Nickel-based wear-resistant anti-corrosion drill handle adapter
By applying a combination of nickel-based corrosion-proof layer and polymer-based sealant top layer on the drill handle adapter, the corrosion resistance and wear resistance of the drill handle adapter is solved, significantly extending its service life and reducing wear of the seals , achieving higher corrosion resistance and wear resistance.
Patent Information
- Application Number
- CN202380038988.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-20
- Filing Date
- 2023-05-17
- Publication Date
- 2024-12-06
AI Technical Summary
Existing drill handle adapters are susceptible to corrosion by the flushing medium during use, resulting in reduced functionality and reduced mechanical strength, and premature seal failure, which cannot effectively solve the corrosion resistance and wear resistance problems.
Coated nickel-based anti-corrosion layer on the exterior and interior surfaces of the drill handle adapter combined with a polymer-based sealant top layer to provide corrosion protection and low friction effects, delay radial crack propagation and lateral fracture, and improve seal life.
Through the combination of nickel-based corrosion-proof layer and polymer-based sealant top layer, the corrosion resistance and wear resistance of the drill handle adapter is significantly improved, and its service life is extended, as well as reducing wear of the flush seal, delaying corrosion and The occurrence of wear.
Smart Images

Figure CN119096031A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a drill shank adapter for top hammer rock drilling having a corrosion and / or wear protection layer. Background Art
[0002] The drill shank adapter is used as a main component in rock drilling rigs, which transfers the impact energy from the piston to the drill string when rotating. In addition, the drill shank adapter is used to transfer the flushing medium from the rock drilling rig into the drill string. Since the drill shank adapter needs to have a high impact resistance, they are usually made of high-strength case-hardened steel. However, a disadvantage of this material is that it is corroded by the flushing medium, which may, for example, contain chlorides, sulfides or other ions that accelerate corrosion. If the drill shank adapter is corroded, its functionality is reduced. As the mechanical strength of the material decreases, the steel may, for example, have problems with stress corrosion cracking.
[0003] Furthermore, it is important to maintain the integrity of the seal inside the flush housing to prevent flush water leakage and maintain good flush pressure. In order for the seal to not wear out prematurely, it is important to keep the surface of the drill shank adapter that contacts the seal in good non-corrosive condition. Corroded surfaces are highly abrasive and can lead to premature failure of the seal in the flush housing of a rock drill rig.
[0004] It is therefore advantageous to provide an anti-corrosion coating on the surface of the drill shank adapter.
[0005] A known method for corrosion protection on a drill shank adapter is to provide a hard chrome coating on its surface. However, the hard chrome layer contains pores and microcracks which can serve as passages for water to penetrate and reach the surface of the drill shank adapter, thereby removing the corrosion protection. Therefore, the problem to be solved is how to provide a method for improving the corrosion resistance and / or wear resistance of the surface of a drill shank adapter. Summary of the invention
[0006] The object of the present invention is to provide measures for increasing the corrosion resistance and / or wear resistance of a drill shank adapter. This object is achieved by providing a drill shank adapter forming part of a drilling assembly, the drill shank adapter comprising: a longitudinal axis; an outer surface; an inner surface; a threaded portion provided at a front end and a plurality of splines provided at a rear end; and a machine portion extending axially between the threaded portion and the splines; wherein at least a portion of the outer surface is coated with a first corrosion protection layer comprising nickel; characterised in that at least a portion of the first corrosion protection layer is coated with a polymer-based sealant top layer.
[0007] Advantageously, the combination of the nickel-based anti-corrosion layer and the polymer-based sealant top sealant results in fewer open cracks and defects between the atmosphere and the steel substrate, thereby achieving improved corrosion resistance. The coating combination provides an anti-corrosion layer on the drill shank adapter and around the flushing slots, thereby delaying radial crack propagation of the drill shank diameter and thus delaying transverse fracture of the threaded portion or machine portion. In addition, the coating combination provides a low-friction surface. The low-friction coating is beneficial to reduce wear on the flushing seal and other rock drill components, thereby further increasing the service life of the seal. In addition, the solution provides high wear resistance and reduced galling.
