Simulation method, method for manufacturing semiconductor device, and semiconductor device
Through simulation method and structure analysis software, the cross-sectional area of the reinforced material in the semiconductor package is optimized, and the curable resin composition is used to solve the problem of connection strength deterioration caused by traditional resin materials, and the high-frequency radio wave transmission efficiency and reliable connection of 5G communication equipment are improved. sex.
Patent Information
- Application Number
- CN202280095457.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-09
- Publication Date
- 2024-12-06
AI Technical Summary
In 5G communication devices, conventional resin materials cause lower high-frequency radio wave transmission efficiency of semiconductor packages, and expansion and contraction of reinforcement materials lead to deterioration of connection strength, and a method is needed to ensure the connection strength between the element and the substrate.
The cross-sectional area relationship between the strain value of the connection part and the reinforced material is calculated by simulation method, and a simulation model is made using structural analysis software, an approximate curve is derived to determine the optimal cross-sectional area of the reinforced material, and a curable resin composition is used as the reinforced material to ensure that Strength of the connection.
Accuracy analysis and optimization of the strength of the component and substrate connection part is achieved, the connection reliability of the semiconductor device is improved, and the communication delay risk is reduced.
Smart Images

Figure BDA0005104899800000131 
Figure BDA0005104899800000141 
Figure BDA0005104899800000142
Abstract
Description
Technical Field
[0001] The present disclosure relates to a simulation method, a method for manufacturing a semiconductor device, and a semiconductor device. Background Art
[0002] In the conventional semiconductor package mounting technology, a semiconductor chip or other element is arranged on a substrate via a conductive connection portion such as solder, and the space around the connection portion is filled with a resin material called an underfill material. The improvement of the physical properties of these resin materials has been explored to meet the requirements corresponding to the purpose of use. For example, Patent Document 1 describes an underfill material that combines the suppression of the increase in thermal expansion coefficient after curing and the reduction of viscosity during filling by including an aminophenol-type epoxy resin.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2019-011409 Summary of the invention
[0006] Technical problem to be solved by the invention
[0007] In recent years, with the popularization of the fifth generation mobile communication standard (5G) technology, new technical problems have arisen in the installation technology of semiconductor packages used in communication equipment, etc. For example, it has been pointed out that the resin material that has been used has become a cause of reducing the transmission efficiency of high-frequency radio waves, and communication delays may occur. Therefore, instead of filling the space around the connection part with a resin material, a structure in which a reinforcing material is arranged only around the periphery of the element is explored.
[0008] In the above structure, since the area around the connection part is not filled with resin material, there is a risk that the connection part will be strained due to expansion and contraction of the reinforcing material arranged at the periphery of the element, and the connection part may be deteriorated. Therefore, in the above structure, it is necessary to ensure sufficient strength of the connection part.
[0009] In view of the above facts, one aspect of the present disclosure is to provide a simulation method that can accurately analyze the strength of the connection between the element and the substrate. Another aspect of the present disclosure is to provide a method for manufacturing a semiconductor device having excellent strength of the connection between the element and the substrate and a semiconductor device.
[0010] Means for solving technical problems
[0011] <1> A simulation method comprising the following steps:
[0012] The step of preparing a simulation model of a semiconductor device, the semiconductor device comprising a substrate, an element, a connection portion electrically connecting the substrate and the element, and a reinforcing material disposed around the periphery of the element; and
[0013] A step of calculating the amount of strain of the simulation model with respect to the connection portion.
[0014] <2> according to <1> The simulation method further comprises the step of deriving an approximate curve of an Nth-order polynomial represented by the following formula (1) from the strain amount Y calculated using the simulation model and the corresponding cross-sectional area X of the reinforcement material.
[0015] Formula (1) Y = aX N +cX (N-1) +dX (N-2) +…+b
[0016] In the formula, a, b, c and d are arbitrary constants, and N is an integer greater than or equal to 2.
[0017] <3> according to <1> or <2> The simulation method, wherein the simulation model is produced using structural analysis software.
[0018] <4> A method for manufacturing a semiconductor device, the semiconductor device comprising a substrate, a semiconductor device, a connection portion for electrically connecting the substrate and the semiconductor device, and a reinforcing material disposed at a peripheral portion of the semiconductor device.
[0019] The manufacturing method includes the step of determining a cross-sectional area X of the reinforcing material according to a strain amount Y of the connecting portion.
[0020] <5> according to <4> The method for manufacturing a semiconductor device, wherein the cross-sectional area X of the reinforcing material satisfies the following formula (2):
[0021] Formula (2): X min ×0.7≤X≤X min ×1.3
[0022] Where, X min It is the cross-sectional area of the reinforcing material when the strain Y about the connection part reaches the minimum value.
[0023] <6> according to <4> In the method for manufacturing a semiconductor device, the strain amount Y of the connection portion is calculated using a simulation model.
[0024] <7> according to <4> In the method for manufacturing a semiconductor device, the reinforcing material is a cured product of a curable resin composition.
[0025] <8> according to <7> In the method for manufacturing a semiconductor device, the curable resin composition comprises an epoxy resin.
