Liquid crystalline media comprising polymerizable compounds

By adding monocyclic compounds with specific structures to LC media and using various UV light sources for polymerization, the problems of reliability and response time in the polymer stabilization process of LC displays have been solved, achieving efficient and low-cost polymer compound processing.

CN119095933APending Publication Date: 2024-12-06MERCK PATENT GMBH

Patent Information

Application Number
CN202380036315.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-27
Filing Date
2023-04-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In existing LC display technologies, when using UV light sources for polymer stabilization, there are problems such as reduced reliability of the LC medium, prolonged response time, and reduced voltage hold-up ratio, which are particularly noticeable when using short-wavelength UV light sources, and the cost of replacing the light source is high.

Method used

By using polymer compounds containing monocyclic groups, polymerizable compounds with specific structures are added to LC media, and polymerization is carried out using UV-C, UV-B, and UV-LED light sources, achieving rapid and complete polymerization while maintaining high reliability and voltage retention ratio.

Benefits of technology

It achieves rapid and complete polymerization of polymer compounds under different UV light sources, maintains high voltage hold-up ratio and response speed, reduces energy consumption and production costs, and reduces residual effects on display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005101443060000041
    Figure BDA0005101443060000041
  • Figure BDA0005101443060000051
    Figure BDA0005101443060000051
  • Figure BDA0005101443060000052
    Figure BDA0005101443060000052
Patent Text Reader

Abstract

The present invention relates to LC media comprising two or more polymerizable compounds, one of which has a monocyclic group; the use thereof for optical, electro-optical and electronic purposes, in particular in LC displays, in particular in LC displays in PSA (Polymer Continuous Alignment) or SA (Self-Alignment) mode; an LC display in a PSA or SA mode comprising an LC medium; the invention relates to an LC medium and a method for manufacturing an LC display by using the LC medium, in particular to an energy-saving LC display and a preparation method of the energy-saving LC display.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to LC media comprising two or more polymerizable compounds, one of which has a monocyclic group; to their use for optical, electro-optical and electronic purposes, in particular in LC displays, especially LC displays in PSA (polymer sustained alignment) or SA (self-alignment) mode; to LC displays in PSA or SA mode comprising the LC medium; and to methods for producing LC displays using the LC medium, in particular energy-saving LC displays and methods for producing energy-saving LC displays.

[0002] The prevalence of 8K and gaming monitors has led to an increased demand for LC display (LCD) panels with higher refresh rates and therefore LC media with faster response times. Many of these LCD panels are using polymer-stabilized (PS) or polymer-persistently aligned (PSA) modes, such as PS-VA (vertical alignment), PS-IPS (in-plane switching) or PS-FFS (fringe field switching) modes or modes derived therefrom, or self-aligned (SA) modes, such as polymer-stabilized SA-VA.

[0003] In the PS or PSA mode, a small amount (usually 0.1 to 1%) of one or more polymerizable mesogenic compounds, also called RMs (reactive mesogens), is added to the LC medium. After the LC medium is filled into the display, the RMs are then polymerized in situ by UV photopolymerization while a voltage is applied to the electrodes of the display. As a result, a small tilt angle is generated in the LC molecules of the LC medium, which is stabilized by the polymerized RMs. The UV polymerization process, also called "PSA process", is usually carried out in two steps, a first UV exposure step ("UV1 step") in which a voltage is applied to generate the tilt angle, and a second UV exposure step ("UV2 step") in which no voltage is applied to complete the polymerization of the RMs.

[0004] In the SA-VA mode, the alignment layer is omitted in the display. Instead, a small amount (typically 0.1 to 2.5%) of a self-aligning (SA) additive is added to the LC medium, which induces the desired alignment, e.g., vertical or planar alignment, in situ by a self-assembly mechanism. The SA additive typically contains an organic mesogen core group and one or more polar anchor groups attached thereto, e.g., hydroxyl, carboxyl, amino or thiol groups, which can interact with the substrate surface, thereby causing the additive alignment on the substrate surface and also inducing the desired alignment in the LC molecules. The SA additive may also contain one or more polymerizable groups that can be polymerized under conditions similar to the RMs used in the PSA process. In addition to the SA additive, the LC medium may also contain one or more RMs.

[0005] In the display manufacturing method of the PSA mode display, as the radiation source of the UV1 step and / or the UV2 step, a UV C type and / or UV B type lamp is generally used. The UV C type lamp generally has an emission spectrum in which the shortest UV wavelength is about 300 nm, and the UV B type lamp generally has an emission spectrum in which the shortest UV wavelength is about 320 nm.

[0006] On the other hand, to achieve low viscosity and fast response time, the LC host mixture of the polymerizable LC medium used in PSA mode displays usually contains one or more compounds with alkenyl groups. However, this can lead to reduced reliability of the mixture and a significant drop in its voltage holding ratio (VHR) when exposed to the UV light required to polymerize the RM. It is particularly problematic when using shorter UV wavelengths of less than 320nm. This can be overcome by using longer UV wavelength radiation sources for PSA processes. However, running changes in radiation sources in large-scale production processes for displays is costly and time-consuming. Likewise, this will then pose problems for finding RMs with absorption at longer wavelengths that are high enough to enable rapid and complete photopolymerization.

[0007] UV-LED lamps have also been proposed for use in PSA processes, as they exhibit lower energy consumption, longer lifetime and, due to a narrower emission peak, more efficient optical energy transfer to the LC medium, which allows a reduction in UV intensity and / or UV irradiation time. This enables a reduction in cycle time and saves energy and production costs.

[0008] Therefore, there is a need for polymerizable LC media, especially those based on LC host mixtures containing alkenyl compounds, which contain RMs that can be efficiently polymerized both at UV wavelengths emitted by UV C type lamps (where the shortest wavelength is about 300 nm) and at UV wavelengths emitted by UV B type lamps (where the shortest wavelength is about 320 nm). There is also a need for polymerizable LC media, especially those based on LC host mixtures containing alkenyl compounds, which show high reliability and only a small reduction in VHR values ​​after UV stress and at the same time show fast response times.

[0009] Furthermore, there is a great need for PSA or SA displays and LC media and polymerizable compounds for such PSA or SA displays, which are able to achieve high specific resistances, at the same time a large operating temperature range, short response times (even at low temperatures), and low threshold voltages, low tilt angles, high tilt stability, multiplicity of grayscales, high contrast and wide viewing angles, high reliability and high VHR values ​​after UV exposure, and in the case of polymerizable compounds, low melting points and high solubility in LC host mixtures. In displays for mobile applications, it is particularly desirable to have available LC media that exhibit low threshold voltages and high birefringence.

[0010] The present invention is based on the object of providing novel suitable materials for PSA or SA displays, in particular RMs and LC media comprising the same, which do not have the disadvantages indicated above or have them to a reduced extent.

[0011] In particular, the present invention is based on the object of an LC medium comprising RMs for PSA or SA displays which enables very high specific resistance values ​​to be achieved, high VHR values, high reliability, low threshold voltage, short response time, high birefringence, exhibits good UV absorption, in particular at UV wavelengths in the range from 300 to 360 nm, enables rapid and complete polymerization of the RMs, allows the creation of low tilt angles, preferably as rapid as possible, enables high stability of the tilt angles even after longer times and / or after UV exposure, reduces or prevents the appearance of “image sticking” and “ODF mura” in the display, and, in the case of the RMs, polymerizes as rapidly and completely as possible and exhibits high solubility in LC media typically used as host mixtures for PSA or SA displays.

[0012] It was a further object of the present invention to provide LC media for PSA displays in which the RM exhibits both a fast polymerization speed and good reliability parameters, such as a high VHR or a good tilt stability.

[0013] It is a further object of the present invention to provide novel LC media containing RMs, in particular for use in optical, electro-optical and electronic applications, and suitable processes and intermediates for their preparation.

[0014] It is a further object of the present invention to provide LC media containing RMs which exhibit one or more of the following advantageous effects:

[0015] - it produces the desired degree of tilt angle after exposure to UV light,

[0016] - it results in good tilt stability,

[0017] - it leads to high and stable VHR and only a small decrease of CHR after UV stress, especially in the case of LC media based on LC host mixtures containing alkenyl compounds,

[0018] - it is suitable for PSA displays produced by a polymerization process using UV-C type lamps and / or UV-B type lamps,

[0019] - it is suitable for PSA displays prepared by a polymerization process using UV-LED lamps,

[0020] - it enables good control of the time frame of the first UV step, where the tilt angle is created during the UV treatment,

[0021] - it enables to keep the time frame of the second UV step (where any residual RMs are polymerized and the tilt angle is stabilized) as short as possible to minimize energy consumption and production costs,

[0022] - After the first and second UV exposure steps, the residual RMs have little or no negative impact on the LC mixture performance parameters (such as VHR, tilt stability, etc.).

[0023] It was found that one or more of these objectives can be achieved by providing an LC medium comprising polymerizable compounds as disclosed and claimed hereinafter, one of the polymerizable compounds being a monocyclic compound.

[0024] The present invention therefore relates to an LC medium comprising one or more polymerisable compounds of the formula IA and one or more polymerisable compounds of the formula IB

[0025] P-Sp-M 1 -Sp-P IA

[0026] P-Sp-M 2 -Sp-P IB

[0027] where the individual radicals independently of one another and on each occurrence have the following meanings identically or differently

[0028] P is a polymerizable group,

[0029] Sp is a spacer group or a single bond,

[0030] M 1 is a benzene ring optionally substituted by one or more groups L or P-Sp-,

[0031] M 2 A group selected from the following formula

[0032]

[0033] wherein the benzene ring is optionally substituted by one or more groups L or P-Sp-,

[0034] L is F, Cl, -CN, or a straight-chain, branched or cyclic alkyl group having 1 to 25 C atoms, wherein one or more non-adjacent CH2- groups are optionally replaced by -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O-, in a manner such that the O- and / or S- atoms are not directly connected to each other, and wherein one or more H atoms are each optionally replaced by P, F or Cl.

[0035] The present invention further relates to novel compounds of formula IA.

[0036] The present invention further relates to an LC medium having a negative dielectric anisotropy and comprising one or more polymerizable compounds selected from the group consisting of formula IA, one or more polymerizable compounds selected from the group consisting of formula IB and IC, and further comprising one or more compounds of formula II

[0037]

[0038] where the individual radicals independently of one another and on each occurrence have the following meanings identically or differently

[0039] R 21 , R 22 is H, a straight-chain, branched or cyclic alkyl or alkoxy radical having 1 to 20 C atoms, wherein one or more non-adjacent CH2- groups are optionally connected via -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O-, CR- 0 =CR 00 -、-C≡C-、 substituted, and wherein one or more H atoms are each optionally replaced by F, Cl, CN or CF3, preferably an alkyl or alkoxy group having 1 to 6 C atoms,

[0040] R 0 , R 00 is H or an alkyl radical having 1 to 12 C atoms,

[0041] A 1 , A 2 A group selected from the following formulae:

[0042]

[0043]

[0044] Preferably selected from the formulae A1, A2, A3, A4, A5, A6, A9 and A10, very preferably selected from the formulae A1, A2, A3, A4, A5, A9 and A10,

[0045] Z 1 , Z 2 is -CH2CH2-, -CH=CH-, -CF2O-, -OCF2-, -CH2O-, -OCH2-, -CO-O-, -O-CO-, -C2F4-, -CF=CF-, -CH=CH-CH2O- or a single bond, preferably a single bond,

[0046] L 1 , L 2 , L 3 , L 4is F, Cl, OCF3, CF3, CH3, CH2F or CHF2, preferably F or Cl, very preferably F,

[0047] Y is H, F, Cl, CF3, CHF2 or CH3, preferably H or CH3, very preferably H,

[0048] L C is CH3 or OCH3, preferably CH3,

[0049] a1 is 0, 1, or 2,

[0050] a2 is 0 or 1.

[0051] The invention further relates to the use of an LC medium as described above and hereinafter in an LC display in PSA or SA mode.

[0052] Furthermore, the invention relates to a process for preparing an LC medium as described above and hereinafter, comprising the step of mixing one or more polymerizable compounds of the formula IA and one or more polymerizable compounds of the formula IB with one or more compounds of the formula II and optionally with further LC compounds and / or additives.

[0053] Furthermore, the present invention relates to an LC display comprising an LC medium according to the invention as described above and hereinafter, which is a PSA or SA display, preferably a PS-VA, PS-IPS, PS-FFS or SA-VA display.

[0054] Furthermore, the invention relates to an LC display comprising an LC medium as described above and hereinafter, wherein the polymerisable compound is present in polymerised form, the LC display preferably being a PSA or SA display, very preferably a PS-VA, PS-IPS, PS-FFS or SA-VA display.

[0055] Furthermore, the invention relates to an LC display of the PSA type comprising two substrates, at least one of which is transparent to light, an electrode arranged on each substrate or two electrodes arranged on only one of the substrates, and a layer of LC medium as described above and below positioned between the substrates, wherein the polymerizable compound is polymerized between the substrates of the display by UV light polymerization.

[0056] Furthermore, the invention relates to a method for producing an LC display as described above and in the following, comprising the steps of filling or otherwise providing an LC medium as described above and in the following between the substrates of the display, and polymerizing the polymerizable compound, preferably by irradiation with UV light, preferably having a wavelength >300 nm, more preferably in the range of 300 to 380 nm, very preferably in the range of 300 to 360 nm, and preferably simultaneously applying a voltage to the electrodes of the display.

[0057] The invention furthermore relates to a method for producing an LC display as described above and hereinafter, in which the irradiation of the polymerizable compounds is carried out using UV C type lamps and / or UV B type lamps.

[0058] When used in PSA displays, the LC media according to the invention exhibit the following advantageous properties:

[0059] - Produced by a suitable tilt within a certain process window,

[0060] - Rapid polymerization resulting in minimal residue of RM after UV process,

[0061] -High voltage holding rate after UV process,

[0062] - Good tilt stability,

[0063] -Good VHR,

[0064] - sufficient stability against heat,

[0065] - Sufficient solubility in organic solvents commonly used in display manufacturing.

[0066] Furthermore, the LC media according to the invention exhibit one or more of the following advantageous properties:

[0067] - it produces the desired degree of tilt angle after exposure to UV light,

[0068] - it provides high tilt stability,

[0069] - it shows good UV absorption, especially at longer UV wavelengths, preferably in the range preferably with wavelengths > 300 nm, more preferably in the range from 300 to 380 nm, very preferably in the range from 300 to 360 nm, and enables rapid and complete polymerization of the RM at these wavelengths,

[0070] - it is suitable for PSA displays produced by a polymerization process using UV C type lamps or UV B type lamps,

[0071] - it enables to control the time frame of the first UV step, where the tilt angle is created during the UV treatment,

[0072] - it keeps the time frame of the second UV step as short as possible to minimize production costs,

[0073] - It reduces or avoids any negative impact of residual RMs on LC mixture performance parameters (such as VHR, tilt stability, etc.) after the first and second UV exposure steps.

[0074] As described below, alkenyl groups in compounds of formula II or other components of the LC medium are not to be regarded as falling within the meaning of the term "polymerizable group" as used herein. The polymerisation conditions for the polymerizable compounds of the LC medium are preferably chosen such that the alkenyl substituents do not participate in the polymerisation reaction. Preferably, the LC medium disclosed and claimed in the present application does not contain additives which initiate or enhance the participation of alkenyl groups in polymerisation reactions.

[0075] Unless otherwise stated, the polymerizable compound and the compound of formula II are preferably selected from achiral compounds.

[0076] As used herein, the expression "UV light having a wavelength of..." followed by a given range of wavelengths (in nm), or a given lower or upper wavelength limit (in nm), indicates that the UV emission spectrum of the corresponding radiation source has an emission peak, which is preferably the highest peak in the corresponding spectrum within the given wavelength range, or above the given lower wavelength limit, or below the given upper wavelength limit, and / or the UV absorption spectrum of the corresponding chemical compound has a long wavelength tail or a short wavelength tail extending into the given wavelength range, or above the given lower wavelength limit, or below the given upper wavelength limit.

[0077] As used herein, the term "full width at half maximum" or "FWHM" refers to the width of a spectrum curve measured between those points on the y-axis that are half the maximum amplitude.

[0078] As used herein, the term "substantially transmits" means that the filter transmits a substantial portion of incident light of a desired wavelength, preferably at least 50% of the intensity. As used herein, the term "substantially blocks" means that the filter does not transmit a substantial portion of incident light of an undesired wavelength, preferably at least 50% of the intensity. As used herein, the term "desired (undesired) wavelength" means, for example, for a bandpass filter, a wavelength within (outside) a given range λ, and for a cutoff filter, a wavelength above (below) a given λ value.

[0079] As used herein, the terms "active layer" and "switchable layer" refer to a layer in an electro-optical display, such as an LC display, which comprises one or more molecules, such as LC molecules, having structural and optical anisotropy, which molecules change their orientation when subjected to an external stimulus, such as an electric or magnetic field, resulting in a change in the transmittance of the layer for polarized or unpolarized light.

[0080] As used herein, the terms "tilt" and "tilt angle" are to be understood as meaning the tilted alignment of the LC molecules of the LC medium relative to the cell surface in an LC display, preferably a PSA display herein, and are to be understood as including "pretilt" and "pretilt angle". The tilt angle herein refers to the average angle (<90°) between the longitudinal molecular axis of the LC molecules (LC director) and the plane-parallel outer plate surfaces forming the LC cell. Low absolute values ​​of the tilt angle (i.e. large deviations from an angle of 90°) correspond herein to large tilts. A suitable method for measuring the tilt angle is given in the Examples. Unless otherwise stated, the tilt angle values ​​disclosed above and below relate to this method of measurement.

[0081] As used herein, the terms "reactive mesogen" and "RM" are understood to mean a compound containing a mesogenic or liquid crystal backbone and attached thereto one or more functional groups suitable for polymerization, and the functional groups are also referred to as "polymerizable groups" or "P".

[0082] Unless otherwise indicated, the term "polymerizable compound" as used herein shall be understood to mean a polymerizable monomeric compound.

[0083] The SA-VA displays of the present invention will be of polymer-stabilized mode since they comprise or are manufactured by using an LC medium comprising RMs of formulae I and II. Therefore as used herein, even if not explicitly mentioned, the term "SA-VA display" when referring to the displays of the present invention is to be understood as meaning a polymer-stabilized SA-VA display.

[0084] As used herein, the term "low molecular weight compound" is understood to mean a monomer and / or a compound that is not prepared by polymerization, as opposed to a "polymeric compound" or "polymer."

[0085] As used herein, the term "non-polymerizable compound" will be understood to mean a compound that does not contain functional groups suitable for polymerization under the conditions normally applied to RM polymerization.

[0086] As used herein, the term "mesogenic group" is known to those skilled in the art and is described in the literature and refers to a group that substantially contributes to the generation of a liquid crystal (LC) phase in a low molecular weight or polymeric substance due to its anisotropy of attractive and repulsive interactions. A compound containing a mesogenic group (mesogenic compound) does not necessarily have an LC phase per se. A mesogenic compound can exhibit LC phase behavior only after mixing with other compounds and / or after polymerization. Typical mesogenic groups are, for example, rigid rod-shaped or disc-shaped units. Terms and definitions used in connection with mesogenic or LC compounds are given in Pure Appl. Chem. 2001, 73 (5), 888 and C. Tschierske, G. Pelzl, S. Diele, Angew. Chem. 2004, 116, 6340-6368.

[0087] As used herein, the term "spacer" (hereinafter also referred to as "Sp") is known to those skilled in the art in the art and is described in the literature, see for example Pure Appl. Chem. 2001, 73 (5), 888 and C. Tschierske, G. Pelzl, S. Diele, Angew. Chem. 2004, 116, 6340-6368. As used herein, the term "spacer" or "spacer" refers to a flexible group, for example an alkylene group, which is connected to a mesogenic group or a polymerizable group in a polymerizable mesogenic compound. In this context, represents a trans-1,4-cyclohexylene ring, and It represents a 1,4-phenylene ring.

[0088] In the group In the case of phenylene, the single bond between two ring atoms can be connected to any free position of the benzene ring.

[0089] If in the formulae shown above and below, a terminal group such as R 1A、2A , R 1 , R 2 , R 11、12、13 , R 31、32 , R 41、42 , R 51、52 , R 61、62 , R 71、72 , R 81、82、83 , R Q , R 0 , R, R M , R S , R S1、S2、S3、S4or L represents alkyl and / or alkoxy, which may be straight-chain or branched. It is preferably straight-chain, has 2, 3, 4, 5, 6 or 7 C atoms and therefore preferably represents ethyl, propyl, butyl, pentyl, hexyl, heptyl, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy or heptyloxy, furthermore, methyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, methoxy, octyloxy, nonyloxy, decyloxy, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, methoxy, octyloxy, nonyloxy, decyloxy, undecyl, dodecyl, tridecyl or tetradecyl.

[0090] If one of the abovementioned terminal groups represents an alkyl group in which one or more CH2 groups are replaced by S, this may be straight-chain or branched. It is preferably straight-chain, has 1, 2, 3, 4, 5, 6 or 7 C atoms and therefore preferably represents thiomethyl, thioethyl, thiopropyl, thiobutyl, thiopentyl, thiohexyl or thioheptyl.