[0008] In one embodiment, at least a portion of the interior surface is additionally coated with a first anti-corrosion layer and / or a polymer-based sealant top layer. Advantageously, this provides protection against cavitation and corrosion on the interior as well as the exterior of the drill shank adapter, thereby extending the life of the drill shank adapter.
[0009] In one embodiment, the thickness of the first anti-corrosion layer is between 5 and 200 microns. Advantageously, this thickness provides an optimal balance between providing adequate corrosion and wear protection without adding excessive cost.
[0010] In one embodiment, the polymer-based sealant top layer has a thickness of between 0.5-10 microns. Advantageously, this provides an optimal balance of being thick enough to be effective without unnecessarily increasing cost or increasing the risk of streaking when the coating dries. The polymer-based sealant top layer may also penetrate into cracks, providing additional adhesion and corrosion protection.
[0011] In one embodiment, the first corrosion protection layer is a nickel phosphorus alloy. Advantageously, nickel phosphide provides a hard coating and thus increases wear resistance.
[0012] In one embodiment, the phosphorus content of the nickel phosphorus alloy is 6-9 weight percent. Advantageously, this phosphorus content provides increased wear resistance without undesirable brittleness.
[0013] In one embodiment, the polymer-based sealant top layer comprises a polymer having a coefficient of friction between 0.05-0.15. Advantageously, the low friction coating helps reduce wear on the flush seal and other rock drill components, thereby further increasing the useful life of the seal.
[0014] In one embodiment, the first anti-corrosion and polymer-based sealant top layer is located on the machine portion. Advantageously, this provides corrosion protection for the areas of the drill shank adapter that are most exposed to corrosion and most important to be protected from corrosion.
[0015] In one embodiment, the first anti-corrosion layer and the top layer of polymer-based sealant are located on all parts of the drill shank adapter. Advantageously, this provides a high degree of all-round corrosion resistance.
[0016] In one embodiment, the rear end of the drill shank adapter (also referred to as the impact face) is uncoated. Advantageously, this avoids unwanted spalling in this area, which could adversely block the circulation system.
[0017] According to another aspect of the present application is a method for providing corrosion protection on a drill shank adapter as described above or below, comprising the following steps: - depositing a first corrosion protection layer comprising nickel on at least a portion of the outer surface of the drill shank adapter; - depositing a top layer of a polymer-based sealant on top of the first anti-corrosion layer; - Heat treated coated drill shank adapter.
[0018] Advantageously, the method provides a measure of providing a drill shank adapter with highly effective corrosion protection, as well as a low friction and high wear resistance coating.
[0019] In one embodiment, the first anti-corrosion layer is applied using an electroless nickel plating bath. Advantageously, the process is fast and less harmful to the environment than chrome plating. Another benefit of the process is the ability to provide a coating with a more uniform thickness and a high degree of reproducibility.
[0020] In one embodiment, a top layer of polymer-based sealant is sprayed on. Advantageously, the method provides a coating having a uniform thickness.
[0021] In one embodiment, the heat treatment is performed at a temperature between 150-300° C. for 30-120 minutes. Advantageously, this temperature range provides a balance between having sufficiently high temperatures and heating times to form a hard and wear resistant surface without having excessively high temperatures and times that the surface hardening properties of the steel substrate are adversely affected.
[0022] In one embodiment, the surface of the drill shank adapter is shot peened or sand blasted prior to applying the nickel based anti-corrosion layer. Advantageously, this step provides improved adhesion of the anti-corrosion layer to the surface of the drill shank adapter. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Specific embodiments of the present invention will now be described, by way of example only, with reference to the accompanying drawings, in which:
[0024] Figure 1 is a schematic diagram of a drill shank adapter.