[0026] <9> according to <5> The manufacturing method of the semiconductor device described above, wherein the glass transition temperature Tg of the above-mentioned reinforcement material is above 100°C, the thermal expansion coefficient CTE1 in the temperature range below the glass transition temperature is below 25ppm / °C, and the thermal expansion coefficient CTE2 in the temperature range above the glass transition temperature is below 80ppm / °C.
[0027] <10> A semiconductor device comprises a substrate, an element, a connection portion for electrically connecting the substrate and the element, and a reinforcing material arranged at a peripheral portion of the element.
[0028] The cross-sectional area X of the reinforcing material satisfies the following formula (2):
[0029] Formula (2): X min ×0.7≤X≤X min ×1.3
[0030] Where, X min It is the cross-sectional area of the reinforcing material when the strain Y about the connection part reaches the minimum value.
[0031] <11> according to <10> The semiconductor device described above, wherein the reinforcing material is a cured product of a curable resin composition.
[0032] <12> according to <10> The semiconductor device described above, wherein the curable resin composition contains an epoxy resin.
[0033] <13> according to <10> The semiconductor device described above, wherein the glass transition temperature Tg of the above-mentioned reinforcement material is above 100°C, the thermal expansion coefficient CTE1 in the temperature range below the glass transition temperature is below 25ppm / °C, and the thermal expansion coefficient CTE2 in the temperature range above the glass transition temperature is below 80ppm / °C.
[0034] Effects of the Invention
[0035] According to one embodiment of the present disclosure, a simulation method capable of accurately analyzing the strength of a connection portion between an element and a substrate can be provided. According to another embodiment of the present disclosure, a method for manufacturing a semiconductor device having excellent strength of a connection portion between an element and a substrate and a semiconductor device can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a cross-sectional view schematically showing a specific example of the shape of the reinforcing material.
[0037] Figure 2 This is a cross-sectional view schematically showing a specific example of the shape of the reinforcing material.
[0038] Figure 3 This is a cross-sectional view schematically showing a specific example of the shape of the reinforcing material.
[0039] Figure 4 This is a cross-sectional view schematically showing a specific example of the shape of the reinforcing material.
[0040] Figure 5 This is a cross-sectional view schematically showing a specific example of the shape of the reinforcing material.
[0041] Figure 6 It is a top view schematically showing a method of forming a reinforcing material of a sample produced in an example.
[0042] Figure 7 The following is a Weibull plot prepared from the thermal shock test results of the samples prepared in the examples.
[0043] Figure 8 Graph showing the relationship between the cross-sectional area and strain amount of the reinforcement material of the simulation model prepared in the example. DETAILED DESCRIPTION
[0044] The following describes in detail the mode for implementing the present invention. However, the present invention is not limited to the following embodiments. In the following embodiments, the constituent elements (including element steps, etc.) are not necessarily required except for the cases specifically indicated. The numerical values and their ranges are also the same and do not limit the present invention.
[0045] In the present disclosure, the term "step" includes not only steps that are independent of other steps, but also steps that cannot be clearly distinguished from other steps as long as the purpose of the step can be achieved.
[0046] In the present disclosure, a numerical range expressed using “to” includes the numerical values described before and after “to” as the minimum value and the maximum value, respectively.
[0047] In the present disclosure, in the numerical range recorded in stages, the upper limit or lower limit recorded in one numerical range can also be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical range recorded in the present disclosure, the upper limit or lower limit of its numerical range can also be replaced by the value shown in the embodiment.
[0048] In the present disclosure, each component may contain a plurality of substances corresponding thereto. When a plurality of substances corresponding to each component are present in the composition, the content rate or content of each component refers to the total content rate or total content of the plurality of substances present in the composition unless otherwise specified.
[0049] In the present disclosure, particles corresponding to each component may include multiple types of particles. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component refers to the value of a mixture of the multiple types of particles present in the composition unless otherwise specified.
[0050] <Simulation method>
[0051] The simulation method disclosed herein comprises the following steps:
[0052] The step of preparing a simulation model of a semiconductor device, the semiconductor device comprising a substrate, an element, a connection portion electrically connecting the substrate and the element, and a reinforcing material disposed around the periphery of the element; and
[0053] A step of calculating the amount of strain of the simulation model with respect to the connection portion.
[0054] In the present disclosure, the “periphery of an element” refers to a portion corresponding to the outline of the element or its vicinity (either or both of the inside and outside of the region corresponding to the element) when the element arranged on the substrate is viewed from directly above.
[0055] In the present disclosure, the "cross-sectional area of the reinforcing material" refers to the area of the cross section obtained by cutting the reinforcing material along the thickness direction of the substrate. When the cross-sectional area of the reinforcing material is not constant, the average value of the cross-sectional areas measured at 5 or more locations is taken as the "cross-sectional area of the reinforcing material".
[0056] While studying the relationship between the strain amount of the connection portion and the cross-sectional area of the reinforcing material, the present inventors found that, although there is a correlation between the two, their nature is a complex situation that cannot be explained by a simple linear function.
[0057] For example, when the cross-sectional area of the reinforcing material is small, the amount of strain on the connection portion tends to decrease as the cross-sectional area increases, and when the cross-sectional area is large, the amount of strain on the connection portion tends to increase as the cross-sectional area increases.
