Sintering aid for solid electrolyte for all-solid-state battery and solid electrolyte containing same

By using sintering aids of Li, Te and Zr in oxide solid electrolytes, the problems of increased cost and low conductivity caused by high-temperature sintering are solved, and low-temperature sintering and high-conductivity solid electrolytes are achieved, which improves the battery Security and performance.

CN119096388APending Publication Date: 2024-12-06BASS PUBLIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380017078.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-15
Filing Date
2023-05-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing oxide-based solid electrolytes require high-temperature sintering, which leads to increased manufacturing costs and safety risks, and the ionic conductivity of polymer electrolytes is low.

Method used

An oxide sintering aid containing Li, Te and Zr is used to reduce the sintering temperature and increase the ionic conductivity through the combination of Li2O, TeO2 and ZrO2 to form a solid electrolyte with a sodium superion conductor-type crystal structure.

Benefits of technology

A solid electrolyte with excellent ionic conductivity at room temperature is realized, which reduces the sintering temperature, reduces the manufacturing cost, and improves the thermal stability and water resistance of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096388A_ABST
    Figure CN119096388A_ABST
Patent Text Reader

Abstract

The invention relates to a sintering aid of a solid electrolyte for an all-solid-state battery and the solid electrolyte containing the sintering aid. A solid electrolyte for an all-solid-state battery according to one embodiment of the present invention comprises a solid electrolyte having a sodium superoxide conductor type crystal structure and a sintering aid, wherein the sintering aid is formed from an oxide containing Li, Te, and Zr.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a sintering aid of a solid electrolyte for an all-solid-state battery and a solid electrolyte containing the same. Background Art

[0002] In recent years, the use of secondary batteries has been increasing significantly in various fields, from IT equipment such as mobile phones to electric vehicles and energy storage devices.

[0003] As a secondary battery, lithium-ion batteries using liquid electrolytes are the most widely used. However, when an external impact is applied to the battery, there is a risk that the liquid electrolyte will leak, so additional parts and devices are required to ensure safety.

[0004] In recent years, in order to improve the safety of secondary batteries, the development of all-solid-state batteries using solid electrolytes as electrolytes has been actively carried out. As solid electrolytes for all-solid-state batteries, there are polymer electrolytes, oxide electrolytes, sulfide electrolytes, etc. Among them, sulfide solid electrolytes have the highest ion conductivity, but there is a problem of reacting with water to produce hydrogen sulfide gas. Polymer electrolytes have the advantages of relatively simple processes and the ability to use existing lithium-ion battery processes, but have the disadvantage of significantly low ion conductivity.

[0005] Although the ionic conductivity of oxide electrolytes is lower than that of sulfide electrolytes, it is relatively high and has the advantage of excellent safety. However, oxide electrolytes generally require high sintering temperatures of 1,000°C or more, which may significantly increase manufacturing costs. Summary of the invention

[0006] The present invention is intended to solve the above-mentioned problems of the prior art, and its object is to provide a sintering aid that can sinter an oxide-based electrolyte at a low temperature and has excellent ion conductivity, and a solid electrolyte containing the same.

[0007] A solid electrolyte for an all-solid-state battery according to an embodiment of the present invention includes a solid electrolyte having a sodium superion conductor type crystal structure and a sintering aid, wherein the sintering aid is formed of an oxide including Li, Te, and Zr.

[0008] According to an embodiment of the present invention, the sintering aid may be made of Li2CO3, TeO2 and ZrO2.

[0009] According to an embodiment of the present invention, the sintering aid may include 24-30 mol% Li2O, 67-75 mol% TeO2 and 1-4 mol% ZrO2.

[0010] The ionic conductivity of the solid electrolyte for all-solid-state batteries according to one embodiment of the present invention at room temperature can be 2.01×10-7 to about 1.02×10 -5 S / cm.

[0011] According to one embodiment of the present invention, the solid electrolyte with a sodium superion conductor type crystal structure may be a LAGP solid electrolyte or a LATP solid electrolyte.

[0012] Furthermore, the solid electrolyte and sintering aid for an all-solid-state battery according to the present invention may include other additional configurations within the scope that does not impair the technical concept of the present invention.