[0091] Oxaalkyl preferably denotes straight-chain 2-oxapropyl (=methoxymethyl); 2-oxabutyl (=ethoxymethyl) or 3-oxabutyl (=2-methoxyethyl); 2-, 3- or 4-oxapentyl; 2-, 3-, 4- or 5-oxahexyl; 2-, 3-, 4-, 5- or 6-oxaheptyl; 2-, 3-, 4-, 5-, 6- or 7-oxaoctyl; 2-, 3-, 4-, 5-, 6-, 7- or 8-oxanononyl; 2-, 3-, 4-, 5-, 6-, 7-, 8- or 9-oxadecyl.

[0092] If one of the abovementioned terminal groups represents an alkoxy group or an oxaalkyl group, it may also contain one or more further oxygen atoms, as long as the oxygen atoms are not directly connected to one another.

[0093] If one of the abovementioned terminal groups represents an alkyl group in which one CH2 group has been replaced by -CH=CH-, this may be straight-chain or branched. It is preferably straight-chain and has 2 to 10 C atoms. Thus, in particular, it represents vinyl; prop-1- or -2-enyl; but-1-, -2- or -3-enyl; pent-1-, -2-, -3- or -4-enyl; hex-1-, -2-, -3-, -4- or -5-enyl; hept-1-, -2-, -3-, -4-, -5- or -6-enyl; oct-1-, -2-, -3-, -4-, -5-, -6- or -7-enyl; non-1-, -2-, -3-, -4-, -5-, -6-, -7- or -8-enyl; dec-1-, -2-, -3-, -4-, -5-, -6-, -7-, -8- or -9-enyl.

[0094] If one of the abovementioned terminal groups represents an alkyl or alkenyl group, which is at least monosubstituted by halogen, this group is preferably straight-chain and the halogen is preferably F or Cl. In the case of polysubstitution, the halogen is preferably F. The resulting groups also include perfluorinated groups. In the case of monosubstitution, the fluorine or chlorine substituent can be in any desired position, but is preferably in the ω position.

[0095] In another preferred embodiment, the above-mentioned terminal groups, such as R 1A、2A , R 1 , R 2 , R 11、12、13 , R 31、32 , R 41 、42 , R 51、52 , R 61、62 , R 71、72 , R 81、82、83 , R Q , R 0 , R, R M , R S , R S1 , S2 , S3 , S4 or L one or more selected from -S 1 -F, -OS 1 -F, -O-S1-O-S2, where S 1 C 1-12 -alkylene or C 2-12 -alkenylene and S 2 H, C 1-12 -alkyl or C 2-12 -alkenyl, and very preferably selected from A group consisting of -OCH2OCH3, -O(CH2)2OCH3, -OCH2OCH3, -O(CH2)2OCH3, -O(CH2)3OCH3, -O(CH2)4OCH3, -O(CH2)2F, -O(CH2)3F, and -O(CH2)4F.

[0096] If in the formulae shown above and below, the radical R 1至13 , R 51 , R 52 , R Q , R, R 2A , R 2B , R IIIA , R 1N , R 2N , R B1 , R B2 , RCR1 , R CR2 , R or L denotes alkyl in which one CH2 group has been replaced by -CH=CH-, which may be straight-chain or branched. It is preferably straight-chain and has 2 to 10 C atoms. Thus, in particular, it represents vinyl; prop-1- or -2-enyl; but-1-, -2- or -3-enyl; pent-1-, -2-, -3- or -4-enyl; hex-1-, -2-, -3-, -4- or -5-enyl; hept-1-, -2-, -3-, -4-, -5- or -6-enyl; oct-1-, -2-, -3-, -4-, -5-, -6- or -7-enyl; non-1-, -2-, -3-, -4-, -5-, -6-, -7- or -8-enyl; dec-1-, -2-, -3-, -4-, -5-, -6-, -7-, -8- or -9-enyl.

[0097] If in the formulae shown above and below, the radical R 1至13 , R 51 , R 52 , R Q , R, R 2A , R 2B , R IIIA , R 1N , R 2N , R B1 , R B2 , R CR1 , R CR2 If R, R or L represents an alkyl or alkenyl group which is at least monosubstituted by halogen, this group is preferably straight-chain and halogen is preferably F or Cl. In the case of polysubstitution, halogen is preferably F. The resulting groups also include perfluorinated groups. In the case of monosubstitution, the fluorine or chlorine substituents may be in any desired position, but are preferably in the ω position.

[0098] Halogen is preferably F or Cl, very preferably F.

[0099] Group-CR 0 =CR 00 - is preferably -CH=CH-.

[0100] -CO-, -C(=O)- and -C(O)- represent a carbonyl group, that is,

[0101] Preferred substituents L are, for example, F, Cl, Br, I, -CN, -NO2, -NCO, -NCS, -OCN, -SCN, -C(=O)N(R x )2, -C(=O)Y 1 、-C(=O)R x 、-N(R x) 2, linear or branched alkyl, alkoxy, alkylcarbonyl, alkoxycarbonyl, alkylcarbonyloxy or alkoxycarbonyloxy, each having 1 to 25 C atoms, in which one or more H atoms may optionally be replaced by F or Cl, optionally substituted silyl having 1 to 20 Si atoms, linear or branched alkenyl having 2 to 12 C atoms, or optionally substituted aryl having 6 to 25, preferably 6 to 15 C atoms,

[0102] Where R x represents H, F, Cl, CN or a straight-chain, branched or cyclic alkyl group having 1 to 25 C atoms, wherein one or more non-adjacent CH2-groups are optionally replaced by -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O- in such a way that the O- and / or S-atoms are not directly connected to each other, and wherein one or more H atoms are each optionally replaced by F, Cl, P- or P-Sp-, and

[0103] Y 1 Represents halogen.

[0104] Particularly preferred substituents L are, for example, F, Cl, CN, NO2, CH3, C2H5, OCH3, OC2H5, SCH3, SC2H5, COCH3, COC2H5, COOCH3, COOC2H5, CF3, OCF3, OCHF2, OC2F5, -CH=CH2, -CH2-CH=CH2, -CH=CH-CH3, -CH=CH-CH=CH2 or -C(CH3)=CH2.

[0105] Preferably wherein L has one of the meanings specified above.

[0106] The polymerizable group P is a group suitable for polymerization, such as free radical or ionic chain polymerization, addition polymerization or condensation polymerization, or a group suitable for polymer-analogous reactions, such as addition or condensation on the polymer backbone. Particularly preferred are groups for chain polymerization, in particular those containing a C=C double bond or a -C≡C- triple bond, and groups suitable for ring-opening polymerization, such as oxetane or epoxy.

[0107] Preferred groups P are selected from the following groups

[0108] CH2=CW 1 -CO-O-, CH2=CW 1 -CO-, CH2=CW 2 -(O) k3 -、CW 1 =CH-CO-(O)k3 -、CW 1 =CH-CO-NH-, CH2=CW 1 -CO-NH-, CH3-CH=CH-O-, (CH2=CH)2CH-OCO-, (CH2=CH-CH2)2CH-OCO-, (CH2=CH)2CH-O-, (CH2=CH-CH2)2N-, (CH2=CH-CH2)2N-CO-, HO-CW 2 W 3 -、HS-CW 2 W 3 -、HW 2 N-、HO-CW 2 W 3 -NH-, CH2=CW 1 -CO-NH-, CH2=CH-(COO) k1 -Phe-(O) k2 -、CH2=CH-(CO) k1 -Phe-(O) k2 -, Phe-CH=CH-, HOOC-, OCN- and W 4 W 5 W 6 Si-, where W 1 represents H, F, Cl, CN, CF3, phenyl or alkyl having 1 to 5 C atoms, in particular H, F, Cl or CH3, W 2 and W 3 each independently of one another represents H or alkyl having 1 to 5 C atoms, in particular H, methyl, ethyl or n-propyl, W 4 ,W 5 and W 6 Each independently represents Cl, oxaalkyl or oxacarbonylalkyl having 1 to 5 C atoms, W 7 and W 8 Each independently represents H, Cl or an alkyl group having 1 to 5 C atoms, Phe represents 1,4-phenylene, which is optionally substituted by one or more groups L different from P-Sp- as defined above, k1, k2 and k3 each independently represent 0 or 1, k3 preferably represents 1, and k4 represents an integer from 1 to 10.

[0109] Very preferred groups P are selected from the following groups:

[0110] CH2=CW 1 -CO-O-, CH2=CW 1 -CO-, CH2=CW 2-O-, CH2=CW 2 -, CW 1 =CH-CO-(O) k3 -, CW 1 =CH-CO-NH-, CH2=CW 1 -CO-NH-, (CH2=CH)2CH-OCO-, (CH2=CH-CH2)2CH-OCO-, (CH2=CH)2CH-O-, (CH2=CH-CH2)2N-, (CH2=CH-CH2)2N-CO-, CH2=CW 1 -CO-NH-, CH2=CH-(COO) k1 -Phe-(O) k2 -, CH2=CH-(CO) k1 -Phe-(O) k2 -, Phe-CH=CH- and W 4 W 5 W 6 Si-, where W 1 represents H, F, Cl, CN, CF3, phenyl or alkyl having 1 to 5 C atoms, in particular H, F, Cl or CH3, W 2 and W 3 each independently of one another represents H or alkyl having 1 to 5 C atoms, in particular H, methyl, ethyl or n-propyl, W 4 ,W 5 and W 6 Each independently represents Cl, oxaalkyl or oxacarbonylalkyl having 1 to 5 C atoms, W 7 and W 8 Each independently represents H, Cl or an alkyl group having 1 to 5 C atoms, Phe represents 1,4-phenylene, k1, k2 and k3 each independently represent 0 or 1, k3 preferably represents 1, and k4 represents an integer of 1-10.

[0111] Very particularly preferred groups P are selected from the group CH2=CW 1 -CO-O-, in particular CH2=CH-CO-O-, CH2=C(CH3)-CO-O- and CH2=CF-CO-O-, as well as CH2=CH-O-, (CH2=CH)2CH-O-CO-, (CH2=CH)2CH-O-,

[0112] Further preferred polymerizable groups P are selected from vinyloxy, acrylate, methacrylate, fluoroacrylate, chloroacrylate, oxetane and epoxy groups, with acrylate and methacrylate being most preferred.

[0113] Very preferably, all polymerizable groups in the polymerizable compounds as used in the present invention have the same meaning.

[0114] If the spacer group Sp is different from a single bond, it is preferably of the formula Sp"-X", so that each group P-Sp- conforms to the formula P-Sp"-X"-, where

[0115] Sp" denotes a linear or branched alkylene radical having 1 to 20, preferably 1 to 12 C atoms, which is optionally mono- or polysubstituted by F, Cl, Br, I or CN and in which, in addition, one or more non-adjacent CH2 groups may each be independently of one another by -O-, -S-, -NH-, -N(R)-, -S-, -NH-, -NH- or -N(R)- in such a way that the O and / or S atoms are not directly bonded to one another. 0 )-、-Si(R 0 R 00 )-, -CO-, -CO-O-, -O-CO-, -O-CO-O-, -S-CO-, -CO-S-, -N(R 00 )-CO-O-、-O-CO-N(R 0 )-、-N(R 0 )-CO-N(R 00 )-, -CH=CH- or -C≡C-,

[0116] X" means -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O-, -CO-N(R 0 )-、-N(R 0 )-CO-、-N(R 0 )-CO-N(R 00 )-, -OCH2-, -CH2O-, -SCH2-, -CH2S-, -CF2O-, -OCF2-, -CF2S-, -SCF2-, -CF2CH2-, -CH2CF2-, -CF2CF2-, -CH=N-, -N=CH-, -N=N-, -CH=CR 0 -、-CY 2 =CY 3 -, -C≡C-, -CH=CH-CO-O-, -O-CO-CH=CH- or a single bond,

[0117] R 0 and R 00 each independently of one another represents H or an alkyl group having 1 to 20 C atoms, and

[0118] Y 2 and Y 3 Each independently of one another represents H, F, Cl or CN.

[0119] X" is preferably -O-, -S-, -CO-, -COO-, -OCO-, -O-COO-, -CO-NR 0 -、-NR 0 -CO-、-NR 0 -CO-NR 00 - or single key.

[0120] Typical spacer groups Sp and -Sp"-X"- are, for example, -(CH2) p1 -、-(CH2) p1 -O-, -(CH2) p1 -O-CO-, -(CH2) p1 -CO-O-, -(CH2) p1 -O-CO-O-, -(CH2CH2O) q1 -CH2CH2-, -CH2CH2-S-CH2CH2-, -CH2CH2-NH-CH2CH2- or -(SiR 0 R 00 -O) p1 -, wherein p1 is an integer from 1 to 12, q1 is an integer from 1 to 3, and R 0 and R 00 Has the meaning as stated above.

[0121] Particularly preferred groups Sp and -Sp"-X"- are -(CH2) p1 -、-(CH2) p1 -O-, -(CH2) p1 -O-CO-, -(CH2) p1 -CO-O-, -(CH2) p1 -O-CO-O-, wherein p1 has one of the meanings specified above.

[0122] Particularly preferred radicals Sp" are in each case linear ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, nonylene, decylene, undecylene, dodecylene, octadecylene, ethyleneoxyethylene, methyleneoxybutylene, ethylenethioethylene, ethylene-N-methyliminoethylene, 1-methylalkylene, vinylene, propenylene and butenylene.

[0123] In a preferred embodiment of the invention, the compounds of formula IA and / or IB and subformulae thereof contain a spacer group Sp substituted by one or more polymerizable groups P, such that the group Sp-P corresponds to Sp(P) s , wherein s is ≥ 2 (branched polymerizable group).

[0124] Preferred compounds of formula IA and IB according to this preferred embodiment are those wherein s is 2, ie compounds containing the group Sp(P)2. Very preferred compounds of formula IA and IB according to this preferred embodiment contain a group selected from the following formulae:

[0125] -X-alkyl-CHPP S1

[0126] -X-alkyl-CH((CH2) aa P)((CH2) bb P)S2

[0127] -XN((CH2) aa P)((CH2) bb P)S3

[0128] -X-alkyl-CHP-CH2-CH2P S4

[0129] -X-alkyl-C(CH2P)(CH2P)-C aa H 2aa+1 S5

[0130] -X-alkyl-CHP-CH2P S6

[0131] -X-alkyl-CPP-C aa H 2aa+1 S7

[0132] -X-alkyl-CHPCHP-C aa H 2aa+1 S8

[0133] Wherein P is defined as Formula I,

[0134] Alkyl represents a single bond or a straight-chain or branched alkylene radical having 1 to 12 C atoms, which is unsubstituted or mono- or polysubstituted by F, Cl or CN and in which one or more non-adjacent CH2 groups may each independently of one another be substituted by -C(R) in such a way that the O and / or S atoms are not directly bonded to one another. 0 )=C(R 0 )-、-C≡C-、-N(R 0 )-, -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O- substitution, where R 0 has the meaning as stated above,

[0135] aa and bb each independently represent 0, 1, 2, 3, 4, 5 or 6,

[0136] X has one of the meanings given for X" and is preferably O, CO, SO2, O-CO-, CO-O or a single bond.

[0137] Preferred spacer groups Sp(P)2 are selected from the group consisting of formulae S1, S2 and S3.

[0138] Very preferred spacer groups Sp(P)2 are selected from the following sub-formulae:

[0139] -CHPP S1a

[0140] -O-CHPP S1b

[0141] -CH2-CHPP S1c

[0142] -OCH2-CHPP S1d

[0143] -CH(CH2-P)(CH2-P)S2a

[0144] -OCH(CH2-P)(CH2-P)S2b

[0145] -CH2-CH(CH2-P)(CH2-P)S2c

[0146] -OCH2-CH(CH2-P)(CH2-P)S2d

[0147] -CO-NH((CH2)2P)((CH2)2P)S3a

[0148] P is preferably selected from vinyloxy, acrylate, methacrylate, fluoroacrylate, chloroacrylate, oxetane and epoxy, very preferably acrylate and methacrylate, most preferably methacrylate.

[0149] It is further preferred that all polymerizable groups P present in the same compound have the same meaning and very preferably denote acrylate or methacrylate groups, most preferably methacrylate groups.

[0150] Sp preferably represents a single bond or -(CH2) p1 -、-(CH2) p2 -CH=CH-(CH2) p3 -、-O-(CH2) p1 -、-O-CO-(CH2) p1 , or -CO-O-(CH2) p1 , wherein p1 is 2, 3, 4, 5 or 6, preferably 2 or 3, p2 and p3 are independently 0, 1, 2 or 3 and, if Sp is -O-(CH2) p1 -、-O-CO-(CH2) p1 or -CO-O-(CH2) p1, then the O-atom or CO-group is connected to the benzene ring respectively.

[0151] In a preferred embodiment, in the compounds of formula IA and / or IB, at least one group Sp is a single bond.

[0152] In a very preferred embodiment, in the compounds of the formula IA and / or IB, all groups Sp are single bonds.

[0153] In a further preferred embodiment, in the compounds of the formula IA and / or IB, at least one group Sp is a single bond and at least one group Sp is different from a single bond.

[0154] If the group Sp is different from a single bond, it is preferably selected from -(CH2) p1 -、-(CH2) p2 -CH=CH-(CH2) p3 -、-O-(CH2) p1 -、-O-CO-(CH2) p1 or -CO-O-(CH2) p1 , wherein p1 is 2, 3, 4, 5 or 6, preferably 2 or 3, p2 and p3 are independently 0, 1, 2 or 3, and if Sp is -O-(CH2) p1 -、-O-CO-(CH2) p1 or -CO-O-(CH2) p1 , then the O-atom or CO-group is each attached to a benzene ring. Very preferably, if Sp is different from a single bond, it is selected from -(CH2)2-, -(CH2)3-, -(CH2)4-, -O-(CH2)2-, -O-(CH2)3-, -O-CO-(CH2)2 and -CO-O-(CH)2-, wherein the O atom or CO group is attached to a benzene ring.

[0155] Preferably, in the compounds of formula IA, all polymerizable groups P have the same meaning and very preferably denote acrylate or methacrylate, most preferably methacrylate.

[0156] Preferred compounds of formula IA are selected from the following subformulae:

[0157]

[0158]

[0159] wherein P, Sp and L have the meanings given in formula IA or one of the preferred meanings as given above and below, r1 is 0, 1, 2, 3 or 4 and r2 is 0, 1, 2 or 3.

[0160] Especially preferred are compounds of formula IA-1.

[0161] Very preferably the compounds of formula IA are selected from the following sub-formulae:

[0162]

[0163]

[0164]

[0165]

[0166] in which P, Sp and L have the meanings given in formula IA or one of their preferred meanings as given above and below, and Sp is different from a single bond.

[0167] Particularly preferred are compounds of the formulae IA-1-1 to IA-1-5, very preferred are compounds of the formulae IA-1-1 and IA-1-2, most preferred are compounds of the formula IA-1-1.

[0168] It is also preferred that the compounds of formula IA and its subformulae are selected from the following preferred embodiments (including any combination thereof):

[0169] - all groups P in the compound have the same meaning,

[0170] - all groups P in the compound represent methacrylate,

[0171] - the compound contains exactly two polymerizable groups (represented by the group P),

[0172] - the compound contains exactly three polymerizable groups (represented by the group P),

[0173] -P is selected from the group consisting of acrylates, methacrylates and oxetanes, very preferably acrylates or methacrylates, most preferably methacrylates,

[0174] - all groups Sp represent single bonds,

[0175] - all groups Sp are different from single bonds,

[0176] -When different from a single bond, Sp is -(CH2) p2 -、-(CH2) p2 -O-, -(CH2) p2 -CO-O-, -(CH2) p2 -O-CO-, wherein p2 is 2, 3, 4, 5 or 6, and the O-atom or CO-group is each attached to a benzene ring,

[0177] -L represents F, Cl, CH3, C2H5, OCH3, OC2H5, SCH3, SC2H5, -C(=O)H, -C(=O)CH3 or -C(=O)C2H5, very preferably F, OCH3, SCH3, -C(=O)H, -C(=O)CH3 or -C(=O)C2H5, most preferably -C(=O)H, -C(=O)CH3 or -C(=O)C2H5,

[0178] -r is 0,

[0179] -r is 1 or 2.

[0180] Very preferred compounds of formula IA and its subformulae are those of the following formula:

[0181]

[0182]

[0183] The present invention further relates to novel compounds of formula IA, in particular those selected from formula IA4, IA5 and IA7.

[0184] Preferred compounds of formula IB are selected from the following sub-formulae:

[0185]

[0186]

[0187]

[0188] in which P, Sp and L have the meanings given in formula IB or one of the preferred meanings given above and below,

[0189] r1, r2, r3 are independently 0, 1, 2, 3 or 4, and

[0190] r4 is 0, 1, 2 or 3.

[0191] Preferably, the compound of formula IB is selected from the group consisting of formula IB-1, IB-2, IB-3, IB-5, IB-6, IB-7 and IB-9, especially selected from the group consisting of formula IB-1, IB-2, IB-5, IB-6 and IB-9, more preferably from the group consisting of formula IB-1, IB-5 and IB-9, and most preferably from the group consisting of formula IB-1.

