbenzylammonium tri(p-chlorophenyl)butylborate and 0.05 g of H-Nu 254 (Spectra) as a co-initiator, 0.9 g of Irgacure 369 as a photoinitiator, 30 g of the fluorinated compound prepared in Preparation Example 2 as a plasticizer, and 206 g of methyl isobutyl ketone (MIBK) as a solvent were added, and the mixture was stirred for about 30 minutes with a paste mixer while shielding from light. Thereafter, 0.014 g of a Karstedt (Pt-based) catalyst for matrix crosslinking was added to prepare a photopolymer composition.

[0220] [Chemical formula a]

[0221]

[0222] (2) Preparation of hologram recording media

[0223] The photopolymer composition was coated on a 60 μm thick TAC substrate to a predetermined thickness using a Mayer rod, and dried at 80° C. for 10 minutes. The thickness of the photopolymer layer after drying was about 15 μm.

[0224] Use with Figure 1 The diffraction grating is recorded with the same setup as shown. Specifically, when the prepared photopolymer layer is laminated on a reflector and then irradiated with a laser, a notch filter hologram having a periodic refractive index modulation in the thickness direction can be recorded by interference between the incident light (L) and the light (L') reflected from the reflector. In this example, the notch filter hologram is recorded at an incident angle of 0° (degrees). Notch filters and Bragg reflectors are optical devices that reflect only light of a specific wavelength, and have a structure in which two layers with different refractive indices are periodically and repeatedly stacked at a constant thickness.

[0225] Examples 2 to 4 and Comparative Examples 1 to 5: Preparation of hologram recording media

[0226] A hologram recording medium was prepared in the same manner as in Example 1, except that the mixing amounts of the components of the photopolymer composition were changed as shown in Table 1 below.

[0227] [Table 1]

[0228]

[0229] Test example: Performance evaluation of hologram recording media

[0230] (1) Element ratio

[0231] The surface element ratios of the sample before recording and the sample after recording were analyzed by the method described below.

[0232] Specifically, the sample to be analyzed was fixed to a copper foil with a carbon tape, and the copper foil was placed on a sample holder and fixed with a clip. Then, an X-ray photoelectron spectrometer (ESCA, model name: K-α+, Thermo Fisher Scientific Inc.) was used to acquire data according to the K-α+ standard operating method (SOP-0524-Ok), and the element ratio (atomic %) of the sample surface was analyzed using Avantage software (version 5.980).

[0233] The system specifications of the ESCA device used are as follows.

[0234] -Basal chamber pressure: 1.0×10 -9 millibar

[0235] -X-ray source: monochromatic Al Kα (1486.6eV)

[0236] -X-ray spot size: 400μm

[0237] -Mode: CAE (Constant Analyzer Energy) mode

[0238] - Charge compensation: flood gun (FG03: 100μA, 0.5V)

[0239] Under the following conditions, the surface of the sample to be analyzed in its original state was qualitatively analyzed using an initial full spectrum scan. Based on the qualitative analysis results, each element was quantitatively analyzed by narrow scans (snapshots). The element ratios at three positions were determined for each sample, and the peak background intelligence method was applied for quantitative analysis. The binding energy correction of the core level spectrum was based on C1s (284.8 eV).

[0240] <Full spectrum scanning conditions>

[0241] -Scan cross-section binding energy: -5eV to 1350eV

[0242] - Step size: 1eV

[0243] -Dwell time per point: 20 milliseconds

[0244] -Period: 2

[0245] - Pass energy: 200eV

[0246] <Narrow Scan Condition>

[0247] -Scanning cross-section binding energy: about 20eV

[0248] - Step size: about 0.16eV

[0249] -Dwell time at each point: 1 second

[0250] - Cycles: 10 to 30

[0251] - Pass energy: 150eV

[0252] <Etching Conditions>

[0253] -Source: Ar ions

[0254] -Energy: 6keV

[0255] - Cluster size: 75

[0256] - Nominal size: 1.6×1.0mm 2

[0257] -Mode: GCIB

[0258] (2) Diffraction efficiency (DE)

[0259] The diffraction efficiency (η) is determined by the following Equation 1.