[0013] Effects of the Invention

[0014] According to an embodiment of the present invention, a sintering aid including Li, Te and Zr can be used to perform low-temperature sintering of a solid electrolyte, and the solid electrolyte including such a sintering aid can have excellent ion conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a diagram schematically showing a cross section of an all-solid-state battery.

[0016] In the figure: 10 - all-solid-state battery, 11 - anode, 12 - cathode, 13 - solid electrolyte layer. DETAILED DESCRIPTION

[0017] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings to the extent that a person having ordinary knowledge in the technical field to which the present invention belongs can easily implement them.

[0018] In order to clearly describe the present invention, the description of the parts not related to the present invention is omitted, and the same reference symbols are marked on the same components throughout the specification. It should be understood that the specific shapes, structures and characteristics recorded in the specification can be changed from one embodiment to other embodiments without departing from the concept and scope of the present invention, and the position or configuration of individual components can also be changed without departing from the concept and scope of the present invention.

[0019] Therefore, the following detailed description is not to be interpreted in a limiting sense, but the scope of the present invention should be understood as including the scope of the claims and all equivalent scopes thereof.

[0020] Figure 1 This is a diagram schematically showing a cross section of an all-solid-state battery.

[0021] refer to Figure 1The all-solid-state battery (10) comprises an anode (11), a cathode (12) and a solid electrolyte layer (13). The solid electrolyte layer (13) is arranged between the anode (11) and the cathode (12) and can be in contact with the anode (11) and the cathode (12) respectively. The anode (11) and the cathode (12) can have an anode active material layer and a cathode active material layer respectively, and the anode active material layer and the cathode active material layer can be in contact with the solid electrolyte layer (13) respectively.

[0022] The anode (11) and the cathode (12) can be bonded to the solid electrolyte layer (13) by sintering. That is, the anode (11), the cathode (12) and the solid electrolyte layer (13) can be sintered to form a whole.

[0023] exist Figure 1 In the figure, the all-solid-state battery (10) is shown as including an anode (11), a cathode (12) and a solid electrolyte layer (13) each having one layer, but the present invention is not limited thereto, and the all-solid-state battery may be formed in a form in which the anode, cathode and solid electrolyte layer are each formed of a plurality of layers. Alternatively, the so-called stacked all-solid-state battery may be formed in a form in which a plurality of anodes, cathodes and solid electrolyte layers are alternately stacked.

[0024] The solid electrolyte layer (13) according to one embodiment of the present invention includes an oxide electrolyte as a solid electrolyte. In one embodiment, the solid electrolyte may include an oxide having a sodium superion conductor (Nasicon) crystal structure. In one embodiment, the oxide having a sodium superion conductor crystal structure may be LAGP (Li 1+x Al x Ge 2-x (PO4)3) or LATP(Li 1+x Al x Ti 2-x (PO4)3).

[0025] The solid electrolyte contained in the solid electrolyte layer (13) according to one embodiment of the present invention further contains a sintering aid.

[0026] Oxide electrolytes of a sodium superion conductor crystal structure are generally sintered at a high temperature of 1,000° C. or higher. In this case, as described above, although a certain degree of excellent ion conductivity can be obtained, an increase in manufacturing cost due to high-temperature sintering is inevitable.

[0027] In one embodiment of the present invention, by adding a sintering aid to an oxide-based electrolyte having a sodium super ion conductor type crystal structure, the sintering temperature can be significantly reduced and excellent ion conductivity can be ensured.

[0028] The sintering aid according to one embodiment of the present invention may be formed of an oxide including Li, Te, and Zr. For example, the sintering aid according to one embodiment of the present invention may include Li2O, TeO2, and ZrO2.

[0029] Among the oxides forming the sintering aid, Li2O can function as a network modifier and can also provide Li ions, thereby improving ion conductivity.

[0030] Among the oxides forming the sintering aid, TeO2 can function as a network former. Furthermore, TeO2 can lower the sintering temperature. Furthermore, TeO2 can improve thermal stability, IR transmittance and dielectric constant.

[0031] Among the oxides forming the sintering aid, ZrO2 can function as a nucleating agent. ZrO2 can improve the transition density and viscosity. In addition, ZrO2 can increase the transition temperature but reduce the thermal expansion coefficient.