[0192] Very preferred are compounds of formula IB-1 to IB-12, wherein r1, r2 and r3 are 0. Also preferred are compounds of formula IB-1 to IB-12, wherein at least one of r1, r2 and r3 is not 0, more preferably wherein r1+r2+r3 is 1 or 2.

[0193] Additionally preferred are compounds of the formulae IB-1 to IB-12, in which all radicals P have the same meaning and denote acrylate or methacrylate, very preferably methacrylate.

[0194] Additionally preferred are compounds of the formulae IB-1 to IB-12 in which all radicals Sp represent single bonds.

[0195] Also preferred are compounds of the formulae IB-1 to IB-12, in which one or two groups Sp are different from a single bond and are preferably selected from -(CH2)2-, -(CH2)3-, -(CH2)4-, -O-(CH2)2-, -O-(CH2)3-, -O-CO-(CH2)2 and -CO-O-(CH)2-, in which the O atom or the CO group is attached to the benzene ring.

[0196] Additionally preferred are alkyl groups containing one or more, preferably exactly one, hydrocarbon group -C(R aa )(R bb )OH substituted group Sp of formula IB-1 to IB-12, wherein R aa and R bb independently of one another represent a straight-chain alkyl radical having 1 to 6 C atoms, or R aa and R bb Together with the C atom to which it is attached, it forms a cycloalkyl group having 3 to 12 C atoms, very preferably cyclopropyl, cyclobutyl, cyclopentyl or cyclohexyl, the one or more radicals Sp being very preferably substituted by -C(CH3)2-OH, -C(C2H5)2-OH or -C(CH3)(C2H5)OH, very preferably by -C(CH3)2-OH.

[0197] Also preferred are compounds of formulae IB-1 to IB-12, wherein L is selected from F, Cl, CH3, C2H5, OCH3, OC2H5, SCH3, SC2H5, -CH=CH2, -CH2-CH=CH2, -CH=CH-CH3, -CH=CH-CH=CH2 or -C(CH3)=CH2, -C(CH3)2-OH, -C(C2H5)2-OH or -C(CH3)(C2H5)OH, very preferably F, OCH3 or SCH3.

[0198] It is also preferred that the compound of formula IB is selected from the following sub-formulas

[0199]

[0200]

[0201]

[0202]

[0203]

[0204]

[0205]

[0206]

[0207]

[0208]

[0209]

[0210]

[0211]

[0212]

[0213]

[0214]

[0215]

[0216]

[0217]

[0218]

[0219] in which P, Sp and L, on each occurrence, identically or differently, have one of the meanings given in formula IB-T and Sp' has one of the meanings given for Sp which is different from a single bond.

[0220] Particularly preferred are compounds selected from the group consisting of formulae IB-1-1, IB-1-2, IB-1-3, IB-2-1, IB-2-2, IB-2-3, IB-5-1 to IB-5-11, IB-6- to IB-6-6, IB-9-1, IB-9-2, IB-10-1 and IB-10-2, especially those of formulae IB-1-1, IB-1-2, IB-1-3, IB-5-1 to IB-5-11, IB-9-1 and IB-9-2, very preferably those of formula IB-1-1.

[0221] It is also preferred that the compounds of formula IB and its subformulae are selected from the following preferred embodiments (including any combination thereof):

[0222] - all groups P in the compound have the same meaning,

[0223] - all groups P in the compound represent methacrylate,

[0224] - the compound contains exactly two polymerizable groups (represented by the group P),

[0225] - the compound contains exactly three polymerizable groups (represented by the group P),

[0226] -P is selected from the group consisting of acrylates, methacrylates and oxetanes, very preferably acrylates or methacrylates, most preferably methacrylates,

[0227] - all groups Sp represent single bonds,

[0228] - at least one radical Sp is different from a single bond,

[0229] -When different from a single bond, Sp or Sp' is -(CH2) p2 -、-(CH2) p2 -O-, -(CH2) p2 -CO-O-, -(CH2) p2 -O-CO-, wherein p2 is 2, 3, 4, 5 or 6, and the O-atom or CO-group is each attached to a benzene ring,

[0230] - the compound contains at least one, preferably exactly one, hydrocarbon group -C(R aa )(R bb ) OH-substituted group Sp, where R aa and R bb independently of one another represent a straight-chain alkyl radical having 1 to 6 C atoms, or R aa and R bb Together with the C atom to which it is attached, it forms a cycloalkyl radical having 3 to 12 C atoms, very preferably cyclopropyl, cyclobutyl, cyclopentyl or cyclohexyl

[0231] -L represents F, Cl, CH3, C2H5, OCH3, OC2H5, SCH3 or SC2H5, very preferably F, OCH3 or SCH3,

[0232] -L represents -CH=CH2, -CH2-CH=CH2, -CH=CH-CH3, -CH=CH-CH=CH2 or -C(CH3)=CH2,

[0233] -Sp is substituted by a group selected from -C(CH3)2-OH, -C(C2H5)2-OH and -C(CH3)(C2H5)OH, very preferably -C(CH3)2-OH,

[0234] -L represents -C(CH3)2-OH, -C(C2H5)2-OH and -C(CH3)(C2H5)OH, most preferably -C(CH3)2-OH,

[0235] -r1, r2, r3 and r4 represent 0 or 1,

[0236] -r1+r2 is 0,

[0237] -r1+r2 is 1,

[0238] -r3 is 0,

[0239] -r4 is 0.

[0240] Very preferably the compound of formula IB is selected from the following sub-formulae:

[0241]

[0242]

[0243]

[0244]

[0245]

[0246]

[0247]

[0248]

[0249]

[0250]

[0251]

[0252]

[0253]

[0254]

[0255]

[0256]

[0257]

[0258]

[0259]

[0260]

[0261]

[0262]

[0263]

[0264]

[0265]

[0266]

[0267]

[0268]

[0269] wherein "Me" is methyl and "Et" is ethyl.

[0270] In a preferred embodiment, the LC medium comprises a compound of formula IA1 and a compound selected from the group consisting of formulae IB1, IB2, IB3, IB6, IB11, IB25, IB33, IB55, IB70, IB89, IB110, IB113, IB133 and IB135.

[0271] In a preferred embodiment, the LC medium comprises at least one polymerizable compound of formula IA and / or formula IB having an absorption in the range of 300 to 380 nm. Very preferably, these compounds have an extinction coefficient of at least 0.5 at a wavelength in the range of 300 to 360 nm. Unless otherwise specified, the extinction coefficient and the absorption wavelength are measured in a solution of the compound in DCM at a concentration of 3 g / L.

[0272] The total proportion of polymerizable compounds of the formulae IA and IB and subformulae thereof in the LC media according to the invention is preferably from 0.1 to 2.5%, more preferably from 0.1 to 1.0%, very preferably from 0.2 to 0.6% by weight.

[0273] In a preferred embodiment of the present invention, the LC medium contains one or more, preferably exactly one, compounds of formula IA or a subformulae thereof and one or more, preferably exactly one, compounds of formula IB or a subformulae thereof, and preferably no further polymerizable compounds.

[0274] Preferably, in the LC media of this preferred embodiment, the proportion of the compound of the formula IA or its subformulae is 0.1 to 1.5% by weight, very preferably 0.2 to 1% by weight, and the proportion of the compound of the formula IB or its subformulae is 0.05 to 1.5% by weight, very preferably 0.1 to 1%.

[0275] Preferably, the proportion (in % by weight) of the compound of formula IA is higher than the proportion of the compound of formula IB.

[0276] In a further preferred embodiment, the LC medium comprises, besides the polymerizable compounds of the formulae IA, IB and subformulae thereof, at least one further polymerizable compound.

[0277] Preferably, the further polymerizable compound is selected from the following table D, in particular from the group consisting of the formulae RM-1, RM-4, RM-8, RM-17, RM-19, RM-35, RM-37, RM-39, RM-40, RM-41, RM-48, RM-52, RM-54, RM-57, RM-58, RM-64, RM-74, RM-76, RM-88, RM-91, RM-102, RM-103, RM-109, RM-116, RM-117, RM-120, RM-121, RM-122, R-139, RM-140, RM-142, RM-143, RM-145, RM-146, RM-147, RM-149, RM-156 to RM-163, RM-169, RM-170 and RM-171 to RM-183.

[0278] The proportion of these further polymerizable compounds in the LC medium is preferably from 0.01 to 1.5% by weight, more preferably from 0.05 to 0.9% by weight.

[0279] The polymerizable compounds as described above and below can be prepared analogously to the methods known to the person skilled in the art and described in standard works of organic chemistry, such as, for example, Houben-Weyl, Methoden der organischen Chemie [Methods of Organic Chemistry], Thieme-Verlag, Stuttgart and from commercially available or readily synthesizable starting substances. For example, starting substances for compounds of the formula IA, such as 2,5-dihydroxybenzaldehyde, 2,5-dihydroxyacetophenone, 2,5-dihydroxypropiophenone or 2-tert-butylhydroquinone, are commercially available.

[0280] For example, acrylates or methacrylates can be prepared by esterification of the corresponding alcohol or phenol with an acid derivative, such as (meth)acryloyl chloride or (meth)acrylic anhydride, in the presence of a base such as pyridine or triethylamine, and 4-(N,N-dimethylamino)pyridine (DMAP). Alternatively, esters can be prepared by esterification of alcohols with (meth)acrylic acid in the presence of a dehydrating agent, such as dicyclohexylcarbodiimide (DCC), N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide (EDC) or N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride according to Steglich and DMAP.

[0281] The invention also relates to an LC medium or an LC display as described above, wherein the polymerisable compound is present in polymerised form.

[0282] The LC display is preferably a PS-VA, PS-IPS, PS-FFS or SA-VA display.

[0283] To produce a PSA or polymer-stabilized SA display, the polymerizable compounds contained in the LC medium are polymerized by in situ polymerization in the LC medium between the substrates of the LC display, preferably while applying a voltage to the electrodes.

[0284] As described in the prior art cited at the outset, the structure of the display according to the invention corresponds to the usual geometries of PSA displays. Preference is given to geometries without protrusions, in particular those in which the electrode on the color filter side is unstructured and only the electrode on the TFT side has slots. Particularly suitable and preferred electrode structures for PS-VA displays are described, for example, in US 2006 / 0066793 A1.

[0285] Preferred LC displays of the PSA type according to the invention comprise:

[0286] a first substrate comprising a pixel electrode defining a pixel area, the pixel electrode being connected to a switching element disposed in each pixel area and optionally comprising a micro-slit pattern, and optionally a first alignment layer disposed on the pixel electrode,

[0287] a second substrate comprising a common electrode layer, which may be arranged on the entire portion of the second substrate facing the first substrate, and optionally a second alignment layer,

[0288] - an LC layer arranged between the first substrate and the second substrate and comprising an LC medium as described above and below, wherein the polymerisable compound may also be present in polymerised form.

[0289] The first and / or second alignment layer controls the alignment direction of the LC molecules of the LC layer. For example, in a PS-VA display, the alignment layer is selected so that it imparts a vertical (or perpendicular) alignment (i.e. perpendicular to the surface) or a tilted alignment to the LC molecules. Such an alignment layer may, for example, comprise polyimide, which may also be rubbed, or may be prepared by a photoalignment method.

[0290] The LC layer with the LC medium can be deposited between the substrates of the display by methods conventionally used by display manufacturers, such as the so-called one-drop-filling (ODF) method. The polymerizable components of the LC medium are then polymerized, for example, by UV photopolymerization. The polymerization can be carried out in one step or in two or more steps.

[0291] The PSA display may include further elements such as colour filters, a black matrix, a passivation layer, an optical retardation layer, transistor elements for addressing the individual pixels etc., which are well known to those skilled in the art and may be used without inventive skill.

[0292] The electrode structure can be designed by technicians according to each display type. For example, for PS-VA displays, multi-domain orientation of LC molecules can be induced by providing electrodes with slits and / or ridges or protrusions to produce two, four or more different tilted alignment directions.

[0293] After polymerization, the polymerizable compound forms a copolymer, which results in a certain tilt angle of the LC molecules in the LC medium. Without wishing to be bound by a particular theory, it is believed that at least a portion of the cross-linked polymer formed by the polymerizable compound will phase separate or precipitate from the LC medium and form a polymer layer on the substrate or electrode, or on an alignment layer disposed thereon. Microscopic measurement data (such as SEM and AFM) have confirmed that at least a portion of the formed polymer accumulates at the LC / substrate interface.

[0294] It is also possible to polymerize in a first step to produce the tilt angle, optionally with simultaneous application of a voltage, and then polymerize or crosslink the unreacted compounds of the first step in a second polymerization step without application of a voltage ("final curing").

[0295] Suitable and preferred polymerisation methods are, for example, thermal polymerisation or photopolymerisation, preferably photopolymerisation, in particular UV-induced photopolymerisation, which may be achieved by exposing the polymerisable compound to UV radiation.

[0296] Preferred methods of making PSA displays include one or more of the following features (including any combination thereof):

[0297] - exposing the polymerizable medium in the display to UV light in a 2-step process comprising a first UV exposure step ("UV1 step"), in which a voltage is applied to produce the tilt angle, and a second UV exposure step ("UV2 step"), in which no voltage is applied to complete the polymerization,

[0298] - irradiating the polymerizable medium using a UV radiation source having an emission spectrum ≥ 300 nm, preferably in the range of 300 to 380 nm, very preferably in the range of 300 to 360 nm, preferably at least in a UV2 step, more preferably in both UV1 and UV2 steps,

[0299] - irradiating the polymerizable medium, using as radiation source a UV C type lamp, preferably at least in the UV1 step, more preferably in both the UV1 and UV2 steps,

[0300] - Irradiating the polymerizable medium, as UV radiation source, using a UV C lamp in the UV1 step and a UV B lamp in the UV2 step.

[0301] A preferred embodiment of the present invention relates to a method for preparing a PSA display as described above and below, comprising one or more of the following features (including any combination thereof):

[0302] - irradiating the polymerizable LC medium by UV light in a 2-step process comprising a first UV exposure step ("UV1 step"), wherein a voltage is applied to generate the tilt angle, and a second UV exposure step ("UV2 step"), without applying a voltage, to complete the polymerisation,

[0303] - The polymerizable LC medium is passed through a 2 Up to 10mW / cm 2 irradiation with UV light generated by a UV lamp with an intensity of , preferably in the UV2 step, and optionally also in the UV1 step,

[0304] - irradiating the polymerizable LC medium by UV light having a wavelength preferably >300 nm,

[0305] - irradiating the polymerizable LC medium with UV light while applying voltage to the electrodes of the display,

[0306] - the irradiation with UV light is carried out using a UV C type lamp, preferably at least in the UV2 step, more preferably in both the UV1 and UV2 steps,

[0307] - by irradiation with UV light using a UV C lamp in the UV1 step and a UV B lamp in the UV2 step,

[0308] - Irradiation by UV light is performed using UV-LED type lamps, preferably at least in the UV2 step, more preferably in both UV1 and UV2 steps.

[0309] This preferred method can be performed, for example, by using the desired UV lamp or by using a bandpass filter and / or a cut-off filter, which substantially transmits UV light having the respective desired wavelength and substantially blocks light having the respective undesired wavelength.

[0310] Preferably, UV irradiation is performed using a UV C-type lamp, preferably at least in the UV2 step, more preferably in both UV1 and UV2 steps, or using a C-type lamp in the UV1 step and a B-type lamp in the UV2 step.

[0311] The UV radiation energy is preferably in the range of 2 to 100 J, depending on the production process conditions.

[0312] The LC media according to the present invention may additionally comprise one or more other ingredients or additives, preferably selected from the following list including, but not limited to, comonomers, chiral dopants, polymerization initiators, inhibitors, stabilizers, surfactants, wetting agents, lubricants, dispersants, hydrophobic agents, binders, flow improvers, defoamers, deaerators, diluents, reactive diluents, auxiliaries, colorants, dyes, pigments and nanoparticles.

[0313] The LC medium preferably has a nematic LC phase.

[0314] In a preferred embodiment, the LC medium comprises one or more polymerization initiators. Suitable polymerization conditions and suitable initiator types and amounts are known to the person skilled in the art and are described in the literature. Suitable for free-radical polymerization are, for example, commercially available photoinitiators or (Ciba AG). If a polymerization initiator is used, its proportion is preferably from 0.001 to 5% by weight, particularly preferably from 0.001 to 1% by weight.

[0315] The polymerizable compounds according to the invention are also suitable for polymerization without initiators, which has considerable advantages, for example lower material costs and, in particular, less contamination of the LC medium with possible residual amounts of initiator or degradation products thereof.

[0316] Thus, the polymerization can also be carried out without addition of initiators. Thus, in a further preferred embodiment, the LC medium contains no polymerization initiator.

[0317] In a further preferred embodiment, the LC medium additionally comprises one or more stabilizers to prevent undesired spontaneous polymerization of the RMs, for example during storage or transport. Suitable types and amounts of stabilizers are known to the person skilled in the art and are described in the literature. Particularly suitable are, for example, Series (Ciba AG) commercially available stabilizers, such as 1076. If stabilizers are used, their proportion, based on the total amount of RM or polymerizable component (component A), is preferably 10 to 50,000 ppm, particularly preferably 50 to 5,000 ppm.

[0318] In a preferred embodiment, the LC medium contains one or more chiral dopants, preferably in a concentration of 0.01-1 wt %, very preferably 0.05-0.5 wt %. The chiral dopant is preferably selected from the compounds of Table B below, very preferably R- or S-1011, R- or S-2011, R- or S-3011, R- or S-4011 and R- or S-5011.

[0319] In another preferred embodiment, the LC medium contains the racemate of one or more chiral dopants, which are preferably selected from the chiral dopants mentioned in the previous paragraph.

[0320] In a further preferred embodiment of the present invention, the LC medium contains one or more additional stabilizers.

[0321] Preferably the stabilizer is selected from compounds of formula H

[0322]

[0323] in

[0324] Ar represents an aromatic or heteroaromatic hydrocarbon group having 4 to 40 C atoms, preferably 6 to 30 C atoms;

[0325] Sp represents a spacer group;

[0326] R S represents H, alkyl having 1 to 12 C atoms or alkenyl having 2 to 12 C atoms;

[0327] Z S Indicates -O-, -C(O)O-, -(CH2) z -or-(CH2) z O- or single bond;

[0328] HA means

[0329] R H Indicates H, O . , CH3, OH or OR S, preferably H or O;

[0330] R S1 , R S2 , R S3 and R S4 represent, identically or differently, alkyl having 1 to 6 C atoms, preferably having 1 to 3 C atoms, very preferably CH3;

[0331] G stands for H or R S or group Z S -HA;

[0332] z is an integer from 1 to 6; and

[0333] q is 3 or 4.

[0334] Compounds of formula H are described in EP3354710A1 and EP3354709A1.

[0335] Preferably, the compound of formula H is selected from formula H-1, H-2 and H-3:

[0336]

[0337]

[0338] Where R H has the meaning given above and preferably represents H or O . , and n is an integer from 0 to 12, preferably 5, 6, 7, 8 or 9, very preferably 7, and Sp represents a spacer group, preferably an alkylene group having 1 to 12 C atoms, wherein one or more non-adjacent -CH2- groups may be replaced by -O-.

[0339] Preferred compounds of formula H-1 are those of formula H-1-1:

[0340]

[0341] Where R H has the meanings given above and preferably denotes H or O., and n is an integer from 0 to 12, preferably 5, 6, 7, 8 or 9, very preferably 7.

[0342] Very preferred compounds of formula H-1-1 are those of formula H-1-1-1:

[0343]

[0344] Preferred compounds of formula H-2 are those of formula H-2-1:

[0345]

[0346] Where RH has the meaning given above and preferably represents H or O . , and n2 is, at each occurrence, identically or differently, preferably identically, an integer from 1 to 12, preferably 2, 3, 4, 5 or 6, very preferably 3, and R S On each occurrence, identically or differently, preferably identically, represents alkyl having 1 to 6 C atoms, preferably n-butyl.

[0347] Very preferred compounds of formula H-2-1 are those of formula H-2-1-1:

[0348]

[0349] Preferably, the compound of formula H-3 is selected from formula H-3-1:

[0350]

[0351] Among them, Sp and R H has the meaning given above and R H Preferably represents H or O . , and n is an integer from 0 to 12, preferably 5, 6, 7, 8 or 9, very preferably 7. It is further preferred that the stabilizer is selected from the group consisting of the formulae ST-1 to ST-18:

[0352]

[0353]

[0354]

[0355] in

[0356] R ST represents H, an alkyl group or an alkoxy group having 1 to 15 C atoms, wherein one or more CH2 groups may each independently of one another be connected via -C≡C-, -CF2O-, -OCF2-, -CH=CH-, -O-, -CO-O-, -O-CO-, and in addition, one or more H atoms may be replaced by halogen,

[0357] Each time it appears, it means the same or different

[0358] Z STeach independently represents -CO-O-, -O-CO-, -CF2O-, -OCF2-, -CH2O-, -OCH2-, -CH2-, -CH2CH2-, -(CH2)4-, -CH=CH-, -CH2O-, -C2F4-, -CH2CF2-, -CF2CH2-, -CF=CF-, -CH=CF-, -CF=CH-, -CH=CH-, -C≡C- or a single bond,

[0359] L 1 and L 2 each independently represents F, Cl, CH3, CF3 or CHF2,

[0360] p represents 0, 1 or 2,

[0361] q represents 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10.