[0058] Therefore, accurately analyzing the relationship between the strain amount of the connection part and the cross-sectional area of the reinforcing material and optimizing the cross-sectional area of the reinforcing material in such a way that the strain amount of the connection part becomes sufficiently small is an effective strategy for ensuring the strength of the connection part between the element constituting the semiconductor device and the substrate.
[0059] In the method disclosed herein, the method for preparing the simulation model of the semiconductor device is not particularly limited. For example, the simulation model can be prepared by performing structural analysis of the target semiconductor device using structural analysis software.
[0060] In the method of the present disclosure, it is preferable to prepare a plurality of simulation models having different cross-sectional areas of the reinforcing material.
[0061] By calculating the strain amount using a plurality of simulation models with different cross-sectional areas of the reinforcement material, the relationship between the cross-sectional area of the reinforcement material and the strain amount can be analyzed with high accuracy. As a result, a semiconductor device can be efficiently obtained in which the cross-sectional area of the reinforcement material is optimized so that the strain amount is sufficiently reduced.
[0062] From the viewpoint of accuracy of the amount of strain at the connection portion calculated by the simulation model, it is preferable that the simulation model be created based on various parameters.
[0063] Examples of the parameters include the physical properties of materials constituting the semiconductor device and the conditions for connecting the substrate and the element.
[0064] Examples of the physical properties of a material constituting a semiconductor device include storage modulus, glass transition temperature (Tg), coefficient of thermal expansion (CTE), Poisson's ratio, and the like.
[0065] Conditions for connecting the substrate and the element include heating temperature, heating time, and the like.
[0066] The simulation method of the present disclosure may further include the step of deriving an approximate curve from the cross-sectional area X of the reinforcement material of the simulation model and the strain amount Y calculated using the simulation model.
[0067] The approximate curve derived from the cross-sectional area X of the reinforcement material of the simulation model and the strain amount Y calculated using the simulation model is used, for example, to determine the cross-sectional area of the reinforcement material disposed in the peripheral portion of the element when manufacturing the semiconductor device. By determining the cross-sectional area X of the reinforcement material so that the strain amount Y represented by the approximate curve becomes equal to or less than a certain value, it is possible to design a semiconductor device in which the cross-sectional area X of the reinforcement material is optimized so that the strain amount is sufficiently reduced.
[0068] As an approximate curve derived from the cross-sectional area X of the reinforcement material of the simulation model and the strain amount Y calculated using the simulation model, an approximate curve of an Nth-order polynomial represented by the following formula (1) can be cited.
[0069] Formula (1) Y = aX N +cX (N-1) +dX (N-2) +…+b
[0070] In the formula, a, b, c and d are arbitrary constants, and N is an integer greater than or equal to 2.
[0071] From the viewpoint of analytical accuracy of the relationship between the cross-sectional area X and the strain amount Y of the reinforcing material, the larger the value of N in the formula (1), the more preferable it is, and for example, 3 or more is preferable.
[0072] The value of N can be adjusted using the numerical value of the simulation model used in deriving the approximate curve.
[0073] <Method for manufacturing semiconductor device>
[0074] In the manufacturing method of a semiconductor device disclosed in the present invention, the semiconductor device comprises a substrate, an element, a connecting portion electrically connecting the substrate and the element, and a reinforcing material arranged at a peripheral portion of the element, and the manufacturing method includes a step of determining a cross-sectional area X of the reinforcing material based on a strain amount Y with respect to the connecting portion.
[0075] The semiconductor device manufactured by the above method has excellent strength in the connection portion between the substrate and the element.
[0076] From the viewpoint of ensuring sufficient strength of the connection portion, the cross-sectional area X of the reinforcing material is preferably determined so as to satisfy the following formula (2).
[0077] Formula (2): X min ×0.7≤X≤X min ×1.3
[0078] Where, X min It is the cross-sectional area of the reinforcing material when the strain Y about the connection part reaches the minimum value.
[0079] In the method for manufacturing a semiconductor device disclosed herein, there is no particular limitation on the method for determining the cross-sectional area X of the reinforcing material based on the amount of strain Y associated with the connection portion. For example, the method may be performed using the simulation method described above or using other methods. As other methods, a method may be cited in which a sample of a target semiconductor device is prepared and the amount of strain associated with the connection portion of the sample is actually measured.
[0080] The method for manufacturing the semiconductor device is not particularly limited and can be selected from common methods.
[0081] For example, the substrate and the element may be electrically connected by heating after the element is arranged on the substrate via a connection portion such as a solder bump, and then a reinforcing material may be arranged around the element. The outer periphery of the element may be further sealed with a sealing material as needed.
[0082] In the semiconductor device manufactured by the method of the present disclosure, the shape of the reinforcing material disposed in the peripheral portion of the element is not particularly limited. Figure 1 to Figure 3 : is a cross-sectional view schematically showing an example of the shape of the reinforcing material. Figure 1 to Figure 3 As shown, a substrate 1 and an element 2 constituting a semiconductor device 10 are electrically connected by a connection portion 4 , and a reinforcing material 3 is disposed around the element 2 .