[0025] Figure 2 is a schematic diagram of an embodiment of an anti-corrosion layer. DETAILED DESCRIPTION
[0026] Figure 1 A drill shank adapter 2 forming part of a drilling assembly is shown, the drill shank adapter 2 comprising: a longitudinal axis 4; an outer surface 6; an inner surface 8; a threaded portion 10 provided at a front end 12 and a plurality of radially outwardly projecting splines 32 provided at a rear end 14; and a machine portion 16 (also referred to as a body) extending axially between the threaded portion 10 and the splines 32. The splines 32 are configured to be engaged by corresponding splines of a drive bushing in a rotary motor (not shown) to cause the drill shank adapter 2 to rotate about the axis 4 during a drilling operation. The threaded portion 10 may be a male or female thread. The drill shank adapter further comprises a flushing slot 26 providing access to a flushing hole or probe hole (not shown) extending radially through the machine portion 16 in the form of an internal cavity. The drill shank adapter 2 is configured for coupling to an elongated drill string and allowing stress waves to be transmitted to a drill bit (not shown) located at the deepest region of the borehole to apply an impact drilling action. In particular, the front end 12 can be coupled to the rear end of an extended drill rod forming the rearmost of a portion of the drill string, or to a coupler (not shown). The rear end 14, also referred to as the impact surface, is configured to be contacted by a hydraulically driven piston (not shown) that generates a stress wave in the drill shank adapter 2 and the drill string. Optionally, the front end 12 further includes an annular shoulder 28 from which the threaded portion 10 axially protrudes. Optionally, the elongated portion 30 is axially positioned between the machine portion 16 and the threaded portion 10.
[0027] Figure 2 At least a portion of the outer surface 6 of the drill shank adapter 2 is shown coated with a first corrosion protection layer 18 comprising nickel. At least a portion of the first corrosion protection layer 18 is coated with a polymer-based sealant top layer 20. Areas of the outer surface 6 of the drill shank adapter 2 that are not coated with the first corrosion protection layer 18 may also be coated with the polymer-based sealant top layer 20. Part or all of the first corrosion protection layer 18 may be coated with the polymer-based sealant top layer 20.
[0028] At least a portion of the interior surface 8 of the drill shank adapter 2 may also be coated with the first anti-corrosion layer 18 and / or the polymer-based sealant top layer 20. The interior surface 8 of the drill shank adapter 2 includes a flushing slot 26 and a flushing hole / probe extending radially through the machine portion to the threaded opening. At least a portion or all of the interior surface 8 may be coated with only the first anti-corrosion layer 18. At least a portion or all of the interior surface 8 may be coated with only the polymer-based sealant top layer 20. At least a portion or all of the interior surface may be coated with both the first anti-corrosion layer 18 and the polymer-based sealant top layer 20. Any combination of these options is possible.
[0029] In one embodiment, the thickness of the first anti-corrosion layer 18 is between 5 and 200 micrometers, more preferably between 7 and 100 micrometers, and even more preferably between 10 and 50 micrometers.
[0030] In one embodiment, the thickness of the polymer-based sealant top layer 20 is between 0.5-10 microns, preferably between 0.5-5 microns.
[0031] The first corrosion protection layer 18 may be nickel alloyed with sulfur, phosphorus, boron or any other suitable element. Preferably, the first corrosion protection layer 18 is a nickel-phosphorus alloy. Preferably, the phosphorus content of the nickel-phosphorus alloy is 6-9 weight percent.
[0032] In one embodiment, the polymer-based sealant top layer 20 comprises a polymer having a coefficient of friction less than 0.05-0.15, preferably 0.1-0.13. For example, the polymer may be Teflon or a fluorinated polymer such as polytetrafluoroethylene (PTFE) or a non-fluorinated crystalline polymer such as polyetheretherketone (PEEK) or a high-density polymer such as ultra-high molecular weight polyethylene (UHMWPE).
[0033] In one embodiment, the first corrosion resistant layer 18 and the polymer-based sealant top layer 20 are located on the machine portion 16. In one embodiment, the first corrosion resistant layer 18 and the polymer-based sealant top layer 20 are limited to being located only on the machine portion 16. In other words, the first corrosion resistant layer 18 is not located on the splines 32 or the threaded portion 10. Alternatively, the entire exterior surface 6 of the drill shank adapter 2 is coated with the first corrosion resistant layer 18 and the polymer-based sealant top layer 20.