[0362] Preferred compounds of formula ST are those selected from formula ST-3 and in particular:

[0363]

[0364] wherein n=1, 2, 3, 4, 5, 6 or 7, preferably n=3

[0366]

[0367] wherein n=1, 2, 3, 4, 5, 6 or 7, preferably n=3

[0369]

[0370] wherein n=1, 2, 3, 4, 5, 6 or 7, preferably n=1 or 7

[0371]

[0372]

[0373] In the compounds of formulae ST-3a and ST-3b, n preferably represents 3. In the compounds of formula ST-2a, n preferably represents 7.

[0374] Very preferably, the stabilizer is selected from the group of compounds of formula ST-2a-1, ST-3a-1, ST-3b-1, ST-8-1, ST-9-1 and ST-12:

[0375]

[0376]

[0377] In another preferred embodiment, the LC medium comprises one or more stabilizers selected from Table C below.

[0378] Preferably, the proportion of stabilizer in the LC medium is from 10 to 500 ppm, very preferably from 20 to 100 ppm.

[0379] In another preferred embodiment, the LC media according to the invention contain a self-aligning (SA) additive, preferably in a concentration of 0.1-2.5%.

[0380] In a preferred embodiment, the SA-VA display according to the invention does not contain a polyimide alignment layer. In another preferred embodiment, the SA-VA display according to the preferred embodiment contains a polyimide alignment layer.

[0381] Preferred SA additives for this preferred embodiment are selected from compounds comprising a mesogenic group and a linear or branched alkyl side chain terminated by one or more polar anchoring groups selected from hydroxyl, carboxyl, amino or thiol groups.

[0382] Further preferred SA additives contain one or more polymerisable groups, which are optionally linked to the mesogenic group via a spacer group.These polymerisable SA additives can be polymerised in the LC medium under similar conditions as used for RMs in the PSA process.

[0383] Suitable SA additives for inducing vertical alignment, especially SA additives for SA-VA mode displays are disclosed in, for example, US2013 / 0182202 A1, US2014 / 0838581 A1, US2015 / 0166890 A1, and US2015 / 0252265 A1.

[0384] In a further preferred embodiment, the LC media or polymer-stabilized SA-VA displays according to the invention contain one or more self-aligning additives selected from Table E below.

[0385] In another preferred embodiment, the LC media according to the invention contain one or more SA additives, preferably selected from formula II or subformulae thereof or from Table E, in a concentration of 0.1 to 5%, very preferably 0.2 to 3%, most preferably 0.2 to 1.5%.

[0386] In addition to the above-mentioned polymerizable compounds and additives, the LC medium for use in the LC displays of the invention comprises an LC mixture ("host mixture") comprising one or more, preferably two or more, LC compounds selected from non-polymerizable low molecular weight compounds, of which at least one is a compound of formula II. These LC compounds are selected such that they are stable and / or unreactive towards polymerization reactions under the polymerization conditions applied to the polymerizable compounds.

[0387] Particularly preferred embodiments of such LC media are shown below.

[0388] Preferably, the LC medium contains one or more compounds of formula II selected from compounds of formula IIA, IIB, IIC and IID

[0389]

[0390]

[0391] The individual radicals have the following meanings each time they occur, identically or differently and independently of one another:

[0392] R 21 , R 22 is H, alkyl, alkoxy or alkenyl with up to 15 C atoms, which is unsubstituted or monosubstituted by F, Cl, CN or CF3 and in addition, one or more CH2 groups in these groups can be connected via -O-, -S-, -C≡C-, -CF2O-, -OCF2-, -OC-O, -O-CO-, -S-, -C≡C ... Instead,

[0393] L 1 To L 4 is F, Cl, CF3 or CHF2,

[0394] Y is H, F, Cl, CF3, CHF2 or CH3, preferably H or CH3, particularly preferably H,

[0395] Z 1 , Z 2 is a single bond, -CH2CH2-, -CH=CH-, -CF2O-, -OCF2-, -CH2O-, -OCH2-, -COO-, -OCO-, -C2F4-, -CF=CF-, -CH=CHCH2O-,

[0396] p is 0, 1, or 2, and

[0397] q is 0 or 1.

[0398] Preferred compounds of formula IIA, IIB, IIC and IID are those wherein R 22 represents an alkyl or alkoxy radical having up to 15 C atoms, and very preferably represents (O)C v H 2v+1 , those wherein (O) is an oxygen atom or a single bond and v is 1, 2, 3, 4, 5 or 6.

[0399] Additionally preferred are compounds of formula IIA, IIB, IIC and IID wherein R 21 or R 22 represents or contains a cycloalkyl or cycloalkoxy group, preferably selected from

[0400] The group consisting of S 1 C 1-12 -alkylene or C 2-12 -alkenylene and S 2 H, C 1-12 -alkyl or C 2-12 -alkenyl, and very preferably selected from Those that consist of groups.

[0401] Additional preferred compounds of formulae IIA, IIB, IIC and IID are specified below.

[0402] In a preferred embodiment, the LC medium comprises one or more compounds of formula IIA selected from the group consisting of:

[0403]

[0404]

[0405]

[0406]

[0407]

[0408]

[0409]

[0410]

[0411]

[0412]

[0413]

[0414] wherein the index a denotes 1 or 2, alkyl and alkyl* each independently denote a straight-chain alkyl group having 1 to 6 C atoms, alkenyl denotes a straight-chain alkenyl group having 2 to 6 C atoms, and (O) denotes an oxygen atom or a single bond, and alkenyl preferably denotes CH2=CH-, CH2=CHCH2CH2-, CH3-CH=CH-, CH3-CH2-CH=CH-, CH3-(CH2)2-CH=CH-, CH3-(CH2)3-CH=CH- or CH3-CH=CH-(CH2)2-.

[0415] Particularly preferred LC media according to the invention comprise one or more compounds selected from the group consisting of formulae IIA-2, IIA-8, IIA-10, IIA-16, IIA-18, IIA-40, IIA-41, IIA-42 and IIA-43.

[0416] In another preferred embodiment, the LC medium comprises one or more compounds of the formula IIB selected from the group consisting of formulae IIB-1 to IIB-26

[0417]

[0418]

[0419]

[0420]

[0421] wherein alkyl and alkyl* each independently represent a straight-chain alkyl group having 1 to 6 C atoms, alkenyl represents a straight-chain alkenyl group having 2 to 6 C atoms, and (O) represents an oxygen atom or a single bond, and alkenyl preferably represents CH2=CH-, CH2=CHCH2CH2-, CH3-CH=CH-, CH3-CH2-CH=CH-, CH3-(CH2)2-CH=CH-, CH3-(CH2)3-CH=CH- or CH3-CH=CH-(CH2)2-.

[0422] Particularly preferred LC media according to the invention comprise one or more compounds selected from the group consisting of formulae IIB-2, IIB-10 and IIB-16.

[0423] In another preferred embodiment, the LC medium comprises one or more compounds of formula IIC selected from formula IIC-1

[0424]

[0425] Therein, alkyl and alkyl* each independently of one another denote a straight-chain alkyl radical having 1 to 6 C atoms, preferably in an amount of 0.5 to 5% by weight, in particular 1 to 3% by weight.

[0426] In another preferred embodiment, the LC medium comprises one or more compounds of formula IID selected from the group consisting of

[0427]

[0428]

[0429]

[0430] wherein alkyl and alkyl* each independently represent a straight-chain alkyl group having 1 to 6 C atoms, alkenyl represents a straight-chain alkenyl group having 2 to 6 C atoms, and (O) represents an oxygen atom or a single bond, and alkenyl preferably represents CH2=CH-, CH2=CHCH2CH2-, CH3-CH=CH-, CH3-CH2-CH=CH-, CH3-(CH2)2-CH=CH-, CH3-(CH2)3-CH=CH- or CH3-CH=CH-(CH2)2-.

[0431] Particularly preferred LC media according to the invention comprise one or more compounds of the formula IID-4.

[0432] Very preferably, the compound of formula IID is selected from the following sub-formula

[0433]

[0434]

[0435]

[0436]

[0437]

[0438] where v is 1, 2, 3, 4, 5, or 6.

[0439] In a preferred embodiment, the LC medium comprises one or more compounds of formula IID-10a

[0440]

[0441] Where R 21 , Y and q have the meanings given in Formula IID, and R 23 for wherein r is 0, 1, 2, 3, 4, 5 or 6 and s is 1, 2 or 3.

[0442] Preferred compounds of formula IID-10a are compounds IID-10a-1 to IID-10a-14:

[0443]

[0444]

[0445] Particularly preferred LC media according to the invention comprise one or more compounds selected from the group consisting of formulae IIA-2, IIA-8, IIA-10, IIA-16, II-18, IIA-40, IIA-41, IIA-42, IIA-43, IIB-2, IIB-10, IIB-16, IIC-1 and IID-4 and IID-10 or subformulae thereof.

[0446] The proportion of compounds of the formula IIA and / or IIB in the mixture as a whole is preferably at least 20% by weight.

[0447] Preferably, the LC medium comprises one or more compounds of formula IIA-2 selected from the following subformulae:

[0448]

[0449] Alternatively, preferably in addition to the compounds of the formulae IIA-2-1 to IIA-2-5, the LC medium comprises one or more compounds of the following formulae:

[0450]

[0451]

[0452] Additionally preferably, the LC medium comprises one or more compounds of formula IIA-10 selected from the following subformulae:

[0453]

[0454]

[0455] Alternatively, preferably in addition to the compounds of the formulae IIA-10-1 to IIA-10-5, the LC medium comprises one or more compounds of the following formulae:

[0456]

[0457] Preferably, the LC medium comprises one or more compounds of formula IIB-10 selected from the following subformulae:

[0458]

[0459] Alternatively, preferably in addition to the compounds of the formulae IIB-10-1 to IIB-10-5, the LC medium comprises one or more compounds of the formulae IIB-10a-1 to IIB-10a-5:

[0460]

[0461]

[0462] In another preferred embodiment, the LC medium comprises one or more compounds of the formula III which are different from the formula IA,

[0463]

[0464] where the individual radicals independently of one another and on each occurrence have the following meanings identically or differently

[0465] R 31 , R 32 is H, alkyl, alkoxy or alkenyl with up to 15 C atoms, which is unsubstituted, monosubstituted by F, Cl, CN or CF3 or at least monosubstituted by halogen, wherein, in addition, one or more CH2 groups in these radicals can be connected via -O-, -S-, -H-, -H- or -S- in such a way that the O atoms are not directly connected to one another. -C≡C-, -CF2O-, -OCF2-, -OC-O- or -O-CO-,

[0466] A 3 a) 1,4-cyclohexenylene or 1,4-cyclohexylene, in which one or two non-adjacent CH2 groups may be replaced by -O- or -S-,

[0467] b) 1,4-phenylene, in which one or both CH groups may be replaced by N, or

[0468] c) a group selected from the group consisting of spiro[3.3]heptane-2,6-diyl, 1,4-bicyclo[2.2.2]octane-2,6-diyl, naphthalene-2,6-diyl, decahydronaphthalene-2,6-diyl, 1,2,3,4-tetrahydronaphthalene-2,6-diyl, phenanthrene-2,7-diyl and fluorene-2,7-diyl,

[0469] wherein the groups a), b) and c) may be singly or polysubstituted by halogen atoms,

[0470] n is 0, 1 or 2, preferably 0 or 1,

[0471] Z 1is -CO-O-, -O-CO-, -CF2O-, -OCF2-, -CH2O-, -OCH2-, -CH2-, -CH2CH2-, -(CH2)4-, -CH=CH-CH2O-, -C2F4-, -CH2CF2-, -CF2CH2-, -CF=CF-, -CH=CF-, -CF=CH-, -CH=CH-, -C≡C- or a single bond,

[0472] L 11 , L 12 is F, Cl, CF3 or CHF2, preferably H or F, most preferably F,

[0473] W is O or S,

[0474] Y 1 , Y 2 It is H, F, Cl, CF3, CHF2, CH3 or OCH3, preferably H, CH3 or OCH3, very preferably H.

[0475] In the compound of formula III, R 31 and R 32 It is preferably selected from straight-chain alkyl or alkoxy having 1 to 12, preferably 1 to 7 C atoms, straight-chain alkenyl having 2 to 12, preferably 2 to 7 C atoms and cycloalkyl or cycloalkoxy having 3 to 12, preferably 3 to 8 C atoms.

[0476] In a preferred embodiment of the present invention, the LC medium comprises one or more compounds of formula III-1 or III-2

[0477]

[0478] The radicals occurring therein have the same meanings as given above under formula III and are preferably

[0479] R 31 and R 32 each independently of one another is alkyl, alkenyl or alkoxy having up to 15 C atoms, more preferably one or both of them represent alkoxy and

[0480] L 11 and L 12 Each preferably represents F.

[0481] In another preferred embodiment, the LC medium comprises one or more compounds of the formula III-1 selected from the group of compounds of the formulae III-1-1 to III-1-10, preferably compounds of the formula III-1-6,

[0482]

[0483]

[0484] wherein alkyl and alkyl* each independently represent a straight-chain alkyl group having 1 to 6 C atoms, alkenyl and alkenyl* each independently represent a straight-chain alkenyl group having 2 to 6 C atoms, alkoxy and alkoxy* each independently represent a straight-chain alkoxy group having 1 to 6 C atoms, and L 11 and L 12 Each independently represents F or Cl, preferably both are F.

[0485] In another preferred embodiment, the LC medium comprises one or more compounds of the formula III-2 selected from the group of compounds of the formulae III-2-1 to III-2-10, preferably compounds of the formula III-2-1,

[0486]

[0487]

[0488] wherein alkyl and alkyl* each independently represent a straight-chain alkyl group having 1 to 6 C atoms, alkenyl and alkenyl* each independently represent a straight-chain alkenyl group having 2 to 6 C atoms, alkoxy and alkoxy* each independently represent a straight-chain alkoxy group having 1 to 6 C atoms, and L 11 and L 12 Each independently represents F or Cl, preferably both are F.

[0489] Very preferably, the compound of formula III-2 is selected from the group consisting of the following sub-formulae wherein

[0490]

[0491]

[0492] Alkoxy represents straight-chain alkoxy having 1 to 6 C atoms, preferably ethoxy, propoxy, butoxy or pentoxy, very preferably ethoxy or propoxy. Very preferred are compounds of the formulae III-2-1-3, III-2-1-4 and III-2-1-5.

[0493] In another preferred embodiment of the present invention, the LC medium comprises one or more compounds of formula III-3-1

[0494]

[0495] Where L 11 and L 12have the same meanings as given under formula III, (O) represents O or a single bond,

[0496] R 33 represents an alkyl or alkenyl group or a group Cy-C having up to 7 C atoms m H 2m+1 -,

[0497] m and n are identical or different and are 0, 1, 2, 3, 4, 5 or 6, preferably 1, 2 or 3, very preferably 1, and

[0498] Cy denotes a cycloaliphatic radical having 3, 4 or 5 ring atoms, optionally substituted by alkyl or alkenyl each having up to 3 C atoms, or by halogen or CN, and preferably denotes cyclopropyl, cyclobutyl or cyclopentyl.

[0499] Instead of or in addition to the compound of the formula III, preferably in addition to the compound of the formula III, a compound of the formula III3-1 is contained in the LC medium.

[0500] Very preferably the compound of formula III3-1 is the following

[0501]

[0502]

[0503] Here, alkoxy represents a straight-chain alkoxy group having 1 to 6 C atoms.

[0504] In another preferred embodiment of the present invention, the LC medium comprises one or more compounds of formulae III-4 to III-6, preferably compounds of formula III-5

[0505]

[0506] where the parameters have the meanings given above, R 11 Preferably represents a straight chain alkyl group and R 12 Preferably denotes alkoxy, each having 1 to 7 C atoms.

[0507] In another preferred embodiment, the LC medium comprises one or more compounds of formula I selected from the group of compounds of formulae III-7 to III-9, preferably compounds of formula III-8,

[0508]

[0509]

[0510] where the parameters have the meanings given above, R 11 Preferably represents a straight chain alkyl group and R12 Preferably denotes alkoxy, each having 1 to 7 C atoms.

[0511] In a preferred embodiment, the LC medium comprises one or more compounds of formula IV

[0512]

[0513] in

[0514] R 41 represents an unsubstituted alkyl radical having 1 to 7 C atoms, in which, moreover, one or more CH2 groups may be substituted or unsubstituted alkenyl having 2 to 7 C atoms, preferably n-alkyl, particularly preferably having 2, 3, 4 or 5 C atoms, and

[0515] R 42 represents unsubstituted alkyl having 1 to 7 C atoms or unsubstituted alkoxy having 1 to 6 C atoms (each preferably having 2 to 5 C atoms), unsubstituted alkenyl having 2 to 7 C atoms (preferably having 2, 3 or 4 C atoms), more preferably vinyl or 1-propenyl and in particular vinyl.

[0516] The compound of formula IV is preferably selected from the group consisting of compounds of formula IV-1 to IV-3.

[0517]

[0518] in

[0519] Alkyl and alkyl' independently of one another denote an alkyl group having 1 to 7 C atoms, preferably 2 to 5 C atoms,

[0520] Alkenyl is an alkenyl radical having 2 to 5 C atoms, preferably having 2 to 4 C atoms, particularly preferably 2 C atoms,

[0521] alkenyl′ denotes an alkenyl group having 2 to 5 C atoms, preferably having 2 to 4 C atoms, particularly preferably having 2 to 3 C atoms, and

[0522] Alkoxy represents an alkoxy group having 1 to 5 C atoms, preferably having 2 to 4 C atoms.

[0523] Preferably, the LC medium comprises one or more compounds selected from the group consisting of compounds of formulae IV-1-1 to IV-1-6:

[0524]

[0525] Very preferably, the LC media according to the invention comprise one or more compounds of the formula IV-2-1 and / or IV-2-2

[0526]

[0527]

[0528] Very preferably, the LC media according to the invention comprise a compound of the formula IV-3, in particular a compound selected from the group consisting of the formulae IV-3-1 to IV-3-9:

[0529]

[0530]

[0531] In a further preferred embodiment, the LC media according to the invention comprise one or more compounds of the formula IV-3 selected from the compounds of the formulae IV-3-10 to IV-3-27:

[0532]

[0533]

[0534]

[0535] wherein alkyl represents methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or n-pentyl.

[0536] Very preferably, the LC media according to the invention comprise a compound of the formula IV-4, in particular a compound selected from the following formulae:

[0537]

[0538] In another preferred embodiment, the LC medium comprises one or more compounds of formula IV-4 and its subformulae, wherein one or both of "alkenyl" and "alkenyl'" represent Wherein m is 0, 1 or 2, and n is 0, 1 or 2, very preferably selected from the compounds of formulae IV-4-3 to IV-4-6.

[0539] Very preferably, the LC medium according to the invention comprises one or more compounds of the formula IV-1 or its subformulae and / or one or more compounds of the formula IV-3 or its subformulae and / or one or more compounds of the formula IV-4 or its subformulae, wherein the total concentration of these compounds of the formula IV-1 is in the range from 1% to 30%.

[0540] The LC media according to the invention preferably additionally comprise one or more compounds of the formula IVa,

[0541]

[0542] in

[0543] R 41 and R 42 each independently of one another represents a straight-chain alkyl, alkoxy, alkenyl or alkoxyalkyl radical having up to 12 C atoms,

[0544] express

[0545]

[0546] Z 4 It represents a single bond, -CH2CH2-, -CH=CH-, -CF2O-, -OCF2-, -CH2O-, -OCH2-, -COO-, -OCO-, -C2F4-, -C4H8- or -CF=CF-.

[0547] Preferred compounds of formula IVa are specified below:

[0548]

[0549] Here, alkyl and alkyl* each independently represent a straight-chain alkyl radical having 1 to 6 C atoms.

[0550] The LC media according to the invention preferably comprise at least one compound of the formula IVa-1 and / or formula IVa-2.

[0551] The proportion of the compound of the formula IVa in the mixture as a whole is preferably at least 5% by weight.

[0552] Preferably, the LC medium comprises one or more compounds of the formulae IVb-1 to IVb-3

[0553]

[0554] in

[0555] Alkyl and alkyl* each independently represent a straight-chain alkyl radical having 1 to 6 C atoms, and

[0556] Alkenyl and alkenyl* each independently of one another represent straight-chain alkenyl having 2 to 6 C atoms.

[0557] The proportion of compounds of the formulae IV-1 to IV-3 in the mixture as a whole is preferably at least 3% by weight, in particular ≥5% by weight.

[0558] Among the compounds of formulae IVb-1 to IVb-3, the compound of formula IVb-2 is particularly preferred.