[0083] The cross-sectional shape of the reinforcement material 3 can be as follows Figure 1 The shape of the surface in contact with the substrate 1, the side of the component 2 and the back side (the side on the substrate side) of the component 2 is shown; Figure 2 The shape of the surface in contact with the substrate and the side of the component as shown; Figure 3 The shape of the surface in contact with the substrate and the back surface of the element 2 is shown.
[0084] The reinforcing material 3 may be disposed on the entire periphery of the element or may be disposed partially. Figure 4 and Figure 5 FIG. 2 is a top view schematically showing a specific example of the location of the reinforcement material. The reinforcement material 3 may be as follows: Figure 4 As shown, they are continuously arranged at the periphery of the element, or as shown Figure 5 The arrangement shown is discontinuous at the periphery of the element.
[0085] The distance between the substrate and the element (when the distance is not constant, it is the distance at the periphery of the element) is not particularly limited and can be selected according to the size and type of the element, etc. For example, it can be selected from the range of 50 μm to 1000 μm.
[0086] The height of the reinforcing material (when the height is not constant, the maximum value of the height) is not particularly limited and can be selected according to the size and type of the semiconductor device, etc. For example, it can be selected from the range of 50 μm to 1000 μm.
[0087] The width of the reinforcing material (when the width is not constant, the maximum value of the width) is not particularly limited and can be selected according to the size and type of the semiconductor device, etc. For example, it can be selected from the range of 50 μm to 1000 μm.
[0088] The types of substrate and element in the semiconductor device are not particularly limited and can be selected according to the purpose of the semiconductor device, etc.
[0089] The type of reinforcement material in the semiconductor device is not particularly limited and can be selected according to the purpose of the semiconductor device. From the viewpoint of mechanical strength, heat resistance, etc., the reinforcement material is preferably a cured product of a curable resin composition. In the present disclosure, a curable resin composition refers to a composition containing at least a curable resin and, if necessary, other components.
[0090] Specific examples of the curable resin contained in the curable resin composition include thermosetting resins such as epoxy resins, phenolic resins, melamine resins, and unsaturated polyester resins, and ultraviolet curable resins such as acrylic resins. Among them, epoxy resins are preferred.
[0091] From the viewpoint of forming a reinforcing material having a desired shape in the peripheral portion of the element, the reinforcing material is preferably a cured product of a curable resin composition that is liquid at a temperature within a range of 25°C to 50°C.
[0092] The curable resin composition which is liquid at a temperature in the range of 25°C to 50°C makes it easy to apply the curable resin composition to a desired area of the periphery of the element. In addition, by curing the curable resin composition after application, a structure in which a cured product of the curable resin composition is arranged at the periphery of the element can be easily formed.
[0093] In the present disclosure, “liquid in the range of 25°C to 50°C” means liquid at any temperature between 25°C and 50°C.
[0094] The viscosity of the curable resin composition at 25° C. to 50° C. is preferably 10 Pa·s or more, more preferably 20 Pa·s or more, and even more preferably 30 Pa·s or more.
[0095] When the viscosity of the curable resin composition at 25° C. to 50° C. is 10 Pa·s or more, the original shape is easily maintained even when the reinforcing material is left to stand without being cured after being applied to a desired portion.
[0096] The viscosity of the curable resin composition at 25° C. is preferably 300 Pa·s or less, more preferably 250 Pa·s or less, and even more preferably 230 Pa·s or less.
[0097] When the viscosity of the curable resin composition at 25° C. is 300 Pa·s or less, the curable resin composition can be applied locally using a device such as a dispenser, screen printer, or inkjet printer, and thus the workability is excellent.
[0098] The viscosity of the curable resin composition at 50° C. is not particularly limited, and may be, for example, 200 Pa·s or less, 180 Pa·s or less, or 150 Pa·s or less.
[0099] The viscosity of the curable resin composition was measured by the method described in Examples.
[0100] The properties of the cured product of the curable resin composition are not particularly limited and can be selected according to the purpose of the structure and the like.
[0101] From the viewpoint of connection reliability, the thermal expansion coefficient (CTE1, CTE in the range below the glass transition temperature) of the cured product of the curable resin composition is preferably 25 ppm / °C or less, more preferably 22 ppm / °C or less, and further preferably 20 ppm / °C or less. In addition, the thermal expansion coefficient (CTE2, CTE in the range above the glass transition temperature) of the cured product of the curable resin composition is preferably 80 ppm / °C or less, more preferably 75 ppm / °C or less, and further preferably 70 ppm / °C or less.
[0102] From the viewpoint of heat resistance, the glass transition temperature (Tg) of the cured product of the curable resin composition is preferably 100° C. or higher, more preferably 120° C. or higher, and even more preferably 140° C. or higher.
[0103] In the present disclosure, CTE1, CTE2, and Tg of a cured product of a curable resin composition are measured by the method described in Examples.
[0104] The temperature at which the curable resin composition is cured (curing temperature) is not particularly limited, but is preferably 200° C. or less, more preferably 170° C. or less, and even more preferably 150° C. or less from the viewpoint of workability. It is also preferably 80° C. or more, more preferably 90° C. or more, and even more preferably 100° C. or more.