[0260] [Equation 1]

[0261] η(%)={P D / (P D +P T )}×100

[0262] Where, in Equation 1, η is the diffraction efficiency, P D is the output of the diffracted beam of the sample after recording (mW / cm 2 ), and P T is the output of the transmitted light beam of the sample after recording (mW / cm 2 ).

[0263] (3) Heat resistance (ΔDE)

[0264] Heat resistance was evaluated by the change in diffraction efficiency (ΔDE) before and after exposure to high temperature. Specifically, diffraction gratings were recorded on a sample before recording that was not exposed to high temperature and a sample before recording that was exposed to high temperature, and then heat resistance was evaluated by the degree of change in diffraction efficiency. The degree of change in diffraction efficiency was obtained by the following equation 2.

[0265] [Equation 2]

[0266] ΔDE(%)={(|DE0-DE1|) / DE0}×100

[0267] Wherein, in Equation 2, DE0 is the diffraction efficiency measured on the hologram recording medium in which a hologram is recorded after the hologram recording medium before recording is stored in a dark room under constant temperature and humidity conditions of 20°C to 25°C and 40RH% to 50RH%, and DE1 is the diffraction efficiency measured on the hologram recording medium in which a hologram is recorded after the hologram recording medium before recording is stored in a dark room under high temperature conditions of 60°C to 70°C and 40RH% to 50RH%.

[0268] The diffraction grating was recorded by the method described in Example 1, and the diffraction efficiency was obtained by Equation 1.

[0269] (4) Moisture and heat resistance (Δλ)

[0270] For the sample with the diffraction grating recorded, the wavelength showing the maximum reflectivity (ie, the lowest transmittance) was analyzed under room temperature and non-high humidity conditions. The above analysis was performed using UV-Vis spectroscopy, and the analysis wavelength range was 300 nm to 1,200 nm.

[0271] Subsequently, the same sample was stored at a temperature of 60° C. and a humidity of 90 RH % for 72 hours, and the wavelength showing the maximum reflectance (minimum transmittance) was analyzed by the same method.

[0272] The wet heat resistance of the sample is determined by the degree of shift (Δλ) of the wavelength showing the maximum reflectance before and after being placed under high temperature and high humidity conditions. The value of the degree of shift (Δλ) of the wavelength showing the maximum reflectance is evaluated, and as its absolute value is smaller, the wet heat resistance of the sample is more excellent.

[0273] (5) Adhesion to OCA

[0274] The sample on which the diffraction grating was recorded was cut into a size of 25 mm and an optically clear adhesive (OCA) was placed on the sample. 61563 (thickness: 50 μm, TESA) was laminated on the photopolymer layer of the cut sample and then laminated with OCA using glass as a substrate.

[0275] The adhesion of the photopolymer layer attached to the OCA was measured using a texture analysis device (LLOYD). The peel angle during the adhesion measurement was 180°, and the peel speed was about 5 mm / sec.

[0276] (6) Haze

[0277] A 5 cm x 5 cm test specimen was prepared from the sample on which the diffraction grating was recorded. The haze of the test specimen was measured using a haze meter (HM-150, A light source, Murakami) according to JIS K 7136. A total of three haze measurements were performed, and the average value was calculated and defined as the haze value of the sample.

[0278] [Table 2]

[0279]

[0280] As a result of measuring the element ratios on the surfaces of the samples before and after recording, the element ratios on the surfaces of the samples before and after recording were measured to be the same.

[0281] Referring to Table 2, it was determined that when the fluorine ratio was low as in Comparative Example 1, the diffraction efficiency, moisture and heat resistance, and haze were poor, and when the fluorine ratio was high as in Comparative Example 4, the adhesion was reduced. In addition, it was determined that when the silicon ratio was too high as in Comparative Example 2, the diffraction efficiency was poor, and when the silicon ratio was too low, as in Comparative Example 3, the heat resistance and haze were deteriorated, or as in Comparative Example 5, the moisture and heat resistance was deteriorated.