[0559] Particularly preferred compounds of formulae IV-1 to IV-3 are selected from the group consisting of the following formulae:

[0560]

[0561]

[0562] Therein alkyl* denotes alkyl having 1 to 6 C atoms and preferably denotes n-propyl.

[0563] The LC media according to the invention particularly preferably comprise one or more compounds of the formula IVb-1-1 and / or IVb-2-3.

[0564] In a further preferred embodiment, the LC media according to the invention comprise one or more compounds of the formula V

[0565]

[0566] in

[0567] R 51 and R 52 independently of one another denotes H, alkyl, alkoxy or alkenyl having up to 15 C atoms, which is unsubstituted, monosubstituted by F, Cl, CN or CF3 or at least monosubstituted by halogen, wherein, moreover, one or more CH2 groups in these radicals may be connected via -O-, -S-, -C≡C-, -CF2O-, -OCF2-, -OC-O, -O-CO-, -S-, -C≡C ... , and preferably represents alkyl with 1 to 7 C atoms, preferably n-alkyl, particularly preferably n-alkyl with 1 to 5 C atoms, alkoxy with 1 to 6 C atoms, preferably n-alkoxy, particularly preferably n-alkoxy with 2 to 5 C atoms, alkoxyalkyl with 2 to 7 C atoms, preferably with 2 to 4 C atoms, alkenyl or alkenyloxy, preferably alkenyloxy,

[0568] Same or different

[0569]

[0570] in

[0571] Preferably means

[0572] Z 51 , Z 52Each independently represents -CH2-CH2-, -CH2-O-, -CH=CH-, -C≡C-, -COO- or a single bond, preferably -CH2-CH2-, -CH2-O- or a single bond and particularly preferably a single bond, and

[0573] n is 1 or 2.

[0574] The compound of formula V is preferably selected from the compounds of formula V-1 to V-17:

[0575]

[0576]

[0577] Where R 1 and R 2 With the above R 51 and R 52 The specified meaning.

[0578] R 1 and R 2 Preferably each independently of one another represents a straight-chain alkyl or alkenyl group.

[0579] Preferably, the LC medium comprises one or more compounds of formula V-1, V-3, V-4, V-6, V-7, V-10, V-11, V-12, V-14, V-15 and / or V-16.

[0580] The LC media according to the invention very particularly preferably comprise compounds of the formula V-10 and / or IV-1, in particular in an amount of 5 to 30%.

[0581] Preferred compounds of formula V-10 are specified below:

[0582]

[0583] The LC medium according to the invention particularly preferably comprises a tricyclic compound of the formula V-10a and / or V-10b in combination with one or more bicyclic compounds of the formula IV-1. The total proportion of the combination of the compounds of the formula V-10a and / or V-10b and one or more compounds selected from the group consisting of the bicyclohexyl compounds of the formula IV-1 is 5 to 40%, very particularly preferably 15 to 35%.

[0584] Particularly preferred LC media comprise compounds V-10a and IV-1-1:

[0585]

[0586]

[0587] The compounds V-10a and IV-1-1 are preferably present in the mixture in a concentration of 5 to 30%, very preferably 10 to 25%, based on the mixture as a whole.

[0588] Preferably the LC medium comprises at least one compound selected from the group consisting of

[0589]

[0590] Where R 1 , R 2 , R 41 and R 42 Preferably, in compounds V-6, V-7 and IV, R 1 and R 41 each represents an alkyl or alkenyl group having 1 to 6 or 2 to 6 C atoms, and R 2 and R 42 represents an alkenyl group having 2 to 6 C atoms. Preferably, in compound V-14, R 1 represents an alkyl or alkenyl group having 1 to 6 or 2 to 6 C atoms and R 2 represents an alkyl group having 1 to 6 C atoms.

[0591] In another preferred embodiment, the LC media according to the invention comprise one or more compounds of the formula V-7, preferably selected from the compounds of the formulae V-7a to V-7e:

[0592]

[0593]

[0594] Therein alkyl represents an alkyl radical having 1 to 7 C atoms, alkenyl represents an alkenyl radical having 2 to 7 C atoms, and cycloalkyl represents a cycloalkyl radical having 3 to 12 C atoms, preferably cyclopropyl, cyclobutyl, cyclopentyl, cyclopropylalkyl, cyclobutylalkyl or cyclopentylalkyl.

[0595] It is highly preferred that the compounds of formulae V-7a to V-7e are selected from the group consisting of compounds of formulae V7-b1 to V7-b3, V-7d-1 to V-7d-8 and V-7e-1 to V-7e-12.

[0596]

[0597]

[0598]

[0599] wherein alkyl represents ethyl, n-propyl, n-butyl or n-pentyl, preferably n-propyl.

[0600] Also preferred are compounds of formula V, wherein R 51 and R 52 Independently of one another represent alkyl having 1 to 7 C atoms or alkenyl having 2 to 7 C atoms.

[0601] In a preferred embodiment of the present invention, the LC medium additionally comprises one or more compounds of the formulae VI-1 to VI-25

[0602]

[0603]

[0604]

[0605] in

[0606] R represents a straight chain alkyl or alkoxy group having 1 to 6 carbon atoms, (O) represents -O- or a single bond, X represents F, Cl, OCF3 or OCHF2, L x represents H or F, m is 0, 1, 2, 3, 4, 5 or 6 and n is 0, 1, 2, 3 or 4.

[0607] R preferably represents methyl, ethyl, propyl, butyl, pentyl, hexyl, methoxy, ethoxy, propoxy, butoxy, pentyloxy.

[0608] X preferably represents F or OCH3, very preferably F.

[0609] The LC media according to the invention preferably comprise the terphenyls of the formulae VI-1 to VI-25 in an amount of 2 to 30% by weight, in particular 5 to 20% by weight.

[0610] Particularly preferred are compounds of the formulae VI-1, VI-2, VI-4, VI-20, VI-21 and VI-22, in which X represents F. In these compounds, R preferably represents an alkyl group each having 1 to 5 C atoms, and furthermore represents an alkoxy group. In the compound of the formula VI-20, R preferably represents an alkyl group or an alkenyl group, in particular an alkyl group. In the compound of the formula VI-21, R preferably represents an alkyl group. In the compounds of the formulae VI-22 to VI-25, X preferably represents F.

[0611] Terphenyls of the formulae VI-1 to VI-25 are preferably employed in the LC media according to the invention if the Δn value of the mixture is ≥ 0.1. Preferably, the LC media comprises 2 to 20% by weight of one or more terphenyl compounds selected from the group of compounds of the formulae VI-1 to VI-25.

[0612] In another preferred embodiment of the present invention, the LC medium additionally comprises one or more compounds of the formulae VII-1 to VII-9

[0613]

[0614]

[0615] in

[0616] R 1 Each independently has the formula IIA for R 21 one of the specified meanings, and

[0617] w and x each independently represent 1 to 6.

[0618] Particularly preferred are LC media which comprise at least one compound of the formula VII-9.

[0619] LC medium comprising one or more substances containing tetrahydronaphthyl or naphthyl units, such as, for example, compounds of formulae N-1 to N-5,

[0620]

[0621]

[0622] Where R 61 and R 62 Each independently has a 21 The meanings specified preferably represent straight-chain alkyl, straight-chain alkoxy or straight-chain alkenyl, and

[0623] Z 61 and Z 62 Each independently represents -C2H4-, -CH=CH-, -(CH2)4-, -(CH2)3O-, -O(CH2)3-, -CH=CHCH2CH2-, -CH2CH2CH=CH-, -CH2O-, -OCH2-, -COO-, -OCO-, -C2F4-, -CF=CF-, -CF=CH-, -CH=CF-, -CF2O-, -OCF2-, -CH2- or a single bond.

[0624] c) an LC medium comprising one or more compounds selected from the group of difluorodibenzochroman compounds of formula BC, chromans of formula CR and fluorinated phenanthrenes of formulae PH-1 and PH-2,

[0625]

[0626] in

[0627] R 71 and R72 Each independently has R 21 and c is 0, 1 or 2. 71 and R 72 Preferably, independently of one another, they are alkyl or alkoxy radicals having 1 to 6 C atoms.

[0628] The LC media according to the invention preferably comprise the compound of the formula BC, CR, PH-1, PH-2 in an amount of 3 to 20% by weight, in particular in an amount of 3 to 15% by weight.

[0629] Particularly preferred compounds of formula BC and CR are compounds BC-1 to BC-7 and CR-1 to CR-5,

[0630]

[0631]

[0632] in

[0633] Alkyl and alkyl* each independently represent a straight-chain alkyl radical having 1 to 6 C atoms, and

[0634] Alkenyl and alkenyl* each independently of one another represent straight-chain alkenyl having 2 to 6 C atoms.

[0635] Very particular preference is given to LC media which comprise one, two or three compounds of the formula BC-2, BF-1 and / or BF-2.

[0636] d) an LC medium comprising one or more indane compounds of the formula In,

[0637]

[0638] in

[0639] R 81 , R 82 , R 83 each independently of one another represents a straight-chain alkyl, alkoxy, alkoxyalkyl or alkenyl radical having 1 to 6 C atoms,

[0640] R 82 and R 83 It may also represent a halogen, preferably F,

[0641] express

[0642]

[0643] i represents 0, 1 or 2.

[0644] Preferred compounds of formula In are compounds of formula In-1 to In-16 specified below:

[0645]

[0646]

[0647]

[0648] Particularly preferred are compounds of formulae In-1, In-2, In-3 and In-4.

[0649] The compounds of the formula In and the subformulae In-1 to In-16 are preferably employed in a concentration of ≥5% by weight, in particular from 5 to 30% by weight and very particularly preferably from 5 to 25% by weight, in the LC media according to the invention.

[0650] e) an LC medium comprising one or more compounds of the formulae L-1 to L-8,

[0651]

[0652]

[0653] in

[0654] R, R 1 and R 2 Each independently has the following formula IIA for R 21 The parameter s represents 1 or 2.

[0655] The compounds of the formulae L-1 to L-8 are preferably employed in a concentration of 5 to 15% by weight, in particular 5 to 12% by weight and very particularly preferably 8 to 10% by weight.

[0656] f) Preferably the LC medium additionally comprises one or more compounds of the formula IIA-Y

[0657]

[0658] Where R 11 and R 12 With respect to R in the above formula IIA 21 One of the meanings given, and L 1 and L 2 represents F or Cl identically or differently.

[0659] Preferred compounds of formula IIA-Y are selected from the group consisting of the following subformulae wherein:

[0660]

[0661]

[0662] Alkyl and Alkyl* each independently represent a straight-chain alkyl group having 1 to 6 C atoms, Alkoxy represents a straight-chain alkoxy group having 1 to 6 C atoms, Alkenyl and Alkenyl* each independently represent a straight-chain alkenyl group having 2 to 6 C atoms, and O represents an oxygen atom or a single bond. Alkenyl and Alkenyl* preferably represent CH2=CH-, CH2=CHCH2CH2-, CH3-CH=CH-, CH3-CH2-CH=CH-, CH3-(CH2)2-CH=CH-, CH3-(CH2)3-CH=CH- or CH3-CH=CH-(CH2)2-.

[0663] Particularly preferred compounds of formula IIA-Y are selected from the group consisting of the following subformulae:

[0664]

[0665] wherein Alkoxy and Alkoxy* have the meanings defined above and preferably denote methoxy, ethoxy, n-propoxy, n-butoxy or n-pentoxy.

[0666] g) LC medium comprising one or more tetraphenyl compounds selected from the group consisting of:

[0667]

[0668] in

[0669] R Q is alkyl, alkoxy, oxaalkyl or alkoxyalkyl having 1 to 9 C atoms, or alkenyl or alkenyloxy having 2 to 9 C atoms, all of which are optionally fluorinated,

[0670] X Q is F, Cl, a haloalkyl or alkoxy radical having 1 to 6 C atoms or a haloalkenyl or alkenyloxy radical having 2 to 6 C atoms,

[0671] L Q1 To L Q6 are independently H or F, where L Q1 To L Q6 At least one of them is F.

[0672] Preferred compounds of formula Q are those wherein R Q These represent straight-chain alkyl radicals having 2 to 6 C atoms, very preferably ethyl, n-propyl or n-butyl.

[0673] Preferred compounds of formula Q are those wherein L Q3and L Q4 Those where L is F. Also preferred are compounds of formula Q where L Q3 , L Q4 and L Q1 and L Q2 Those in which one or both are F.

[0674] Preferred compounds of formula Q are those wherein X Q Those representing F or OCF3, very preferably F.

[0675] The compound of formula Q is preferably selected from the following sub-formulas

[0676]

[0677] Where R Q has one of the meanings of the formula Q or one of the preferred meanings given above and below, and is preferably ethyl, n-propyl or n-butyl.

[0678] Particularly preferred are compounds of formula Q1, especially those wherein R Q Those which are n-propyl.

[0679] Preferably, the proportion of the compound of the formula Q in the LC medium is >0 to ≤5% by weight, very preferably 0.05 to 2% by weight, more preferably 0.1 to 1% by weight, most preferably 0.1 to 0.8% by weight.

[0680] Preferably, the LC medium contains 1 to 5, preferably 1 or 2, compounds of formula Q.

[0681] Adding a quatphenyl compound of formula Q to the LC mixture of a polymerizable LC medium enables reduction of ODF inhomogeneities while maintaining high UV absorption, enables rapid and complete polymerisation, enables strong and rapid generation of tilt angles, and increases the UV stability of the LC medium.

[0682] Furthermore, the addition of compounds of formula Q having positive dielectric anisotropy to LC media having negative dielectric anisotropy allows for better control of the dielectric constant ε || and ε ┴ values, and in particular enable a high dielectric constant ε || value while maintaining the dielectric anisotropy Δε constant, thereby reducing the kick-back voltage and reducing image retention.

[0683] The LC medium according to the present invention preferably comprises

[0684] - one or more compounds of formula IA or its subformulae, preferably compounds of formula IA1-1, in a proportion preferably of 1% to 30%, very preferably of 2% to 20%, most preferably of 2% to 15%;

[0685] and / or

[0686] - one or more compounds of formula IIA and / or IIB in a total concentration preferably in the range of 30% to 65%, more preferably 35% to 60%, particularly preferably 40% to 55%;

[0687] and / or

[0688] - one or more compounds of formula IV in a total concentration preferably ranging from 35% to 60%, more preferably from 40% to 55%, particularly preferably from 45% to 50%;

[0689] and / or

[0690] - one or more compounds of formula III, preferably compounds of formula III-2, very preferably compounds of formula III-2-1, in a total concentration preferably in the range of 2% to 25%, very preferably 4% to 15%.

[0691] In particular, the LC medium comprises

[0692] - one or more compounds CY-n-Om, in particular CY-3-O4, CY-5-O4 and / or CY-3-O2, preferably in a total concentration ranging from 5% to 30%, preferably from 10% to 20%, based on the mixture as a whole;

[0693] and / or

[0694] - one or more compounds PY-n-Om, in particular PY-1-O2, PY-2-O2 and / or PY-3-O2, in a total concentration preferably ranging from 5% to 40%, preferably from 10% to 30%, based on the mixture as a whole;

[0695] and / or

[0696] one or more compounds CPY-n-Om, in particular CPY-2-O2, CPY-3-O2 and / or CPY-5-O2, preferably in a concentration of >5%, in particular 7 to 20%, based on the mixture as a whole,

[0697] and / or

[0698] one or more compounds CCY-n-Om, preferably CCY-4-O2, CCY-3-O2, CCY-3-O3, CCY-3-O1 and / or CCY-5-O2, preferably in a concentration of >3%, in particular from 5 to 15%, based on the mixture as a whole;

[0699] and / or

[0700] one or more compounds CPY-n-Om and CY-n-Om, preferably in a concentration of 10 to 80%, based on the mixture as a whole,

[0701] and / or

[0702] one or more compounds CPY-n-Om and PY-n-Om, preferably CPY-2-O2 and / or CPY-3-O2 and PY-3-O2 or PY-1-O2, preferably in a concentration of 5 to 20%, more preferably 10 to 15%, based on the mixture as a whole,

[0703] and / or

[0704] one or more compounds selected from the group consisting of CCH-13, CCH-23, CCH-34, CCH-35, CCH-301 and CCH-303, preferably in a total concentration of 3% to 40%, preferably 3% to 25%, based on the mixture as a whole,

[0705] and / or

[0706] - one or more compounds selected from the group consisting of CC-2-V1, CC-3-V1, CC-3-V2, CC-4-V1, CC-3-V, CC-4-V and CC-5-V, preferably in a total concentration of 3% to 40%, more preferably 5% to 30%, based on the mixture as a whole,

[0707] and / or

[0708] one or more compounds CCP-nm and / or CCP-Vn-m and / or CPP-nm, preferably selected from the group consisting of CCP-3-1, CCP-V-1, CCP-V2-1 and CPP-3-2, preferably in a total concentration of 4% to 35%, preferably 5% to 25%, based on the mixture as a whole,

[0709] and / or

[0710] one or more compounds CLP-nm and / or CLP-Vn-m, preferably selected from the group consisting of CLP-3-1, CLP-3-2 and CLP-V-1, preferably in a total concentration of 1% to 25%, preferably 2% to 15%, based on the mixture as a whole,

[0711] and / or

[0712] - one or more compounds selected from the group consisting of PYP-nm, PGIY-n-Om and PGP-n-2V, preferably in a total concentration of 2% to 20%, more preferably 2% to 15%, most preferably 2% to 10%, based on the mixture as a whole,

[0713] and / or

[0714] one or more compounds PP-nm and / or PP-n-nVm, preferably selected from the group consisting of PP-1-3, PP-1-4, PP-1-5, PP-1-2V and PP-1-2V1, preferably in a total concentration of 1% to 15%, preferably 2% to 10%, based on the mixture as a whole,

[0715] and / or

[0716] - The compound PPGU-3-F, preferably in a concentration of 0.1% to 3%, based on the mixture as a whole.

[0717] The invention further relates to an electro-optical display with active-matrix addressing, characterized in that it contains an LC medium according to claim 1 as dielectric and in which the display is a VA, SA-VA, IPS, U-IPS, FFS, UB-FFS, SA-FFS, PS-VA, PS-OCB, PS-IPS, PS-FFS, PS-UB-FFS, PS-positive-VA, PS-TN, polymer-stabilized SA-VA or polymer-stabilized SA-FFS display.

[0718] It is advantageous for the LC media according to the invention to have a nematic phase preferably at ≤-20° C. to ≥70° C., particularly preferably at ≤-30° C. to ≥80° C. and very particularly preferably at ≤-40° C. to ≥90° C.

[0719] The media of the present invention have a clearing temperature of 70°C or higher, preferably 74°C or higher.

[0720] The expression "having a nematic phase" here means on the one hand that at low temperatures no smectic phase and no crystallization is observed at the corresponding temperature and on the other hand that the nematic phase does not become clear when heated. The low-temperature investigation is carried out in a flow viscometer at the corresponding temperature and is checked by storage for at least 100 hours in a test cell with a layer thickness corresponding to the electro-optical use. If the storage stability in a corresponding test cell at a temperature of -20°C is 1000 hours or more, the medium is said to be stable at this temperature. At temperatures of -30°C and -40°C, the response times are 500 hours and 250 hours, respectively. At high temperatures, the clearing point is measured in a capillary by conventional methods.

[0721] The liquid crystal mixture preferably has a nematic phase range of at least 60 K and a maximum of 30 mm at 20° C. 2 ·s -1 The flow viscosity ν 20 .

[0722] The mixture is nematic at a temperature of -20°C or below, preferably at -30°C or below, very preferably at -40°C or below.

[0723] The value of the birefringence Δn in the liquid-crystal mixture is generally from 0.07 to 0.16, preferably from 0.08 to 0.15 and very preferably from 0.09 to 0.14.

[0724] In a preferred embodiment of the invention, the birefringence of the medium is 0.090-0.110, preferably 0.095-0.105, in particular 0.100-0.105.

[0725] In another preferred embodiment, the medium of the present invention has a birefringence of 0.120 or more, preferably 0.125-0.145, more preferably 0.130-0.140.

[0726] The liquid crystal mixtures of the present invention have a dielectric anisotropy Δε of -1.5 to -8.0, preferably -2.0 to -4.0, in particular -2.5 to -3.5,

[0727] The rotational viscosity γ1 at 20° C. is preferably ≤120 mPa·s, in particular ≤100 mPa·s.

[0728] In a preferred embodiment, the rotational viscosity γ1 at 20° C. is ≤100 mPa·s, in particular ≤95 mPa·s.

[0729] The liquid-crystal media according to the invention have relatively low values ​​for the threshold voltage (V0). They are preferably in the range from 1.7 V to 3.0 V, particularly preferably ≤2.7 V and very particularly preferably ≤2.5 V.

[0730] For the present invention, unless explicitly stated otherwise, the term "threshold voltage" relates to the capacitive threshold (V0), also called Freedericks threshold.

[0731] Furthermore, the liquid-crystalline media according to the invention have high voltage holding ratio values ​​in liquid-crystal cells.

[0732] Typically, LC media having a low addressing voltage or threshold voltage show lower voltage holding ratios than those LC media having a higher addressing voltage or threshold voltage, and vice versa.