[0105] Hereinafter, as an example of the curable resin composition, an epoxy resin composition containing an epoxy resin and a curing agent will be described.
[0106] The types of the epoxy resin and curing agent contained in the epoxy resin composition are not particularly limited and can be selected according to desired physical properties and the like.
[0107] The epoxy resin composition may contain a liquid at 25°C and a solid at 25°C as the epoxy resin and the curing agent. For example, the epoxy resin may contain a liquid at 25°C and a solid at 25°C. By using a liquid at 25°C and a solid at 25°C as the epoxy resin and the curing agent, it is easy to obtain an epoxy resin composition that is liquid in the range of 25°C to 50°C and has a thixotropic index of 1.0 or more in the range of 25°C to 50°C.
[0108] [Epoxy resin]
[0109] The type of epoxy resin contained in the epoxy resin composition is not particularly limited. For example, bisphenol epoxy resin, naphthalene epoxy resin, glycidylamine epoxy resin, hydrogenated bisphenol epoxy resin, alicyclic epoxy resin, alcohol ether epoxy resin, cycloaliphatic epoxy resin, fluorene epoxy resin, and siloxane epoxy resin can be mentioned. The epoxy resin can be used alone or in combination of two or more.
[0110] Among the above-mentioned epoxy resins, bisphenol-type epoxy resins and glycidylamine-type epoxy resins are preferred from the viewpoint of the balance of properties of the epoxy resin composition.
[0111] Specific examples of the bisphenol epoxy resin include bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol AD epoxy resin, etc. Among them, bisphenol epoxy resins that are liquid at 25°C are preferred, and bisphenol F epoxy resins that are liquid at 25°C are more preferred.
[0112] As a commercial product of the bisphenol F type epoxy resin which is liquid at 25 degreeC, "Epotohto YDF-8170C" of Nippon Steel & Sumitomo Metal Chemical Corporation is mentioned.
[0113] When the epoxy resin composition contains a bisphenol epoxy resin, the proportion of the bisphenol epoxy resin in the total epoxy resin is not particularly limited and can be selected according to the desired properties of the epoxy resin composition. For example, it can be 30% to 100% by mass, 40% to 90% by mass, or 50% to 70% by mass of the total epoxy resin.
[0114] Specific examples of the glycidylamine epoxy resin include diglycidylamine epoxy resins, trifunctional or higher-functional glycidylamine epoxy resins, etc. Among them, glycidylamine epoxy resins that are liquid at 25°C are preferred, and glycidylamine epoxy resins that are liquid at 25°C or higher-functional glycidylamine epoxy resins are more preferred.
[0115] Examples of the glycidylamine epoxy resin that is liquid at 25° C. include triglycidyl-p-aminophenol. Examples of commercially available triglycidyl-p-aminophenol include “jER-630” and “jER-630LSD” from Mitsubishi Chemical Co., Ltd. and “EP-3950S” from ADEKA Corporation.
[0116] When the epoxy resin composition contains a glycidylamine type epoxy resin, the proportion of the glycidylamine type epoxy resin in the entire epoxy resin is not particularly limited and can be selected according to the desired properties of the reinforcement material. For example, it can be 10% to 100% by mass, 20% to 70% by mass, or 30% to 50% by mass of the entire epoxy resin.
[0117] [Curing agent]
[0118] The type of curing agent contained in the epoxy resin composition is not particularly limited. For example, amine curing agents, phenol curing agents, acid anhydride curing agents, polythiol curing agents, polyaminoamide curing agents, isocyanate curing agents, blocked isocyanate curing agents, etc. can be mentioned. The curing agent can be used alone or in combination of two or more.
[0119] Among the above-mentioned epoxy resins, amine curing agents are preferred from the viewpoint of the balance of characteristics of the epoxy resin composition.
[0120] Examples of the amine curing agent include aliphatic amine compounds such as diethylenetriamine, triethylenetetramine, n-propylamine, 2-hydroxyethylaminopropylamine, cyclohexylamine, and 4,4'-diamino-dicyclohexylmethane; aromatic amine compounds such as diethyltoluenediamine, 3,3'-diethyl-4,4'-diaminodiphenylmethane, and 2-methylaniline; imidazole compounds such as imidazole, 2-methylimidazole, 2-ethylimidazole, and 2-isopropylimidazole; and imidazoline compounds such as imidazoline, 2-methylimidazoline, and 2-ethylimidazoline.
[0121] The curing agent contained in the epoxy resin composition may be liquid at 25° C. or solid at 25° C. From the viewpoint of the balance between ease of application using a dispenser, screen printer, inkjet printer, etc. and shape retention, it is preferred to use a curing agent that is solid at 25° C., and more preferably an amine curing agent that is solid at 25° C.
[0122] Examples of the amine curing agent that is solid at 25° C. include the above-mentioned aliphatic amine compounds. Examples of commercially available products of the amine curing agent that is solid at 25° C. include “Fujicure FXR-1020”, “Fujicure FXR-1030”, “Fujicure FXR-1081” and “Fujicure FXR-1121” from T&KTOKA Corporation.