[0282] On the other hand, it was confirmed that the hologram recording medium according to one embodiment of the present invention satisfied the predetermined element ratio and was therefore excellent in all of diffraction efficiency, heat resistance, wet heat resistance, adhesion to OCA, and transparency.

Claims

1. A hologram recording medium comprising a photopolymer layer, the photopolymer layer comprising: a polymer matrix formed by crosslinking a siloxane-based polymer containing a silane functional group and a (meth)acrylic polyol or a precursor thereof; a photoreactive monomer and a photoinitiator system or a photopolymer obtained therefrom; and a fluorinated compound, wherein the element ratio of carbon is 50 atomic % to 70 atomic %, the element ratio of nitrogen is 0.01 atomic % to 2 atomic %, the element ratio of oxygen is 15 atomic % to 30 atomic %, the element ratio of fluorine is 3 atomic % to 12 atomic %, and the element ratio of silicon is 3 atomic % to 15 atomic %, based on the total amount of carbon atoms, nitrogen atoms, oxygen atoms, fluorine atoms and silicon atoms on the surface of the photopolymer layer determined by photoelectron spectroscopy.

2. The hologram recording medium according to claim 1, wherein the siloxane-based polymer comprises a repeating unit represented by the following Chemical Formula 1 and a terminal group represented by the following Chemical Formula 2: [Chemical formula 1] in, In Chemical Formula 1, Plural R 1 and R 2 are the same as or different from each other and are each independently hydrogen, halogen, or an alkyl group having 1 to 10 carbon atoms, and n is an integer from 1 to 10,000, [Chemical formula 2] Wherein, in Chemical Formula 2, Plural R 11 To R 13 are the same as or different from each other and are each independently hydrogen, halogen, or an alkyl group having 1 to 10 carbon atoms, and R is selected from at least one repeating unit among the repeating units represented by Chemical Formula 1 and any one terminal group among the terminal groups represented by Chemical Formula 2. 1 , R 2 and R 11 To R 13 At least one of them is hydrogen. 3 . The hologram recording medium according to claim 1 , wherein the (meth)acrylic polyol is a polymer in which a hydroxyl group is bonded to a main chain or a side chain of a (meth)acrylate-based polymer. 4 . The hologram recording medium according to claim 1 , wherein a molar ratio of a silane functional group of the siloxane-based polymer to a hydroxyl group of the (meth)acrylic polyol is 1.5 to 4. 5 .

5. The hologram recording medium according to claim 1, wherein the photoreactive monomer comprises: At least one monofunctional monomer selected from benzyl (meth)acrylate, benzyl 2-phenylacrylate, phenoxybenzyl (meth)acrylate, phenol (ethylene oxide) (meth)acrylate, phenol (ethylene oxide) 2 (meth)acrylate, o-phenylphenol (ethylene oxide) (meth)acrylate, phenylthioethyl (meth)acrylate and biphenyl methyl (meth)acrylate; selected from bisphenol A (ethylene oxide) 2~10 At least one multifunctional monomer selected from the group consisting of di(meth)acrylate, bisphenol A epoxy di(meth)acrylate, bisfluorene di(meth)acrylate, modified bisphenol fluorene di(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, phenol novolac epoxy (meth)acrylate and cresol novolac epoxy (meth)acrylate; or a mixture of two or more thereof. 6 . The hologram recording medium according to claim 1 , wherein the photoreactive monomer is contained in an amount of 50 parts by weight to 300 parts by weight based on 100 parts by weight of the polymer matrix.

7. The holographic recording medium of claim 1, wherein the photoinitiator system comprises a photosensitizing dye and a co-initiator.

8. The hologram recording medium according to claim 7, wherein the photosensitive dye comprises a silicon rhodamine compound represented by the following Chemical Formula 3: [Chemical formula 3] in, In chemical formula 3, R 21 To R 29 are each independently hydrogen, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted aryloxy group having 6 to 30 carbon atoms, d and e are each independently an integer from 0 to 3, f is an integer from 0 to 5, and An - It is an anion.