[0733] For the purposes of the present invention, the term "dielectrically positive compounds" refers to compounds with Δε>1.5, the term "dielectrically neutral compounds" refers to those with -1.5≤Δε≤1.5 and the term "dielectrically negative compounds" refers to those with Δε<-1.5. The dielectric anisotropy of the compounds is determined here by dissolving 10% of the compound in an LC host and determining the capacitance of the resulting mixture in at least one test cell, the test cell having in each case a layer thickness of 20 μm and having a homeotropic and a planar surface alignment at 1 kHz. The measuring voltage is generally between 0.5 V and 1.0 V, but is always below the capacitance threshold of the respective LC mixture investigated.

[0734] All temperature values ​​described in the present invention are in ° C.

[0735] The LC media according to the invention are suitable for all VA-TFT (vertically aligned thin film transistor) applications, such as VAN (vertically aligned nematic), MVA (multidomain VA), (S)-PVA (super patterned VA), ASV (advanced super view or axisymmetric VA), PSA (polymer stabilized VA) and PS-VA (polymer stabilized VA). In addition, they are suitable for IPS (in-plane switching) and FFS (fringe field switching) applications with negative Δε.

[0736] The nematic LC media in the displays according to the invention generally comprise two components A and B, which themselves consist of one or more individual compounds.

[0737] Component A has a pronounced negative dielectric anisotropy and provides a dielectric anisotropy of ≤-0.5 for the nematic phase. In addition to one or more compounds of the formula I, it preferably comprises compounds of the formulae IIA, IIB and / or IIC, and one or more compounds of the formula IV-1.

[0738] The proportion of component A is preferably 45-100%, in particular 60-85%.

[0739] For component A, preference is given to selecting one or more individual compounds with a Δε value of ≤−0.8. The smaller the proportion of A in the mixture as a whole, the more negative this value will necessarily be.

[0740] Component B has obvious nematogeneity and its flow viscosity at 20°C is not more than 30 mm 2 ·s -1 , preferably no more than 25mm 2 ·s -1 .

[0741] Many suitable materials are known to those skilled in the art from the literature.

[0742] Particularly preferred individual compounds in component B are extremely low viscosity nematic liquid crystals, whose flow viscosity at 20° C. is not greater than 18 mm 2 ·s -1 , preferably no more than 12mm 2 ·s -1 .

[0743] Component B is monotropically or enantiotropically nematic, has no smectic phase, and is capable of preventing the occurrence of a smectic phase in the LC medium at very low temperatures. For example, if various highly nematic materials are added to a smectic liquid crystal mixture, the nematicity of these materials can be contrasted by suppressing the extent to which the smectic phase is reached.

[0744] The mixture may also optionally comprise a component C comprising compounds having a dielectric anisotropy of Δε≥1.5. These so-called positive compounds are generally present in mixtures of negative dielectric anisotropy in an amount of ≤20% by weight, based on the mixture as a whole.

[0745] Besides one or more compounds of the formulae IA and IB, the medium preferably comprises 4 to 15, in particular 5 to 12 and particularly preferably <10 compounds of the formulae IIA, IIB and / or IIC and optionally one or more compounds of the formula IV-1.

[0746] Besides the compounds of the formulae IA and IB and the compounds of the formulae IIA, IIB and / or IIC and optionally IV-1, further constituents may also be present in an amount of up to 45%, but preferably up to 35%, in particular up to 10%, of the mixture as a whole.

[0747] The further components are preferably selected from nematic or nematogenic substances, in particular from the known substances of the class of azobenzene, benzylidene aniline, biphenyl, terphenyl, phenyl or cyclohexyl benzoate, phenyl or cyclohexyl cyclohexanecarboxylate, phenylcyclohexane, cyclohexylbiphenyl, cyclohexylcyclohexane, cyclohexylnaphthalene, 1,4-dicyclohexylbiphenyl or cyclohexylpyrimidine, phenyldioxane or cyclohexyldioxane, optionally halogenated stilbenes, benzylphenyl ethers, tolans and substituted cinnamic esters.

[0748] The most important compounds suitable as constituents of this type of liquid-crystalline phase can be characterized by the following formula OC

[0749] R 20 -LGER 21 OC

[0750] wherein L and E each designate a carbocyclic or heterocyclic ring system from the group formed by 1,4-disubstituted benzene and cyclohexane rings, 4,4'-disubstituted biphenyl, phenylcyclohexane and cyclohexylcyclohexane systems, 2,5-disubstituted pyrimidine and 1,3-dioxane rings, 2,6-disubstituted naphthalene, dihydronaphthalene and tetrahydronaphthalene, quinazoline and tetrahydroquinazoline,

[0751] G represents -CH=CH--N(O)=N-

[0752] -CH=CQ--CH=N(O)-

[0753] -C≡C--CH2-CH2-

[0754] -CO-O--CH2-O-

[0755] -CO-S--CH2-S-

[0756] -CH=N--COO-Phe-COO-

[0757] -CF2O--CF=CF-

[0758] -OCF2--OCH2-

[0759] -(CH2)4--(CH2)3O-

[0760] or a CC single bond, Q represents halogen, preferably chlorine or -CN, and R 20 and R 21 Each designates an alkyl, alkenyl, alkoxy, alkoxyalkyl or alkoxycarbonyloxy group having up to 18, preferably up to 8, carbon atoms, or one of these groups designates CN, NC, NO2, NCS, CF3, SF5, OCF3, F, Cl or Br.

[0761] In most of these compounds, R 20 and R 21 Different from each other, one of these groups is usually an alkyl or alkoxy group. Other variations of the proposed substituents are also common. Many such substances or mixtures thereof are also commercially available. All these substances can be prepared by methods known from the literature.

[0762] It goes without saying for the person skilled in the art that the VA, IPS or FFS mixtures according to the invention may also comprise compounds in which, for example, H, N, O, Cl and F are replaced by corresponding isotopes.

[0763] The combination of the compounds of the preferred embodiments mentioned above with the above-mentioned polymeric compounds leads to low threshold voltages, low rotational viscosities and very good low-temperature stability in the LC media according to the invention, while maintaining high bright spots and high HR values, and allows particularly low tilt angles (i.e. large tilts) to be established quickly in PSA displays. In particular, the LC media exhibit significantly shortened response times, in particular gray-to-gray response times, in PSA displays compared to LC media from the prior art.

[0764] The LC media according to the invention may also contain further additives known to the person skilled in the art and described in the literature, for example polymerization initiators, inhibitors, stabilizers, surface-active substances or chiral dopants. These may be polymerizable or non-polymerizable. Polymerizable additives are respectively assigned to the polymerizable component or component A). Non-polymerizable additives are respectively assigned to the non-polymerizable component or component B).

[0765] Furthermore, it is possible to add, for example, 0 to 15% by weight of pleochroic dyes to the LC medium, in addition to nanoparticles, conductive salts, preferably ethyldimethyldodecyl 4-hexyloxyammonium benzoate, tetrabutylammonium tetraphenylborate or complex salts of crown ethers (see, for example, Haller et al., Mol. Cryst. Liq. Cryst. 24 , 249-258 (1973)) for improving the electrical conductivity, or adding substances for modifying the dielectric anisotropy, viscosity and / or orientation of the nematic phase. Such substances are described, for example, in DE-A 22 09 127, 2240 864, 23 21 632, 23 38 281, 24 50 088, 26 37 430 and 28 53 728.

[0766] The individual components of the preferred embodiments of the LC media according to the invention listed above are known or the processes for preparing them are available from the prior art to the person skilled in the relevant art, since they are based on standard processes described in the literature. The corresponding compounds of the formula CY are described, for example, in EP-A-0 364 538. The corresponding compounds of the formula ZK are described, for example, in DE-A-26 36 684 and DE-A-3321 373.

[0767] The LC media which can be used according to the invention are prepared in a manner conventional per se, for example by mixing one or more of the above-mentioned compounds with one or more polymerizable compounds as defined above, and optionally with further liquid-crystalline compounds and / or additives. Usually, the desired amount of the component used in smaller amounts is dissolved in the components making up the main constituents, this being advantageously done at elevated temperature. It is also possible to mix the solutions of the components in an organic solvent, for example acetone, chloroform or methanol, and to remove the solvent again, for example by distillation after thorough mixing. The invention also relates to a process for the preparation of the LC media according to the invention.

[0768] It goes without saying to the person skilled in the art that the LC media according to the invention can also comprise compounds in which H, N, O, Cl, F are replaced by corresponding isotopes, for example deuterium.

[0769] The following examples illustrate the present invention but do not limit the present invention. However, they show preferred mixture concepts to those skilled in the art, as well as the compounds preferably used and their respective concentrations, and their combinations with each other. In addition, the examples illustrate which properties and combinations of properties are obtainable.

[0770] For the present invention and in the following examples, the structures of the liquid crystal compounds are indicated by means of acronyms. Unless otherwise specified, the conversion into chemical formulae is carried out according to the following Tables A.1 to A.3. All groups C n H 2n+1 , C m H 2m+1 and C l H 2l+1 or C n H 2n , C m H 2m and C l H 2l is a straight-chain alkyl or alkenyl group, in each case with n, m or 1 C atoms, respectively. Preferably, n, m and 1 are independently of one another 1, 2, 3, 4, 5, 6 or 7. Table A.1 shows the codes for the ring elements of the core of the compounds, Table A.2 lists the bridging units, and Table A.3 lists the meanings of the symbols for the left-hand and right-hand end groups of the molecules. The acronym consists of the code for the ring element with the optional linking group, followed by a first hyphen and the code for the left-hand end group, and a second hyphen and the code for the right-hand end group.

[0771] Table A.1: Ring elements

[0772]

[0773]

[0774]

[0775] Table A.2: Bridge unit

[0776]

[0777]

[0778] Table A.3: Terminal groups

[0779]

[0780]

[0781] Where n and m are each integers, and the three dots "..." are placeholders for other abbreviations from this table.

[0782] Table B shows illustrative compound structures along with their respective abbreviations.

[0783] Table B

[0784] In Table B, n, m, k and l are each independently an integer, preferably 1 to 9, preferably 1 to 7, k and l may also be 0 and preferably 0 to 4, more preferably 0 or 2 and most preferably 2, n is preferably 1, 2, 3, 4 or 5 or in the combination "-nO-", n is preferably 1, 2, 3 or 4, very preferably 2 or 4, m is preferably 1, 2, 3, 4 or 5 or in the combination "-Om", m is preferably 1, 2, 3 or 4, more preferably 2 or 4. The combination "-nVm" is preferably "2V1". (O)C m H 2m+1 Meaning C m H 2m+1 or OC m H 2m+1 .

[0785]

[0786]

[0787]

[0788]

[0789]

[0790]

[0791]

[0792]

[0793]

[0794]

[0795]

[0796]

[0797]

[0798]

[0799]

[0800]

[0801]

[0802]

[0803]

[0804]

[0805]

[0806] In a preferred embodiment of the present invention, the LC media according to the invention comprise one or more compounds selected from the group consisting of the compounds from Table B.

[0807] Table C

[0808] Table C shows possible chiral dopants which can be added to the LC media according to the invention.

[0809]

[0810]

[0811] The LC medium preferably comprises 0 to 10% by weight, in particular 0.01 to 5% by weight, particularly preferably 0.1 to 3% by weight of dopant. The LC medium preferably comprises one or more dopants selected from the group consisting of compounds from Table C.

[0812] Table D

[0813] Table D shows possible stabilizers which can be added to the LC media according to the invention. wherein n represents an integer from 1 to 12, preferably 1, 2, 3, 4, 5, 6, 7 or 8, and no terminal methyl groups are shown.

[0814]

[0815]

[0816]

[0817]

[0818]

[0819]

[0820]

[0821] The LC medium preferably comprises 0 to 10% by weight, in particular 1 ppm to 5% by weight, particularly preferably 1 ppm to 1% by weight of stabilizer. The LC medium preferably comprises one or more stabilizers selected from the group consisting of compounds from Table D.

[0822] Table E

[0823] Table E shows illustrative reactive mesogen-based compounds which can be used in the LC media according to the invention.

[0824]

[0825]

[0826]

[0827]

[0828]

[0829]

[0830]

[0831]

[0832]

[0833]

[0834]

[0835]

[0836]

[0837]

[0838]

[0839]

[0840]

[0841]

[0842]

[0843] In a preferred embodiment, the mixture according to the invention comprises one or more polymerizable compounds, preferably selected from the group consisting of polymerizable compounds of formulae RM-1 to RM-182. Among these, compounds RM-1, RM-4, RM-8, RM-17, RM-19, RM-35, RM-37, RM-39, RM-40, RM-41, RM-48, RM-52, RM-54, RM-57, RM-58, RM-64, RM-74, RM-76, RM-88, RM-91, RM-102, RM-103, RM-109, RM-116, RM-117, RM-120, RM-121, RM-122, RM-139, RM-140, RM-142, RM-143, RM-145, RM-146, RM-147, RM-149, RM-156 to RM-163, RM-169, RM-170 and RM-171 to RM-183 are particularly preferred.

[0844] Table F

[0845] Table F shows self-alignment additives for homeotropic alignment which can be used together with the polymerisable compounds in the LC media of SA-VA and SA-FFS displays according to the invention:

[0846]

[0847]

[0848]

[0849]

[0850]

[0851]

[0852]

[0853]

[0854]

[0855]

[0856]

[0857] In a preferred embodiment, the LC media, SA-VA and SA-FFS displays according to the invention comprise one or more SA additives selected from the formulae SA-1 to SA-48, preferably from the formulae SA-14 to SA-48, very preferably from the formulae SA-20 to SA-34 and SA-44, in combination with one or more RMs. Example

[0858] The following examples explain the present invention without limiting it. However, they show preferred mixture concepts and preferably used compounds and their corresponding concentrations and their combinations with each other to those skilled in the art. In addition, the examples illustrate obtainable properties and property combinations.

[0859] In addition, the following abbreviations and symbols are used:

[0860] V0 represents the threshold voltage at 20°C, capacitive [V],

[0861] n e represents the extraordinary refractive index at 20°C and 589nm,

[0862] n o represents the ordinary refractive index at 20°C and 589nm,

[0863] △n represents the optical anisotropy at 20°C and 589nm,

[0864] ε ⊥ represents the dielectric constant perpendicular to the director at 20°C and 1kHz,

[0865] ε || represents the dielectric constant parallel to the director at 20°C and 1kHz,

[0866] Δε represents the dielectric anisotropy at 20°C and 1kHz,

[0867] cl.p., T(N,I) represents the clearing point [℃],

[0868] γ1 represents the rotational viscosity at 20°C [mPa·s],

[0869] K1 is the elastic constant at 20°C, the “bending” deformation [pN],

[0870] K2 represents the elastic constant at 20°C, "torsion" deformation [pN],

[0871] K3 represents the elastic constant at 20°C, "bending" deformation [pN].

[0872] K av represents the average elastic constant [pN] at 20°C, defined as

[0873] K av. ≡( 3 / 2K1+K3) / 3≈(K1+K2+K3) / 3,

[0874] LTS stands for the low temperature stability of the phase measured in the test box,

[0875] VHR stands for voltage holding ratio.

[0876] Unless expressly stated otherwise, all concentrations in the present application are given as percentages by weight and relate to the respective entire mixture, which comprises all solid or liquid-crystalline components (without solvent).

[0877] Unless otherwise stated, all temperature values ​​indicated in this application, such as melting point T(C,N), transition from smectic phase (S) to nematic phase (N) T(S,N) and clearing point T(N,I) are expressed in degrees Celsius (°C). Mp stands for melting point, cl.p. = clearing point. In addition, C = liquid crystal phase, N = nematic phase, S = smectic phase and I = isotropic phase. The data between these symbols represent transition temperatures.

[0878] All physical properties are and have been determined according to "Merck Liquid Crystals, Physical Properties of Liquid Crystals" Status November 1997, Merck KGaA, Germany, and are valid for a temperature of 20°C, with Δn measured at 589 nm and Δε measured at 1 kHz, unless expressly stated otherwise in each case.

[0879] The term "threshold voltage" as used in the present invention relates to the capacitive threshold (V0), which is also referred to as the Freedericks threshold unless otherwise stated. In the embodiments, the optical threshold is also generally for a relative contrast ratio of 10% (V 10 ) given.

[0880] Unless otherwise stated, the process for polymerising the polymerisable compounds in a PSA display as described above and below is carried out at a temperature at which the LC medium exhibits a liquid crystal phase, preferably a nematic phase, and most preferably at room temperature.

[0881] Unless otherwise stated, the methods for preparing the test cells and measuring their electro-optical and other properties were performed by the methods described below or methods analogous thereto.

[0882] Displays used to measure capacitive threshold voltages typically consist of two plane-parallel glass outer plates separated by 25 μm, each with an electrode layer on the inside and an unrubbed polyimide alignment layer on top, which results in vertical edge alignment of the liquid crystal molecules.

[0883] A PSVA display or PSVA test box for measuring the tilt angle typically consists of two plane-parallel glass outer plates spaced about 4 μm apart, each of which has an electrode layer on the inside and a polyimide alignment layer on top, unless otherwise specified, wherein the two polyimide layers are rubbed antiparallel to each other and result in vertical edge alignment of the liquid crystal molecules. A SAVA display or test box has the same structure, but one or both polyimide layers are omitted. The polymerizable compound is typically polymerized in the display or test box by irradiating with UV light of a defined intensity for a predetermined time while applying a voltage (typically 10V-30V AC, 1kHz) to the display.

[0884] The intensity was measured using a standard instrument (Hoenle UV-meter high end with UV sensor).

[0885] The tilt angle is usually determined using the Mueller Matrix Polarimeter "AxoScan" from Axometrics. Small values ​​(ie large deviations from an angle of 90°) correspond to large tilts.

[0886] Unless otherwise stated, the term "tilt angle" means the angle between the LC director and the substrate, and "LC director" means the preferred orientation direction of the optical principal axes of the LC molecules in a LC molecule layer having uniform orientation, which in the case of rod-shaped, uniaxially positively birefringent LC molecules corresponds to their molecular long axes.

[0887] Example 1

[0888] The nematic LC host mixture N1 was prepared as follows

[0889]

[0890] The polymerizable mixture P1 according to the present invention is prepared by adding both polymerizable compounds IA1 and IB1 to the nematic LC host mixture N1.

[0891] For comparison purposes, polymerizable reference mixtures C1A and C1B were prepared by adding only one of the polymerizable compounds IA1 and IB1 to the nematic LC host mixture N1.

[0892]

[0893] Compound IA1 has a wavelength λ of 300 nm at an extinction coefficient E=0.5 (measured in DCM at a concentration of 0.3 g / L).

[0894] Compound IB1 has a wavelength λ of 320 nm at an extinction coefficient E=0.5 (measured in DCM at a concentration of 0.3 g / L).

[0895] Therefore, the compound is suitable for PSA processes using UV C-type lamps in both UV1 and UV2 steps.

[0896] The polymerizable mixture compositions are shown in Table 1.1.

[0897] Table 1.1 – Composition of polymerizable mixtures

[0898]

[0899] Tilt Angle Generation

[0900] The electro-optical VA test box with the AF glass substrate containing the polymerizable mixture was exposed to UV light in a two-step process (a first step (UV1) for generating the tilt angle and a second step (UV2) for polymerizing any residual monomers that were not polymerized in the first step). In the UV1 step, voltage was applied (0.1 V step and cured at DC 15 V). In the UV2 step, no voltage was applied. As a radiation source, a C-type fluorescent UV lamp with a cutoff filter of 313 nm was used. The UV intensity was checked by a UV detector using 313 nm. Unless otherwise specified, the other conditions were as follows:

[0901] UV1 (C-type lamp): 5mW / cm 2 10 to 300 seconds at room temperature

[0902] UV2 (C-type lamp): 0.5mW / cm 2 120 min at RT

[0903] The tilt angle generated in the test box after varying the irradiation time after the above UV1 step was measured using an Otsuka T_RETS-10 system.

[0904] The time required to achieve a tilt angle of 88° is shown in Table 1.2 below.

[0905] Table 1.2 – Tilt angles

[0906] mixture C1B P1 Tilt angle (°) 88 Time(s) 147 to 153 113 to 118

[0907] It can be seen that the polymerizable mixture P1 according to the invention comprising both compound IA1 and compound IB1 shows a significantly faster tilt angle development than the reference mixture C1B which indeed contains only compound IB1.

[0908] Tilt stability

[0909] The tilt stability, ie the change in the tilt angle after repeated electrical stress, is a criterion for evaluating the risk of image sticking. Low values ​​of the change in the tilt angle indicate good tilt stability and a low potential risk of image sticking.

[0910] For the determination of tilt stability, a test cell containing the mixture was prepared and the monomers were polymerized using two UV steps as described above to produce the tilt angle. The test cell was then placed on the backlight unit at 40 V. PP Electrical stress was applied at 60 Hz with a square wave of 100 μm for 168 h. After a relaxation time of 5 to 10 min, the tilt angle was measured using an Otsuka T_RETS-10 system.