[0123] The mixing ratio of the epoxy resin and the curing agent contained in the epoxy resin composition is preferably set so that the ratio of the number of functional groups (active hydrogen in the case of an amine curing agent) of the curing agent to the number of epoxy groups of the epoxy resin (the number of functional groups of the curing agent / the number of epoxy groups of the epoxy resin) is within the range of 0.5 to 2.0, more preferably within the range of 0.6 to 1.3, and even more preferably within the range of 0.8 to 1.2, from the perspective of suppressing the respective unreacted components to a small amount.
[0124] [Inorganic fillers]
[0125] The epoxy resin composition may further contain an inorganic filler. By containing an inorganic filler, the thermal expansion coefficient of the cured product of the epoxy resin composition can be reduced, the thermal conductivity can be improved, and the like.
[0126] Specific examples of the inorganic filler include silicon dioxide, aluminum oxide, calcium carbonate, zirconium silicate, calcium silicate, silicon nitride, aluminum nitride, boron nitride, beryllium oxide, zirconium oxide, zircon, forsterite, steatite, spinel, mullite, titanium oxide, talc, clay, and mica.
[0127] Among the above inorganic fillers, silicon dioxide is preferred from the viewpoint of reducing the thermal expansion coefficient, and aluminum oxide is preferred from the viewpoint of improving the thermal conductivity. The inorganic filler may be used alone or in combination of two or more.
[0128] The content of the inorganic filler contained in the epoxy resin composition is not particularly limited. From the viewpoint of reducing the thermal expansion coefficient of the cured product and improving the thermal conductivity, the content of the inorganic filler is preferably 40% by mass or more of the epoxy resin composition as a whole, more preferably 50% by mass or more, and further preferably 60% by mass or more. From the viewpoint of suppressing the viscosity increase of the epoxy resin composition, the content of the inorganic filler is preferably 90% by mass or less of the reinforcement material as a whole, more preferably 80% by mass or less, and further preferably 75% by mass or less.
[0129] When the inorganic filler is in the form of particles, the average particle size is not particularly limited. For example, the volume average particle size is preferably 0.05 μm to 20 μm, and more preferably 0.1 μm to 15 μm. When the volume average particle size is 0.05 μm or more, there is a tendency to further suppress the viscosity increase of the reinforcing material. When the volume average particle size is 20 μm or less, there is a tendency to further improve the imparting property to narrow gaps.
[0130] The volume average particle size of the inorganic filler refers to the particle size (D50) at which the volume accumulation from the smaller diameter side in the volume-based particle size distribution obtained by a laser scattering diffraction particle size distribution analyzer reaches 50%.
[0131] [Various additives]
[0132] The epoxy resin composition may contain various additives such as a thixotropy imparting agent, a curing accelerator, a stress relaxation agent, a coupling agent, and a coloring agent in addition to the above-mentioned components.
[0133] When the epoxy resin composition contains components other than the epoxy resin, the curing agent, and the inorganic filler, the total content thereof is preferably 10% by mass or less, more preferably 5% by mass or less, based on the entire epoxy resin composition.
[0134] <Semiconductor Device>
[0135] The semiconductor device disclosed herein includes a substrate, an element, a connection portion electrically connecting the substrate and the element, and a reinforcing material disposed around the element, wherein a cross-sectional area X of the reinforcing material satisfies the following formula (2).
[0136] Formula (2): X min ×0.7≤X≤X min ×1.3
[0137] Where, X minIt is the cross-sectional area of the reinforcing material when the strain Y about the connection part reaches the minimum value.
[0138] The semiconductor device of the present disclosure has excellent strength in the connection portion between the substrate and the element.
[0139] The details and preferred embodiments of the components included in the semiconductor device of the present disclosure are the same as the details and preferred embodiments of the semiconductor device manufactured by the above-mentioned method for manufacturing a semiconductor device.
[0140] Example
[0141] Hereinafter, the present disclosure will be specifically described using examples, but the scope of the present disclosure is not limited to these examples.
[0142] (Structural Analysis of Semiconductor Devices)
[0143] Structural analysis software (Marc2021, manufactured by MSC Software Co., Ltd.) was used to perform structural analysis of semiconductor devices used in reliability tests. Specifically, each side of the semiconductor device was divided into four equal regions, and one of the regions was used as the object of structural analysis. Furthermore, five simulation models were made in which the cross-sectional area X of the reinforcement material was changed to the value shown in Table 1. The element class is a hexahedron with 8 nodes. In order to shorten the calculation time, scaling analysis was used in the analysis.
[0144] First, a global model is created using rough elements, and calculations are performed on a computer using structural analysis software. Based on the calculation results, the part of the semiconductor device where the strain amount related to the connection part reaches the maximum is used as a local model, and a simulation model is created using more detailed elements.
[0145] Next, the displacements in the X, Y, and Z directions obtained from the calculation results of the Global Model were input into the Local Model, and the calculation was performed using a computer to output the maximum total equivalent plastic strain of the connection. The results are shown in Table 1.