9. The hologram recording medium according to claim 7, wherein the coinitiator comprises a borate anion represented by the following Chemical Formula 4: [Chemical formula 4] BX 1 X 2 X 3 X 4 in, In chemical formula 4, X 1 To X 4 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an alkylaryl group having 7 to 30 carbon atoms, or an allyl group, provided that X 1 To X 4 At least one of the groups is not an aryl group. 10 . The hologram recording medium according to claim 1 , wherein the fluorinated compound is included in an amount of 20 parts by weight to 200 parts by weight based on 100 parts by weight of the polymer matrix.

11. The hologram recording medium according to claim 1, wherein the photopolymer layer comprises 17 wt% to 38 wt% of the polymer matrix, 36 wt% to 58 wt% of the photoreactive monomer, and 17 wt% to 38 wt% of the fluorinated compound, based on the total weight of the polymer matrix, the photoreactive monomer and the fluorinated compound.

12. The hologram recording medium according to claim 1, wherein when the notch filter hologram is recorded, the diffraction efficiency is 80% or more.

13. The hologram recording medium according to claim 1, wherein a diffraction efficiency variation value ΔDE calculated by the following equation 2 is 10% or less: [Equation 2] ΔDE(%)={(|DE0-DE1|) / DE0}×100 in, In Equation 2, DE0 is the diffraction efficiency measured for the hologram recording medium in which a notch filter hologram is recorded after the hologram recording medium before recording is stored in a dark room under constant temperature and humidity conditions of 20°C to 25°C and 40RH% to 50RH%, and DE1 is the diffraction efficiency measured for the hologram recording medium in which a notch filter hologram is recorded after the hologram recording medium before recording is stored in a dark room under high temperature conditions of 60°C to 70°C and 40RH% to 50RH%.

14. The hologram recording medium according to claim 1, wherein the degree of shift of the wavelength showing the maximum reflectivity before and after storage for 72 hours under the conditions of a temperature of 60°C and a relative humidity of 90% is -10 nm to 10 nm.

15. The hologram recording medium according to claim 1, wherein the photopolymer layer has an adhesive force to the optically transparent adhesive of 1000 gf / 25 mm or more.

16. The hologram recording medium according to claim 1, wherein a haze is 3% or less.

17. A method for preparing a hologram recording medium, comprising the steps of: applying a photopolymer composition to form a photopolymer layer, wherein the photopolymer composition comprises: a polymer matrix formed by crosslinking a siloxane-based polymer containing silane functional groups and a (meth)acrylic polyol or a precursor thereof, a fluorinated compound, a photoreactive monomer, and a photoinitiator system; as well as irradiating a coherent laser onto a predetermined area of ​​the photopolymer layer and selectively polymerizing the photoreactive monomer contained in the photopolymer layer to record optical information, wherein the element ratio of carbon is 50 atomic % to 70 atomic %, the element ratio of nitrogen is 0.01 atomic % to 2 atomic %, the element ratio of oxygen is 15 atomic % to 30 atomic %, the element ratio of fluorine is 3 atomic % to 12 atomic %, and the element ratio of silicon is 3 atomic % to 15 atomic %, based on the total amount of carbon atoms, nitrogen atoms, oxygen atoms, fluorine atoms and silicon atoms on the surface of the photopolymer layer determined by photoelectron spectroscopy.

18. The method for preparing a hologram recording medium according to claim 17, wherein the photopolymer composition contains a Pt-based catalyst, wherein the Pt-based catalyst is contained in an amount of 0.01 parts by weight to 0.30 parts by weight based on 100 parts by weight of the (meth)acrylic polyol.

19. The method for producing a hologram recording medium according to claim 17, wherein in the step of forming the photopolymer layer, a coating layer formed by applying a photopolymer composition is dried at 50°C to 120°C.

20. An optical element comprising the hologram recording medium according to claim 1.