[0911] The change in the tilt angle Δtilt is determined according to equation (1)

[0912] tilt 于应力后 -tilt 于倾斜产生后 =Δ tilt (1)

[0913] The lower the value of Δtilt, the higher the tilt stability.

[0914] The results are shown in Table 1.3.

[0915] Table 1.3 – Tilt stability

[0916] mixture C1A C1B P1 Δ Tilt (°) 0.66 0.53 0.42

[0917] It can be seen that the polymerizable mixture P1 according to the invention comprising both compound IA1 and compound IB1 shows a better tilt stability than the reference mixtures C1A and C1B which do contain only one of the compounds.

[0918] Voltage Holding Ratio (VHR)

[0919] For VHR measurement, polymerizable LC medium was filled into a test cell with fishbone pattern ITO electrodes and the monomer was polymerized under the same conditions as described above for tilt angle generation. VHR was measured at 60°C while applying a voltage of 1 V / 0.6 Hz before and after UV C-type light exposure (as used for tilt angle generation).

[0920] Light stress generally causes a reduction in the VHR of the LC mixture, therefore, the smaller the absolute reduction in the VHR value after stress, the better the performance for display applications.

[0921] The results are shown in Table 1.5.

[0922] Table 1.5-VHR

[0923] mixture C1A C1B P1 P12 VHR (%) Initial 97.1 98.3 95.8 95.2 VHR (%) after 2 hours UV 66.7 50.9 82.8 87.6

[0924] It can be seen that the polymerizable mixtures P1 and P12 according to the invention comprising both compound IA1 and compound IB1 show slightly lower initial VHR values ​​than some of the reference mixtures C1A and C1B which do contain only one of the monomers. However, after UV stress, the mixtures P1 and P12 according to the invention show a significantly less drop in VHR, while in the reference mixtures C1A and C1B the VHR values ​​drop sharply.

[0925] Residual RM

[0926] The residual content of unpolymerized monomers in the mixture is determined after UV photopolymerization (in ppm). The lower the residual monomer content after a given time interval, the faster the polymerization. For this purpose, the polymerizable mixture is filled in a test cell and is measured by using a UV light source with a power of 5 mW / cm 2 The UV exposure of a C-type fluorescent UV lamp with a constant intensity was continued for varying time intervals for polymerization. The UV intensity was checked by a UV detector using 313 nm. After the photopolymerization was continued for a certain time interval, the test box was opened, and the mixture was dissolved and rinsed out of the test box with methyl ethyl ketone and analyzed by ultra-performance liquid chromatography (UPLC).

[0927] The results are shown in Table 1.4.

[0928] Table 1.4 – Residual RM

[0929]

[0930] nd = Not Detectable

[0931] It can be seen that in the polymerizable mixture P1 according to the invention comprising both compound IA1 and compound IB1, the residual content of monomers after polymerization decreases faster than in the polymerizable reference mixtures C1A and C1B which do contain only one of the compounds.

[0932] In summary, the above results demonstrate that the polymerizable mixture according to the present invention comprising both polymerizable compounds of Formula IA and Formula IB shows significant improvements such as faster tilt angle generation, better tilt stability, higher VHR after UV stress and lower amounts of residual monomers.

[0933] The results indeed also demonstrate that LC media comprising a combination of two polymerisable compounds are suitable for use in a PSA process using UV C-type lamps for both UV1 and UV2 steps.

[0934] Example 2

[0935] The polymerizable mixtures P21, P22 and P23 according to the present invention were prepared by adding polymerizable compounds IA1 and IB110 in varying concentrations to the nematic LC host mixture N1.

[0936] For comparison purposes, a polymerizable reference mixture C2 was prepared by adding only polymerizable compound IB110 to the nematic LC host mixture N1.

[0937]

[0938] Compound IA1 has a wavelength λ of 334 nm at an extinction coefficient E=0.5 (measured in DCM at a concentration of 0.3 g / L).

[0939] The polymerizable mixture compositions are shown in Table 2.1.

[0940] Table 2.1 – Composition of polymerizable mixtures

[0941]

[0942] *From Example 1

[0943] Tilt stability

[0944] Tilt stability was measured as described in Example 1. The results are shown in Table 2.2.

[0945] Table 2.2 – Tilt stability

[0946] mixture C1A* C2 P23 Δ Tilt (°) 0.66 1.42 0.50

[0947] *From Example 1

[0948] It can be seen that the polymerizable mixture P23 according to the invention comprising both compound IA1 and compound IB110 shows a better tilt stability than the reference mixtures C1A and C2 which do contain only one of these compounds.

[0949] Voltage Holding Ratio (VHR)

[0950] The VHR initially and after UV stress was measured as described in Example 1, except that a UV B-type lamp was used for UV stress due to the higher absorption wavelength of Compound B110.

[0951] The results are shown in Table 2.3.

[0952] For comparison purposes, Table 2.3 also contains data for mixture C1A with 0.5% monomer IA1 in LC host mixture N1 from Example 1, which was obtained using a UV C type lamp, since compound IA1 is less compatible with the longer emission wavelengths of UV B type lamps than with the shorter emission wavelengths of UV C type lamps due to its shorter absorption wavelength.

[0953] Table 2.3 - VHR

[0954] mixture C2 P21 P22 P23 C1A* VHR (%) Initial 97.5 97.8 95.5 96.7 97.1 VHR (%) after 2 hours UV 73.5 80.1 86.9 89.3 66.7

[0955] *From Example 1

[0956] It can be seen that the polymerizable mixtures P21, P22 and P23 according to the invention comprising both compound IA1 and compound IB110 show similar initial VHR values ​​to the reference mixtures C1A and C2 which do contain only one of the compounds. After UV stress, the mixtures P21, P22 and P23 according to the invention show a significantly less drop in VHR than the reference mixtures C1A and C2.

[0957] Residual RM

[0958] The residual content of unpolymerized monomers in the mixture (in ppm) was determined as described in Example 1, except that a UV B-type lamp was used for the UV irradiation stress due to the higher absorption wavelength of compound B110.

[0959] The results are shown in Table 2.4.

[0960] For comparison purposes, also included are data for mixture C1A with 0.5% monomer IA1 in LC host mixture N1 from Example 1, obtained using UV C type lamps, since compound IA1 is less compatible with the longer emission wavelengths of UV B type lamps than with the shorter emission wavelengths of UV C type lamps due to its shorter absorption wavelength.

[0961] Table 2.4 – Residual RM

[0962]

[0963] *From Example 1

[0964] nd = Not Detectable

[0965] It can be seen that in the polymerizable mixtures P22 and P23 according to the invention comprising both compound IA1 and compound IB110, the residual content of monomers after polymerization decreases just as fast or even faster than in the respective polymerizable reference mixtures C1A and C2 which do contain only one of these compounds.

[0966] It can also be seen that compound IA1 does show even lower residual RM amounts after UV polymerization with a B-type lamp when used in combination with compound IB1, as compared to when used alone in LC host mixture N1 after UV polymerization with a C-type lamp. This is particularly surprising, since compound IA1 is expected to be less compatible with B-type lamps than with C-type lamps due to its shorter absorption wavelength. Therefore, it can be inferred that the use of compound IA1 in combination with compound IB1 provides a synergistic effect that makes the combination compatible with B-type lamps as well.

[0967] In summary, the above results demonstrate that the polymerizable mixture according to the present invention comprising both polymerizable compounds of Formula IA and Formula IB shows significant improvements, such as faster tilt angle generation, better tilt stability, higher VHR after UV stress, and lower amounts of residual monomers, compared to the polymerizable mixture containing only one of the polymerizable compounds.

[0968] The results indeed also demonstrate that LC media comprising a combination of two polymerisable compounds are suitable for a PSA process using UV C type lamps for the UV1 step and UVB type lamps for the UV2 step.

[0969] Example 3

[0970] The polymerizable mixture P3 according to the present invention is prepared by adding polymerizable compounds IA1 and IB33 to the nematic LC host mixture N1.

[0971] For comparison purposes, a polymerizable reference mixture C3 was prepared by adding only compound IB33 to the nematic LC host mixture N1.

[0972]

[0973] Compound IB33 has a wavelength λ of 320 nm at an extinction coefficient E=0.5 (measured in DCM at a concentration of 0.3 g / L).

[0974] The polymerizable mixture compositions are shown in Table 3.1.

[0975] Table 3.1 – Composition of polymerizable mixtures

[0976]

[0977] *From Example 1

[0978] Tilt stability

[0979] Tilt stability was measured as described in Example 1. The results are shown in Table 3.2.

[0980] Table 3.2 – Tilt stability

[0981] mixture C3 C1A* P3 Δ Tilt (°) 0.67 0.66 0.49

[0982] *From Example 1

[0983] It can be seen that the polymerizable mixture P3 according to the invention comprising both compound IA1 and compound IB33 shows a better tilt stability than the reference mixtures C1A and C3 which do contain only one of these compounds.

[0984] Voltage Holding Ratio (VHR)

[0985] The VHR initially and after UV stress was measured as described in Example 1.

[0986] The results are shown in Table 3.3.

[0987] Table 3.3 – VHR

[0988] mixture C3 C1A* P3 VHR (%) Initial 96.3 97.1 95.2 VHR (%) after 2 hours UV 79.9 66.7 87.6

[0989] *From Example 1

[0990] It can be seen that the polymerizable mixture P3 according to the invention comprising both compound IA1 and compound IB33 shows similar initial VHR values ​​to the reference mixtures C1A and C3 which do contain only one of the compounds. After UV stress, the mixture P3 according to the invention shows a significantly less drop in VHR than the reference mixtures C1A and C3.

[0991] Residual RM

[0992] The residual content of unpolymerized monomers in the mixture (in ppm) was determined as described in Example 1.

[0993] The results are shown in Table 3.4.

[0994] Table 3.4 – Residual RM

[0995]

[0996] *From Example 1

[0997] nd = Not Detectable

[0998] It can be seen that in the polymerizable mixture P3 according to the invention comprising both compound IA1 and compound IB3, the residual content of monomers after polymerization decreases just as quickly or even faster than in the respective polymerizable reference mixtures C1A and C3 which do contain only one of the compounds.

[0999] In summary, the above results demonstrate that the polymerizable mixture according to the present invention comprising both polymerizable compounds of Formula IA and Formula IB shows significant improvements, such as faster tilt angle generation, better tilt stability, higher VHR after UV stress, and lower amounts of residual monomers, compared to the polymerizable mixture containing only one of the polymerizable compounds.

[1000] The results indeed also demonstrate that LC media comprising a combination of two polymerisable compounds are suitable for use in a PSA process using UV C-type lamps for both UV1 and UV2 steps.

[1001] Example 4

[1002] A polymerizable mixture P4 was prepared by adding 0.5% of compound IA1 and 0.5% of compound IB3 to the nematic LC host mixture N1.

[1003]

[1004] Example 5

[1005] Polymerizable mixture P5 was prepared by adding 0.25% of compound IA1 and 0.5% of compound IB3 to the nematic LC host mixture N1.

[1006] Example 6

[1007] The nematic LC host mixture N2 was prepared as follows

[1008]

[1009] The polymerizable mixture P6 was prepared by adding 0.5% of polymerizable compound IA1 and 0.3% of polymerizable compound IB1 to the nematic LC host mixture N2.

[1010] Example 7

[1011] The nematic LC host mixture N3 was prepared as follows

[1012]

[1013]

[1014] Polymerizable mixture P7 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB1 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N3.

[1015]

[1016] Example 8

[1017] The nematic LC host mixture N4 was prepared as follows

[1018]

[1019] Polymerizable mixture P8 was prepared by adding 0.4% of compound IA1 and 0.2% of compound IB1 to the nematic LC host mixture N4.

[1020] Example 9

[1021] Polymerizable mixture P9 was prepared by adding 0.5% of compound IA1, 0.25% of compound IB1 and 150 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N4.

[1022] Example 10

[1023] The nematic LC host mixture N5 was prepared as follows

[1024]

[1025] Polymerizable mixture P10 was prepared by adding 0.5% of compound IA1 and 0.3% of compound IB110 to the nematic LC host mixture N5.

[1026] Embodiment 11

[1027] A polymerizable mixture P11 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB110 and 50 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1028] Example 12

[1029] The nematic LC host mixture N6 was prepared as follows

[1030]

[1031]

[1032] Polymerizable mixture P12 was prepared by adding 0.5% of compound IA1 and 0.3% of compound IB1 to the nematic LC host mixture N6.

[1033] Embodiment 13

[1034] Polymerizable mixture P13 was prepared by adding 0.4% of compound IA1 and 0.2% of compound IB2 to the nematic LC host mixture N2.

[1035]

[1036] Embodiment 14

[1037] Polymerizable mixture P14 was prepared by adding 0.3% of compound IA1, 0.2% of compound IB2 and 150 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1038] Embodiment 15

[1039] Polymerizable mixture P15 was prepared by adding 0.4% of compound IA1, 0.2% of compound IB2 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N3.

[1040] Example 16

[1041] Polymerizable mixture P16 was prepared by adding 0.5% of compound IA1 and 0.4% of compound IB3 to the nematic LC host mixture N2.

[1042] Embodiment 17

[1043] Polymerizable mixture P17 was prepared by adding 0.4% of compound IA1, 0.3% of compound IB3 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N3.

[1044] Embodiment 18

[1045] Polymerizable mixture P18 was prepared by adding 0.4% of compound IA1, 0.2% of compound IB133 and 150 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N1.

[1046]

[1047] Embodiment 19

[1048] Polymerizable mixture P19 was prepared by adding 0.4% of compound IA1, 0.5% of compound IB133 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1049] Embodiment 20

[1050] Polymerizable mixture P20 was prepared by adding 0.5% of compound IA1, 0.5% of compound IB133 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N3.

[1051] Embodiment 21

[1052] Polymerizable mixture P21 was prepared by adding 0.4% of compound IA1, 0.2% of compound IB135 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N1.

[1053]

[1054] Embodiment 22

[1055] Polymerizable mixture P22 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB135 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1056] Embodiment 23

[1057] Polymerizable mixture P23 was prepared by adding 0.4% of compound IA1, 0.2% of compound IB135 and 150 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N3.

[1058] Embodiment 24

[1059] Polymerizable mixture P24 was prepared by adding 0.5% compound IA1, 0.4% compound IB55 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N1.

[1060]

[1061] Embodiment 25

[1062] Polymerizable mixture P25 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB55 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1063] Embodiment 26

[1064] Polymerizable mixture P26 was prepared by adding 0.4% compound IA1, 0.4% compound IB55 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N3.

[1065] Embodiment 27

[1066] Polymerizable mixture P27 was prepared by adding 0.5% compound IA1, 0.4% compound IB70 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N1.

[1067]

[1068] Embodiment 28

[1069] Polymerizable mixture P28 was prepared by adding 0.3% compound IA1, 0.4% compound IB69 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1070] Embodiment 29

[1071] Polymerizable mixture P29 was prepared by adding 0.4% compound IA1, 0.4% compound IB69 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N3.

[1072] Embodiment 30

[1073] The nematic LC host mixture N7 was prepared as follows

[1074]

[1075] Polymerizable mixture P30 was prepared by adding 0.4% of compound IA1, 0.2% of compound IB1 and 50 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N7.

[1076] Embodiment 31

[1077] The nematic LC host mixture N8 was prepared as follows

[1078]

[1079]

[1080] Polymerizable mixture P31 was prepared by adding 0.4% of compound IA1, 0.2% of compound IB1 and 50 ppm of stabilizer ST-3b-1 to the nematic LC host mixture N8.

[1081]

[1082] Embodiment 32

[1083] The nematic LC host mixture N9 was prepared as follows

[1084]

[1085] Polymerizable mixture P32 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB1 and 150 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N9.

[1086] Embodiment 33

[1087] The nematic LC host mixture N10 was prepared as follows

[1088]

[1089] A polymerizable mixture P33 was prepared by adding 0.5% of compound IA1, 0.4% of compound IB1 and 0.6% of SA additive SA23 to the nematic LC host mixture N10.

[1090]

[1091] Embodiment 34

[1092] The nematic LC host mixture N11 was prepared as follows

[1093]

[1094]

[1095] Polymerizable mixture P34 was prepared by adding 0.4% of compound IA1, 0.3% of compound IB1 and 100 ppm of stabilizer ST-3a-1 to nematic LC host mixture N11.

[1096] Embodiment 35

[1097] The nematic LC host mixture N12 was prepared as follows

[1098]

[1099] Polymerizable mixture P35 was prepared by adding 0.4% of compound IA1, 0.2% of compound IB1 and 150 ppm of stabilizer ST-3b-1 to the nematic LC host mixture N12.

[1100] Embodiment 36

[1101] The nematic LC host mixture N13 was prepared as follows

[1102]

[1103] Polymerizable mixture P36 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB1 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N13.

[1104] Embodiment 37

[1105] The nematic LC host mixture N14 was prepared as follows

[1106]

[1107]

[1108] Polymerizable mixture P37 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB1 and 50 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N14.

[1109] Embodiment 38

[1110] The nematic LC host mixture N15 was prepared as follows

[1111]

[1112] Polymerizable mixture P38 was prepared by adding 0.4% of compound IA1, 0.3% of compound IB1 and 50 ppm of stabilizer ST-3b-1 to the nematic LC host mixture N15.

[1113] Embodiment 39

[1114] The nematic LC host mixture N16 was prepared as follows

[1115]

[1116]

[1117] Polymerizable mixture P39 was prepared by adding 0.5% compound IA1, 0.4% compound IB1 and 150 ppm stabilizer ST-8-1 to the nematic LC host mixture N16.

[1118]

[1119] Embodiment 40

[1120] The nematic LC host mixture N17 was prepared as follows

[1121]

[1122]

[1123] Polymerizable mixture P40 was prepared by adding 0.5% compound IA1, 0.3% compound IB1 and 150 ppm stabilizer ST-3a-1 to the nematic LC host mixture N17.

[1124] Embodiment 41

[1125] Nematic LC host mixture N18 was prepared as follows

[1126]

[1127] Polymerizable mixture P41 was prepared by adding 0.5% of compound IA1, 0.5% of compound IB3 and 100 ppm of stabilizer ST-12 to nematic LC host mixture N18.

[1128]

[1129] Embodiment 42

[1130] The nematic LC host mixture N19 was prepared as follows

[1131]

[1132] Polymerizable mixture P42 was prepared by adding 0.5% compound IA1, 0.4% compound IB3 and 100 ppm stabilizer ST-3a-1 to nematic LC host mixture N19.

[1133] Embodiment 43

[1134] The nematic LC host mixture N20 was prepared as follows

[1135]

[1136]

[1137] Polymerizable mixture P43 was prepared by adding 0.4% of compound IA1, 0.3% of compound IB1 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N20.

[1138] Embodiment 44

[1139] The nematic LC host mixture N21 was prepared as follows

[1140]

[1141]

[1142] Polymerizable mixture P44 was prepared by adding 0.5% compound IA1, 0.3% compound IB1 and 150 ppm stabilizer ST-9-1 to the nematic LC host mixture N21.

[1143]

[1144] Embodiment 45

[1145] The nematic LC host mixture N22 was prepared as follows

[1146]

[1147] Polymerizable mixture P45 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB1 and 50 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N22.

[1148] Embodiment 46

[1149] The nematic LC host mixture N23 was prepared as follows

[1150]

[1151] Polymerizable mixture P46 was prepared by adding 0.5% compound IA1, 0.3% compound IB1 and 0.6% SA additive SA32 to the nematic LC host mixture N23.

[1152]

[1153] Embodiment 47

[1154] The nematic LC host mixture N24 was prepared as follows

[1155]

[1156] Polymerizable mixture P47 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB3 and 150 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N24.

[1157] Embodiment 48

[1158] The nematic LC host mixture N25 was prepared as follows

[1159]

[1160]

[1161] Polymerizable mixture P48 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB1 and 100 ppm of stabilizer ST-3b-1 to the nematic LC host mixture N25.

[1162] Embodiment 49

[1163] The nematic LC host mixture N26 was prepared as follows

[1164]

[1165]

[1166] Polymerizable mixture P49 was prepared by adding 0.4% of compound IA1, 0.2% of compound IB2 and 150 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N26.

[1167] Embodiment 50

[1168] The nematic LC host mixture N27 was prepared as follows

[1169]

[1170] Polymerizable mixture P50 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB1 and 50 ppm of stabilizer ST-8-1 to the nematic LC host mixture N27.

[1171] Embodiment 51

[1172] The nematic LC host mixture N28 was prepared as follows

[1173]

[1174]

[1175] Polymerizable mixture P51 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB2 and 50 ppm of stabilizer ST-9-1 to the nematic LC host mixture N28.

[1176] Embodiment 52

[1177] The nematic LC host mixture N29 was prepared as follows

[1178]

[1179] Polymerizable mixture P52 was prepared by adding 0.5% of compound IA1, 0.4% of compound IB3 and 150 ppm of stabilizer ST-3b-1 to the nematic LC host mixture N29.

[1180] Embodiment 53

[1181] The nematic LC host mixture N30 was prepared as follows

[1182]

[1183] Polymerizable mixture P53 was prepared by adding 0.4% of compound IA1, 0.2% of compound IB1 and 150 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N30.