[0146] Table 1
[0147]
[0148] (Input items in simulation model)
[0149] The storage modulus, thermal expansion coefficient (CTE), glass transition temperature (Tg), and Poisson's ratio of each material shown in Table 2 were input into the prepared simulation model. Si and Cu are elastomers, solder is an elastoplastic body, and other materials are viscoelastic bodies in consideration of relaxation characteristics. As the yield stress of the solder, a value of 29 MPa was input at -40°C and a value of 12.6 MPa was input at 130°C.
[0150] As temperature conditions, the initial temperature was 220°C, which is the temperature at which the solder melts, then the temperature was lowered to room temperature (20°C), then the temperature was raised to 125°C and held for 13 minutes, then the temperature was lowered to -55°C and held for 13 minutes. The above steps were regarded as one cycle, and the operation was repeated 11 times (the 11th cycle was completed at the time point of raising the temperature to 125°C and holding for 13 minutes). The time for heating and cooling was 2 minutes.
[0151] Table 2
[0152]
[0153] (Preparation of resin composition)
[0154] The materials shown in Table 3 were mixed to prepare a resin composition. The details of each material are as follows. The mixing ratio of the epoxy resin and the curing agent was set in such a way that the number of epoxy groups of the epoxy resin and the number of active hydrogens of the curing agent were equal. The physical properties of the prepared resin composition or its cured product were prepared by the method shown below. The results are shown in Table 3.
[0155]
[0156] (Viscosity measurement)
[0157] The viscosity of the resin composition at 10 rpm (revolutions / minute) was measured under a temperature condition of 25° C. using a dynamic viscoelasticity measuring apparatus (AR-2000, manufactured by TA Instruments).
[0158] (Determination of CTE1, CTE2 and Tg)
[0159] The resin composition was cured at 120° C. for 15 minutes to obtain a cured product. The cured product was cut into a size of 8 mm in diameter and 20 mm in length to prepare a measurement sample.
[0160] The length change (linear expansion coefficient) of the measurement sample when the temperature was increased from 0°C to 240°C at 5°C / min was measured by a compression method using a thermomechanical analyzer (TMA2940, manufactured by TA Instruments). The average value of the linear expansion coefficient in the measurement temperature range of 10°C to 30°C was taken as CTE1, and the average value of the linear expansion coefficient in the measurement temperature range of 180°C to 200°C was taken as CTE2. In addition, the temperature corresponding to the intersection of the tangent lines at 100°C and 200°C was taken as the glass transition temperature (Tg).
[0161] (Determination of storage modulus)
[0162] The resin composition was cured at 120° C. for 15 minutes to obtain a cured product. The cured product was cut into a size of 60 mm×10 mm and a thickness of 2 mm to prepare a measurement sample.
[0163] The storage modulus of the measurement sample was measured using a thermomechanical analyzer (Q800, manufactured by TA Instruments) in a dual cantilever beam mode at a temperature increase of 3° C. / min from 0° C. to 260° C. at a frequency of 1 Hz.
[0164] Table 3
[0165]
[0166] (Manufacturing of semiconductor devices)
[0167] A semiconductor device for evaluation was produced using the prepared resin composition, substrate, and element.
[0168] As a substrate, WALTS-KIT (WLP(S)300P / 400P-2, 30 mm×30 mm, thickness: 978 μm) manufactured by Walts Corporation was used.
[0169] As the element, WLP TEG M2 (0.4 mm pitch BGA, 6 mm×6 mm, thickness 725 μm) manufactured by Walts Corporation was used.
[0170] Flux (SPARKLE FLUX WF-6400 manufactured by Senju Metal Industry Co., Ltd.) was applied to the solder bumps of the components. Then, a flip chip bonding machine (FC3000W manufactured by Toray) was used to temporarily mount the components on the substrate at 25°C in such a way that the center of the substrate and the center of the components were aligned. Then, a reflow device (SNR-1065GT manufactured by Senju Metal Industry Co., Ltd.) was used to perform a reflow treatment at a maximum temperature of 260°C. Then, a flux washer (YWV-4635S manufactured by Sakura Seiki Co., Ltd.) was used to remove the flux at a water temperature of 80°C to obtain a structure in which the substrate and the components were bonded via solder.
[0171] The resin composition (25° C.) was applied to the periphery of the element arranged on the substrate using a dispenser (FAD2500 manufactured by Musashi Engineering Co., Ltd.) and a nozzle (TNPD-22G manufactured by Musashi Engineering Co., Ltd.).
[0172] The region to which the resin composition was applied was a region having a width of 1.25 mm at the periphery of the device (sample A) and a region having a width of 1.88 mm at the periphery of the device (sample B), and three samples of each were prepared.
[0173] The pressure of the dispenser was 400 kPa, and the speed was 5 mm / s (sample A) and 2.5 mm / s (sample B).
[0174] The nozzle position is as follows Figure 6 As shown, the height difference a between the upper portion of the element 2 and the front end of the nozzle 5 is set to 300 μm, and the distance b between the center of the nozzle 5 and the end of the element 2 is set to 500 μm.
[0175] After the dispensing was completed, a heat treatment was performed at 120° C. for 15 minutes to cure the resin composition and form a reinforcing material on the outer periphery of the element.