[0034] In one embodiment, the first corrosion protection layer 18 and the polymer-based sealant top layer 20 are located within the flushing slot 26, which results in less cracking on the machine portion.
[0035] In one embodiment, a first corrosion protection layer 18 and a top layer 20 of a polymer-based sealant are located on the threaded portion 10 .
[0036] In one embodiment, the rear end / strike surface 14 of the drill shank adapter 2 remains uncoated. In other words, the rear end / strike portion 14 of the drill shank adapter is free of the first anti-corrosion layer 18 and the polymer-based sealant top layer 20. In one embodiment, all portions of the drill shank adapter 2 except the rear end / strike surface 14 are coated with the first anti-corrosion layer 18 and the polymer-based sealant top layer 20.
[0037] The present application further relates to a method for providing corrosion protection on a drill shank adapter 2, comprising the following steps:
[0038] a) depositing a first corrosion protection layer 18 comprising nickel on at least a portion of the outer surface 6 of the drill shank adapter 2;
[0039] b) depositing a polymer-based sealant top layer 20 on top of the first anti-corrosion layer 18;
[0040] c) Heat treating the coated drill shank adapter 20.
[0041] In one embodiment, the first corrosion protection layer 18 is applied using an electroless nickel bath. Nickel or a nickel-based alloy adheres to the substrate, which is the metal of the drill shank adapter. In electroless nickel plating, the object reacts with the plating bath chemistry to produce a uniform and smooth layer with very little surface porosity. The uniform deposition makes it ideal for complex, non-line-of-sight geometries, and post-plating grinding is generally not required. Alternatively, the first corrosion protection layer can be applied by electroplating or any other suitable method.
[0042] In one embodiment, the polymer-based sealant top layer 20 is sprayed on. Alternatively, the polymer-based sealant top layer 20 may be applied by dipping or any other suitable method.
[0043] The purpose of the heating step is to enable the formation of a Ni-P intermetallic phase to improve adhesion to the substrate and to cure the polymer-based sealant top layer. Typically, this heat treatment is performed in a furnace.
[0044] In one embodiment, the heat treatment is performed at a temperature of 150-300° C., preferably 225-260° C. In one embodiment, the heat treatment is performed for 30-120 minutes, preferably 45-75 minutes.
[0045] The same method may be used to apply the first corrosion protection layer 18 and / or the polymer-based sealant top layer 20 to the interior surface 8 of the drill shank adapter 2 .
[0046] In one embodiment, the surface of the drill shank adapter (2) is shot peened or sand blasted before the nickel-based anti-corrosion layer (18) is applied.
[0047] A drill shank adapter as described above or below may be part of a drill string and / or a drilling rig arrangement.
[0048] Example
[0049] Overview of the tested drill shank adapters
[0050] Table 1 shows the corrosion protection applied to the drill shank adapters used in the field trials:
[0051] Drill shank adapter Anti-corrosion coating A (the present invention) Contains a first layer of nickel corrosion protection and a top layer of polymer-based sealant (Nedox 10k3 from Magnaplate) B (Control) Hard chrome anti-corrosion layer, thickness is about 40 microns. C (Control) No corrosion protection Table 1: Overview of drill shank adapter coatings
[0052] Field Test 1
[0053] Field trials were conducted in a mine in Sweden. The number of drilling meters and the drilling duration were recorded for each tested drill shank adapter. In this test, two drill shank adapters failed after a similar number of drilling meters, however the reasons for failure were different. Delamination of abrasive corrosion pits was observed for the chrome-plated control drill shank adapter B, thus indicating that corrosion was the main cause of failure. The drill shank adapter A of the present invention did not have any delamination of abrasive corrosion pits and showed significantly less general corrosion than the drill shank adapter B. In contrast, the drill shank adapter A of the present invention failed due to thread wear. Therefore, for the control drill shank adapter B, corrosion was the limiting factor for the life of the drill shank adapter, while for the drill shank adapter A of the present invention, corrosion was not a limiting factor after approximately the same number of drilling hours.