[1184] Embodiment 54

[1185] The nematic LC host mixture N31 was prepared as follows

[1186]

[1187]

[1188] Polymerizable mixture P54 was prepared by adding 0.3% of compound IA1, 0.4% of compound IB133 and 150 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N31.

[1189] Embodiment 55

[1190] The nematic LC host mixture N32 was prepared as follows

[1191]

[1192] Polymerizable mixture P55 was prepared by adding 0.3% compound IA1, 0.4% compound IB110 and 0.6% SA additive SA23 to the nematic LC host mixture N32.

[1193] Embodiment 56

[1194] The nematic LC host mixture N33 was prepared as follows

[1195]

[1196] Polymerizable mixture P56 was prepared by adding 0.5% compound IA1, 0.4% compound IB33, 0.6% SA additive SA23 and 50 ppm stabilizer ST-9-1 to the nematic LC host mixture N33.

[1197] Embodiment 57

[1198] The nematic LC host mixture N34 was prepared as follows

[1199]

[1200]

[1201] Polymerizable mixture P57 was prepared by adding 0.4% compound IA1, 0.3% compound IB1, 0.6% SA additive SA32 and 50 ppm stabilizer ST-8-1 to the nematic LC host mixture N34.

[1202] Embodiment 58

[1203] The nematic LC host mixture N35 was prepared as follows

[1204]

[1205] Polymerizable mixture P58 was prepared by adding 0.5% compound IA1, 0.4% compound IB33 and 150 ppm stabilizer ST-12 to the nematic LC host mixture N35.

[1206] Embodiment 59

[1207] The nematic LC host mixture N36 was prepared as follows

[1208]

[1209] Polymerizable mixture P59 was prepared by adding 0.4% of compound IA1, 0.2% of compound IB2 and 150 ppm of stabilizer ST-9-1 to the nematic LC host mixture N36.

[1210] Embodiment 60

[1211] The nematic LC host mixture N37 was prepared as follows

[1212]

[1213] Polymerizable mixture P60 was prepared by adding 0.5% compound IA1, 0.3% compound IB1, 0.6% SA additive SA23 and 50 ppm stabilizer ST-3a-1 to the nematic LC host mixture N37.

[1214] Embodiment 61

[1215] The nematic LC host mixture N38 was prepared as follows

[1216]

[1217] Polymerizable mixture P61 was prepared by adding 0.4% of compound IA1, 0.3% of compound IB1 and 150 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N38.

[1218] Embodiment 62

[1219] The nematic LC host mixture N39 was prepared as follows

[1220]

[1221]

[1222] Polymerizable mixture P62 was prepared by adding 0.5% compound IA1, 0.4% compound IB3 and 150 ppm stabilizer ST-9-1 to the nematic LC host mixture N39.

[1223] Embodiment 63

[1224] The nematic LC host mixture N40 was prepared as follows

[1225]

[1226] Polymerizable mixture P63 was prepared by adding 0.4% of compound IA1, 0.3% of compound IB1 and 150 ppm of stabilizer ST-12 to the nematic LC host mixture N40.

[1227] Embodiment 64

[1228] The nematic LC host mixture N41 was prepared as follows

[1229]

[1230]

[1231] Polymerizable mixture P64 was prepared by adding 0.4% of compound IA1, 0.3% of compound IB1 and 150 ppm of stabilizer ST-9-1 to the nematic LC host mixture N41.

[1232] Embodiment 65

[1233] The nematic LC host mixture N42 was prepared as follows

[1234]

[1235] Polymerizable mixture P65 was prepared by adding 0.5% compound IA1, 0.5% compound IB3 and 150 ppm stabilizer ST-3a-1 to the nematic LC host mixture N42.

[1236] Embodiment 66

[1237] The nematic LC host mixture N43 was prepared as follows

[1238]

[1239]

[1240] Polymerizable mixture P66 was prepared by adding 0.4% compound IA1, 0.3% compound IB1 and 150 ppm stabilizer ST-3b-1 to the nematic LC host mixture N43.

[1241] Embodiment 67

[1242] The nematic LC host mixture N44 was prepared as follows

[1243]

[1244] Polymerizable mixture P67 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB1 and 150 ppm of stabilizer ST-12 to the nematic LC host mixture N44.

[1245] Embodiment 68

[1246] The nematic LC host mixture N45 was prepared as follows

[1247]

[1248]

[1249] Polymerizable mixture P68 was prepared by adding 0.5% compound IA1, 0.3% compound IB1 and 150 ppm stabilizer ST-9-1 to the nematic LC host mixture N45.

[1250] Embodiment 69

[1251] The nematic LC host mixture N46 was prepared as follows

[1252]

[1253] Polymerizable mixture P69 was prepared by adding 0.5% compound IA1, 0.3% compound IB1, 0.6% SA additive SA32 and 150 ppm stabilizer ST-8-1 to the nematic LC host mixture N46.

[1254] Embodiment 70

[1255] The nematic LC host mixture N47 was prepared as follows

[1256]

[1257] Polymerizable mixture P70 was prepared by adding 0.5% compound IA1, 0.3% compound IB1, 0.6% SA additive SA32 and 100 ppm stabilizer ST-3b-1 to the nematic LC host mixture N47.

[1258] Embodiment 71

[1259] The nematic LC host mixture N48 was prepared as follows

[1260]

[1261]

[1262] Polymerizable mixture P71 was prepared by adding 0.4% compound IA1, 0.2% compound IB1, 0.6% SA additive SA32 and 150 ppm stabilizer ST-9-1 to the nematic LC host mixture N48.

[1263] Embodiment 72

[1264] The nematic LC host mixture N49 was prepared as follows

[1265]

[1266] Polymerizable mixture P72 was prepared by adding 0.5% of compound IA1 and 0.3% of compound IB1 to the nematic LC host mixture N49.

[1267] Embodiment 73

[1268] The nematic LC host mixture N50 was prepared as follows

[1269]

[1270] Polymerizable mixture P73 was prepared by adding 0.5% compound IA1, 0.3% compound IB89 and 150 ppm stabilizer ST-3a-1 to the nematic LC host mixture N50.

[1271]

[1272] Embodiment 74

[1273] The nematic LC host mixture N51 was prepared as follows

[1274]

[1275]

[1276] Polymerizable mixture P74 was prepared by adding 0.5% of compound IA1, 0.3% of compound IB3 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N51.

[1277] Embodiment 75

[1278] The nematic LC host mixture N52 was prepared as follows

[1279]

[1280] Polymerizable mixture P75 was prepared by adding 0.4% of compound IA1, 0.2% of compound IB1 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N52.

[1281] Embodiment 76

[1282] Polymerizable mixture P76 was prepared by adding 0.5% compound IA1, 0.4% compound IB6 and 150 ppm stabilizer ST-3a-1 to the nematic LC host mixture N3.

[1283]

[1284] Embodiment 77

[1285] Polymerizable mixture P77 was prepared by adding 0.4% compound IA1, 0.4% compound IB6 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1286] Embodiment 78

[1287] Polymerizable mixture P76 was prepared by adding 0.5% compound IA1, 0.4% compound IB25 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N3.

[1288]

[1289] Embodiment 79

[1290] Polymerizable mixture P79 was prepared by adding 0.5% compound IA1, 0.4% compound IB25 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1291] Embodiment 80

[1292] Polymerizable mixture P80 was prepared by adding 0.5% compound IA1, 0.4% compound IB111 and 150 ppm stabilizer ST-3a-1 to the nematic LC host mixture N1.

[1293]

[1294] Embodiment 81

[1295] Polymerizable mixture P81 was prepared by adding 0.5% of compound IA1, 0.4% of compound IB111 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1296] Embodiment 82

[1297] Polymerizable mixture P82 was prepared by adding 0.5% compound IA1, 0.4% compound IB113 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N3.

[1298]

[1299] Embodiment 83

[1300] Polymerizable mixture P83 was prepared by adding 0.5% of compound IA1, 0.4% of compound IB113 and 150 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1301] Embodiment 84

[1302] Polymerizable mixture P84 was prepared by adding 0.5% compound IA1, 0.4% compound IB90 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N1.

[1303]

[1304] Embodiment 85

[1305] Polymerizable mixture P85 was prepared by adding 0.5% compound IA1, 0.3% compound IB90 and 150 ppm stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1306] Embodiment 86

[1307] Polymerizable mixture P86 was prepared by adding 0.45% of compound IA5 and 0.05% of compound IB133 to the nematic LC host mixture N1.

[1308]

[1309] The VHR values ​​of mixture P86 before and after UV exposure were measured as described in Example 1. The results are shown in Table 4.1.

[1310] Table 4.1 – VHR

[1311] mixture P86 VHR (%) Initial 96.1 VHR (%) after 0.5 hours UV 90.2

[1312] It can be seen that polymerizable mixture P86 shows only a small decrease in VHR after UV stress compared to reference mixtures C1A and C1B from Example 1.

[1313] The residual content of unpolymerized monomers in mixture P86 (in ppm) was measured as described in Example 1. The results are shown in Table 4.2.

[1314] Table 4.2 – Residual RM

[1315]

[1316] nd = Not Detectable

[1317] It can be seen that in the polymerizable mixture P86, the residual contents of both monomers IA5 and IB133 after polymerization decrease rapidly.

[1318] Embodiment 87

[1319] Polymerizable mixture P87 was prepared by adding 0.5% compound IA5, 0.1% compound IB133 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1320] Embodiment 88

[1321] Polymerizable mixture P88 was prepared by adding 0.4% compound IA5, 0.25% compound IB1 and 100 ppm stabilizer ST-8-1 to the nematic LC host mixture N2.

[1322] Embodiment 89

[1323] Polymerizable mixture P89 was prepared by adding 0.45% compound IA5, 0.1% compound IB3 and 100 ppm stabilizer ST-8-1 to the nematic LC host mixture N2.

[1324] Embodiment 90

[1325] Polymerizable mixture P89 was prepared by adding 0.35% compound IA5, 0.25% compound IB2 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1326] Embodiment 91

[1327] Polymerizable mixture P91 was prepared by adding 0.4% compound IA5, 0.2% compound IB135 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N74.

[1328] Embodiment 92

[1329] Polymerizable mixture P92 was prepared by adding 0.3% compound IA5, 0.2% compound IB6 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1330] Embodiment 93

[1331] The polymerizable mixture P93 was prepared by adding 0.4% of compound IA5, 0.2% of compound IB69 and 100 ppm of stabilizer ST-3a-1 to the nematic LC host mixture N2.

[1332] Embodiment 94

[1333] Polymerizable mixture P94 was prepared by adding 0.5% compound IA5, 0.1% compound IB33 and 100 ppm stabilizer ST-3a-1 to the nematic LC host mixture N62.

[1334] Embodiment 95

[1335] Polymerizable mixture P95 was prepared by adding 0.5% compound IA6, 0.4% compound IB1 and 100 ppm stabilizer ST-3a-1 to nematic LC host mixture N1

[1336]

[1337] Embodiment 96

[1338] Polymerizable mixture P96 was prepared by adding 0.4% compound IA6, 0.25% compound IB1 and 100 ppm stabilizer ST-8-1 to the nematic LC host mixture N2.

[1339] Embodiment 97

[1340] Polymerizable mixture P97 was prepared by adding 0.45% of compound IA6, 0.05% of compound IB133 and 100 ppm of stabilizer ST-12-1 to the nematic LC host mixture N62.

Claims

1. An LC medium comprising one or more polymerizable compounds of formula IA and one or more polymerizable compounds of formula IB P-Sp-M 1 -Sp-P IA P-Sp-M 2 -Sp-P IB where the individual radicals independently of one another and on each occurrence have the following meanings identically or differently P is a polymerizable group, Sp is a spacer group or a single bond, M 1 is a benzene ring optionally substituted by one or more groups L or P-Sp-, M 2 is a group selected from Formulas 1 to 3 wherein the benzene ring is optionally substituted by one or more groups L or P-Sp-, L is F, Cl, -CN, or a straight-chain, branched or cyclic alkyl group having 1 to 25 C atoms, wherein one or more non-adjacent CH2- groups are optionally replaced by -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O-, in a manner such that the O- and / or S- atoms are not directly connected to each other, and wherein one or more H atoms are each optionally replaced by P, F or Cl.

2. LC medium according to claim 1, characterized in that In formula IA, all polymerizable groups P represent methacrylate.

3. LC medium according to claim 1 or 2, characterized in that The compound of formula IA is selected from the following subformulae: wherein P, Sp and L have the meanings given in claim 1 or 2, r1 is 0, 1, 2, 3 or 4 and r2 is 0, 1, 2 or 3.

4. LC medium according to one or more of claims 1 to 3, characterized in that The compound of formula IA is selected from the following subformulae: wherein P, Sp and L have the meanings given in claim 1 or 2 and Sp is different from a single bond.

5. LC medium according to one or more of claims 1 to 4, characterised in that The compound of formula IA is selected from the following subformulae:

6. LC medium according to one or more of claims 1 to 5, characterised in that The compound of formula IB is selected from the following subformulae: wherein P, Sp and L have the meanings given in claim 1 or 2, r1, r2, r3 are independently 0, 1, 2, 3 or 4, and r4 is 0, 1, 2 or 3.

7. LC medium according to one or more of claims 1 to 6, characterised in that It comprises one or more compounds of formula II: where the individual radicals independently of one another and on each occurrence have the following meanings identically or differently R 21 , R 22 is H, a straight-chain, branched or cyclic alkyl or alkoxy radical having 1 to 20 C atoms, wherein one or more non-adjacent CH2- groups are optionally connected via -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O-, CR- 0 =CR 00 -、-C≡C-、 substituted, and wherein one or more H atoms are each optionally replaced by F, Cl, CN or CF3, R 0 , R 00 is H or an alkyl radical having 1 to 12 C atoms, A 1 , A 2 is a group selected from the following formulae: Z 1 and Z 2 is -CH2CH2-, -CH=CH-, -CF2O-, -OCF2-, -CH2O-, -OCH2-, -CO-O-, -O-CO-, -C2F4-, -CF=CF-, -CH=CH-CH2O- or a single bond, L 1 , L 2 , L 3 , L 4 is F, Cl, OCF3, CF3, CH3, CH2F or CHF2, Y is H, F, Cl, CF3, CHF2 or CH3, L C is CH3 or OCH3, a1 is 0, 1, or 2, a2 is 0 or 1.

8. LC medium according to any one of claims 1 to 7, characterised in that It further comprises one or more compounds selected from the group consisting of compounds of formula IIA, IIB, IIC and IID: The individual radicals have the following meanings each time they occur, identically or differently and independently of one another: R 21 , R 22 is H, alkyl, alkoxy or alkenyl with up to 15 C atoms, which is unsubstituted or monosubstituted by F, Cl, CN or CF3 and in addition, one or more CH2 groups in these groups can be connected via -O-, -S-, -C≡C-, -CF2O-, -OCF2-, -OC-O or -O-CO-, in such a way that the O- and / or S-atoms are not directly connected to each other. Instead, L 1 To L 4 is F, Cl, CF3 or CHF2, Y is H, F, Cl, CF3, CHF2 or CH3, Z 1 , Z 2 is a single bond, -CH2CH2-, -CH=CH-, -CF2O-, -OCF2-, -CH2O-, -OCH2-, -COO-, -OCO-, -C2F4-, -CF=CF-, -CH=CHCH2O-, p is 0, 1, or 2, and q is 0 or 1.

9. LC medium according to one or more of claims 1 to 8, characterised in that It comprises one or more compounds of formula III: where the individual radicals independently of one another and on each occurrence have the following meanings identically or differently R 31 , R 32 is H, alkyl, alkoxy or alkenyl with up to 15 C atoms, which is unsubstituted or monosubstituted by F, Cl, CN or CF3 and in addition, one or more CH2 groups in these groups can be connected via -O-, -S-, -C≡C-, -CF2O-, -OCF2-, -OC-O-, -O-CO ... Instead, A 3 a) 1,4-cyclohexenylene or 1,4-cyclohexylene, in which one or two non-adjacent CH2 groups may be replaced by -O- or -S-, b) 1,4-phenylene, in which one or both CH groups may be replaced by N, or c) a group selected from the group consisting of spiro[3.3]heptane-2,6-diyl, 1,4-bicyclo[2.2.2]octane-2,6-diyl, naphthalene-2,6-diyl, decahydronaphthalene-2,6-diyl, 1,2,3,4-tetrahydronaphthalene-2,6-diyl, phenanthrene-2,7-diyl and fluorene-2,7-diyl, wherein the groups a), b) and c) may be singly or polysubstituted by halogen atoms, n is 0, 1, or 2, Z 1 is -CO-O-, -O-CO-, -CF2O-, -OCF2-, -CH2O-, -OCH2-, -CH2-, -CH2CH2-, -(CH2)4-, -CH=CH-CH2O-, -C2F4-, -CH2CF2-, -CF2CH2-, -CF=CF-, -CH=CF-, -CF=CH-, -CH=CH-, -C≡C- or a single bond, L 11 , L 12 is F, Cl, CF3 or CHF2, W is O or S, Y 1 , Y 2 It is H, F, Cl, CF3, CHF2, CH3 or OCH3.

10. LC medium according to one or more of claims 1 to 9, characterised in that It comprises one or more compounds of formula IV: in R 41 represents an unsubstituted alkyl radical having 1 to 7 C atoms, in which, in addition, one or more CH2 groups may be substituted or unsubstituted alkenyl having 2 to 7 C atoms, and R 42 represents an unsubstituted alkyl group having 1 to 7 C atoms or an unsubstituted alkoxy group having 1 to 6 C atoms.

11. LC medium according to one or more of claims 1 to 10, characterised in that It comprises one or more compounds of formula V: in R 51 , R 52 independently of one another denotes H, alkyl, alkoxy or alkenyl having up to 15 C atoms, which is unsubstituted, monosubstituted by F, Cl, CN or CF3 or at least monosubstituted by halogen, wherein, in addition, one or more CH2 groups in these radicals may be connected via -O-, -S-, -C≡C-, -CF2O-, -OCF2-, -OC-O-, -O-CO-, -S-, -C≡C ...C≡C-, -C≡C-, -C≡C-, -C≡C-, -C≡C-, -C≡C-, -C≡C-, -C≡C-, -C≡C-, -C≡ Instead, Same or different Z 51 , Z 52 Each independently represents -CH2-CH2-, -CH2-O-, -CH=CH-, -C≡C-, -COO- or a single bond, and n is 1 or 2.

12. LC medium according to one or more of claims 1 to 11, characterised in that It further comprises one or more additives selected from the group consisting of a chiral dopant, a stabilizer, a polymerization initiator and a self-aligning additive.

13. A process for the preparation of an LC medium according to one or more of claims 1 to 12, comprising the following steps: Mixing one or more polymerizable compounds as defined in one or more of claims 1 to 6 with one or more compounds of the formula II, III, IV and / or V as defined in one or more of claims 7 to 11, and optionally with further liquid-crystalline compounds and / or additives, and optionally polymerizing the polymerizable compounds.

14. An LC display comprising an LC medium as defined in one or more of claims 1 to 12.

15. An LC display according to claim 14 which is a PS-VA, PS-IPS, PS-FFS or SA-VA display.

16. LC display according to claim 14 or 15, characterized in that It comprises two substrates, at least one of which is transparent to light; an electrode arranged on each substrate or two electrodes arranged on only one of the substrates; and a layer of LC medium according to one or more of claims 1 to 12 positioned between the substrates, wherein the polymerizable compound is polymerized by UV light polymerization between the substrates of the display.

17. A method for producing an LC display according to claim 16, comprising the following steps: An LC medium according to one or more of claims 1 to 12 is provided between the substrates of the display, and the polymerisable compound is polymerised by irradiation with UV light.

18. A method according to claim 18, wherein a voltage is applied to an electrode of the display during polymerisation of the polymerisable compound.

19. The method according to claim 17 or 18, wherein the irradiation is performed using a UV C lamp or a UV B lamp.

20. Use of an LC medium according to one or more of claims 1 to 12 or an LC display according to one or more of claims 14 to 16 or a process according to one or more of claims 17 to 19 for energy-saving LC displays or for a process for the production of energy-saving LC displays.

21. A compound selected from the following formula:

Citation Information

Patent Citations

  • modified NEMATIC PHASES

    DE2209127A1

  • Liquid crystalline dielectrics for electronic components - contg biphenylyl carboxylic acid phenyl ester or benzoic acid biphenylyl ester components

    DE2450088A1

  • phenylcyclohexane derivatives and their use in liquid crystalline dielectrics

    DE2636684A1

  • Heterocyclic diaza cpd. in liquid crystalline dielectric - for electrooptical registration devices, giving stable orientation parallel to electrode surfaces

    DE2637430A1

  • LIQUID-CRYSTALLINE CARBONIC ACID ESTERS, PROCESS FOR THEIR PRODUCTION, DIELECTRICS CONTAINING THEM AND ELECTROOPTIC DISPLAY ELEMENT

    DE2853728A1

Cited By

  • Liquid crystal composition, liquid crystal display device comprising the liquid crystal composition

    TWI931162B