[0176] (Evaluation of connection reliability)
[0177] The connection reliability of the produced semiconductor samples A and B was evaluated by the following method using a thermal shock tester (NT2031W, manufactured by Kusumoto Chemicals Co., Ltd.).
[0178] Before the test, the initial resistance value (R0) of the periphery of the element of each sample was measured. Then, a thermal shock test device was used to maintain the temperature at -55°C and 125°C for 15 minutes, and the process was repeated (100 cycles). After the test, the resistance value (Ri) of the periphery of the element of the sample was measured. If the Ri value based on R0 is less than a 20% increase rate, the same test is performed on the sample again, and the test is terminated when the Ri increase rate reaches more than 20%.
[0179] Weibull plots were prepared from the results of thermal shock tests ( Figure 7 The number of cycles until 20% cumulative failure was calculated. The results are shown in Table 4. The values shown in Table 4 are the average values of the samples (n==3).
[0180] Table 4
[0181] Sample A Sample B Width of reinforcement material (mm) 1.25 1.88 <![CDATA[Cross-sectional area of the reinforcement material (mm 2 )]]> 0.62 1.04 Cycles at 20% cumulative failures (number of cycles) 3104 1683
[0182] (Verification of simulation results)
[0183] A scatter plot was made from the cross-sectional area X of the reinforcement material of the simulation model shown in Table 1 and the strain Y calculated by the simulation model, and an approximate curve was derived. Figure 8 middle.
[0184] like Figure 8As shown, the following tendency was confirmed: when the cross-sectional area of the reinforcement material of the simulation model was small, the strain amount on the connection portion decreased as the cross-sectional area increased, while when the cross-sectional area value was large, the strain amount on the connection portion increased as the cross-sectional area increased.
[0185] and then, Figure 8 The tendency shown is consistent with the evaluation results of the connection reliability of actually manufactured semiconductor devices.
Claims
1. A simulation method comprising the following steps: The step of preparing a simulation model of a semiconductor device, the semiconductor device comprising a substrate, an element, a connection portion electrically connecting the substrate and the element, and a reinforcing material disposed around the periphery of the element; and A step of calculating the amount of strain of the simulation model with respect to the connection portion.
2. The simulation method according to claim 1, further comprising the step of deriving an approximate curve of an Nth-order polynomial represented by the following formula (1) from the strain amount Y calculated using the simulation model and the corresponding cross-sectional area X of the reinforcement material, Equation (1) Y = aX N + cX (N-1) + dX (N-2) + … + b In the formula, a, b, c and d are arbitrary constants, and N is an integer greater than or equal to 2.
3. The simulation method according to claim 1 or 2, wherein: The simulation model was made using structure analysis software.
4. A method for manufacturing a semiconductor device, the semiconductor device comprising a substrate, a semiconductor device, a connection portion for electrically connecting the substrate and the semiconductor device, and a reinforcing material arranged at a peripheral portion of the semiconductor device, The manufacturing method includes the step of determining a cross-sectional area X of the reinforcing material according to a strain amount Y with respect to the connecting portion.
5. The method for manufacturing a semiconductor device according to claim 4, wherein: The cross-sectional area X of the reinforcement material satisfies the following formula (2): Formula (2): X min ×0.7≤X≤X min ×1.3 Where, X min It is the cross-sectional area of the reinforcing material when the strain Y about the connection part reaches the minimum value.
6. The method for manufacturing a semiconductor device according to claim 4, wherein: The strain amount Y of the connection portion is calculated using a simulation model.
7. The method for manufacturing a semiconductor device according to claim 4, wherein: The reinforcing material is a cured product of a curable resin composition.
8. The method for manufacturing a semiconductor device according to claim 7, wherein: The curable resin composition includes an epoxy resin.
9. The method for manufacturing a semiconductor device according to claim 5, wherein: The reinforcing material has a glass transition temperature Tg of 100°C or higher, a thermal expansion coefficient CTE1 of 25 ppm / °C or lower in a temperature range below the glass transition temperature, and a thermal expansion coefficient CTE2 of 80 ppm / °C or lower in a temperature range above the glass transition temperature.
10. A semiconductor device comprising a substrate, an element, a connection portion electrically connecting the substrate and the element, and a reinforcing material disposed around the periphery of the element, in, The cross-sectional area X of the reinforcement material satisfies the following formula (2): Formula (2): X min ×0.7≤X≤X min ×1.3 In the formula, X min It is the cross-sectional area of the reinforcing material when the strain Y about the connection part reaches the minimum value.
11. The semiconductor device according to claim 10, wherein The reinforcing material is a cured product of a curable resin composition.
12. The semiconductor device according to claim 10, wherein: The curable resin composition includes an epoxy resin.
13. The semiconductor device according to claim 10, wherein: The reinforcing material has a glass transition temperature Tg of 100°C or higher, a thermal expansion coefficient CTE1 of 25 ppm / °C or lower in a temperature range below the glass transition temperature, and a thermal expansion coefficient CTE2 of 80 ppm / °C or lower in a temperature range above the glass transition temperature.
Citation Information
Patent Citations
Underfill material, semiconductor package and method for producing semiconductor package
JP2019011409A