[0054] Field Test 2
[0055] Another field trial was conducted in a mine in Australia. Table 2 shows the number of hours of drilling before the drill shank adapter failed.
[0056] Drill shank adapter Meters drilled before failure A (the present invention) 4800 B (Control) 1950 Table 2: Meters drilled before failure in field test 2
[0057] It can be seen that the drill shank adapter A of the present invention significantly outperforms the control drill shank adapter B in terms of meters drilled before failure, thus demonstrating that the life of the drill shank adapter having corrosion protection according to the present invention is significantly increased.
[0058] Field Test 3
[0059] Another field trial was conducted in a mine in India, which normally does not have significant corrosion problems. It was found that the life of the drill shank adapter of the drill shank adapter A of the present invention was improved by 27% compared to the control drill shank adapter C. It was observed that the drill shank adapter A of the present invention did not break inside the rock drill and improved the service life of the seals in the rock drill.
Claims
1. A drill shank adapter (2) forming part of a drilling assembly, the drill shank adapter (2) comprising: longitudinal axis (4); external surface(6); Internal surface (8); a threaded portion (10) disposed at a front end (12) and a plurality of splines (32) disposed at a rear end (14); and a machine portion (16) extending axially between the threaded portion (10) and the spline (32); wherein at least a portion of the outer surface (6) is coated with a first anti-corrosion layer (18) comprising nickel; Features: At least a portion of the first anti-corrosion layer (18) is coated with a top layer (20) of a polymer-based sealant.
2. The drill shank adapter (2) according to claim 1, wherein: At least a portion of the interior surface (8) is additionally coated with the first anti-corrosion layer (18) and / or the polymer-based sealant top layer (20).
3. The drill shank adapter (2) according to claim 1 or claim 2, wherein: The thickness of the first anti-corrosion layer (18) is between 5 and 200 micrometers.
4. A drill shank adapter (2) according to any one of the preceding claims, wherein The thickness of the polymer-based sealant top layer (20) is between 0.5 and 10 microns.
5. A drill shank adapter (2) according to any one of the preceding claims, wherein The first anti-corrosion layer (18) is a nickel-phosphorus alloy.
6. The drill shank adapter (2) according to claim 5, wherein: The phosphorus content of the nickel-phosphorus alloy is 6-9 weight percent.
7. A drill shank adapter (2) according to any one of the preceding claims, wherein The polymer-based sealant top layer (20) comprises a polymer having a coefficient of friction between 0.05 and 0.
15.
8. A drill shank adapter (2) according to any one of the preceding claims, wherein The first anti-corrosion layer (18) and the polymer-based sealant top layer (20) are located on the machine part (16).
9. A drill shank adapter (2) according to any one of the preceding claims, wherein The first anti-corrosion layer (18) and the polymer-based sealant top layer (20) are located on all parts of the drill shank adapter (2).
10. The drill shank adapter (2) according to any one of claims 1 to 8, wherein: The rear end (14) of the drill shank adapter (2) is uncoated.
11. A method for providing corrosion protection on a drill shank adapter (2) according to any one of claims 1 to 10, comprising the following steps: - depositing a first corrosion protection layer (18) comprising nickel on at least a portion of the outer surface (6) of the drill shank adapter (2); - depositing a polymer-based sealant top layer (20) on top of said first anti-corrosion layer (18); - Heat treating the coated drill shank adapter (20).
12. The method according to claim 11, wherein: The first anti-corrosion layer (18) is applied using an electroless nickel plating bath.
13. The method according to claim 11 or 12, wherein: The polymer based sealant top layer (20) is sprayed on.
14. The method according to any one of claims 11 to 13, wherein: The heat treatment is performed at a temperature between 150-300° C. for 30-120 minutes.
15. The method according to any one of claims 11 to 14, wherein: The surface of the drill shank adapter (2) is shot blasted or sand blasted before the nickel-based anti-corrosion layer (18) is applied.