[0032] Thus, the sintering aid according to one embodiment of the present invention can reduce the sintering temperature and improve the ion conductivity by including Li2O, TeO2 and ZrO2.

[0033] The sintering temperature of the sintering aid according to one embodiment of the present invention is about 400° C. to about 500° C.

[0034] The solid electrolyte according to one embodiment of the present invention may contain 95% by mass or more of an oxide electrolyte having a sodium super ion conductor crystal structure and 5% by mass or less of a sintering aid. When the solid electrolyte according to one embodiment of the present invention is sintered at 400°C to 500°C, the ionic conductivity measured at room temperature is about 2.01×10 -7 to about 1.02×10 -5 S / cm.

[0035] Hereinafter, the present invention will be described in more detail with reference to specific embodiments and test examples of the present invention.

[0036] [Example]

[0037] Example 1

[0038] The precursor powder for manufacturing the sintering aid was prepared by mixing Li2CO3 24 mol%, TeO2 75 mol% and ZrO2 1 mol%. After the precursor powder was mixed, it was put into a furnace and melted at a temperature of about 1,000°C for about 1 hour. Thereafter, the homogenized melt was poured onto a quenching roller and cooled to room temperature, crushed, and sieved to obtain a sintering aid in the form of cullet with a size of less than 200 μm.

[0039] Additional Examples and Comparative Examples

[0040] Precursor powders were prepared by setting the composition ratios of Li2CO3, TeO2 and ZrO2 differently, and then, a sintering aid in the form of cullet was obtained through the same process as in Example 1.

[0041] Table 1 shows the composition ratios of the sintering aids in the above-described Examples and Comparative Examples.

[0042] [Table 1]

[0043]

[0044] The transition temperature and crystallization temperature of the sintering aids according to the examples and comparative examples prepared as described above were confirmed by thermal analysis. The transition temperature and crystallization temperature of the sintering aids according to the examples and comparative examples are shown in Table 2.

[0045] [Table 2]

[0046]

[0047]

[0048] Referring to Table 2, it is confirmed that the solid electrolyte manufactured by including the sintering aid based on Examples 1 to 5 of the present invention has a transition temperature below 316°C and a crystallization temperature below 432°C. In contrast, the solid electrolyte manufactured by including the sintering aid based on Comparative Examples 1 to 5 has a transition temperature of above 320°C and a crystallization temperature of above 440°C, showing a relatively higher temperature than Examples 1 to 5. In this way, the sintering aids based on the embodiments and comparative examples of the present invention have low-temperature characteristics, and thus can contribute to the low-temperature characteristics of the solid electrolyte containing them. In particular, the sintering aids based on Examples 1 to 5 have relatively lower sintering temperatures and crystallization temperatures, so the solid electrolyte manufactured by including them can further reduce the sintering temperature.

[0049] The sintering aids of the above-mentioned examples and comparative examples were mixed with LAGP and sintered to produce a solid electrolyte. Specifically, about 3 mass % of the sintering aids of each example and comparative example were mixed with Li 1.5 Al 0.5 Ge 1.5 About 97 mass % of (PO4)3 was mixed and sintered at 400°C to 500°C for about 6 hours to produce a solid electrolyte.

[0050] In addition, the ion conductivity of the solid electrolytes produced by the above-produced examples and comparative examples including the sintering aid was measured by impedance analysis. The ion conductivity of the solid electrolytes according to the examples and comparative examples is shown in Table 3.

[0051] [Table 3]

[0052]

[0053] With reference to Table 3, it is confirmed that the solid electrolytes manufactured by including the sintering aids according to Examples 1 to 5 of the present invention have relatively excellent ionic conductivity. In particular, it is confirmed that the solid electrolyte manufactured by including the sintering aid according to Example 2 of the present invention (i.e., a sintering aid including Li2O, TeO2, and ZrO2 in a molar ratio of 25:72:3) has a relative excellent ionic conductivity of 1.02×10 -5 S / cm. Thus, it can be confirmed that when the sintering aid containing Li2O, TeO2 and ZrO2 has a specific composition ratio, it can greatly contribute to the improvement of the ionic conductivity of the solid electrolyte.

[0054] On the other hand, a water resistance test evaluation of a solid electrolyte including a sintering aid according to an embodiment of the present invention was performed, and as a result, it was confirmed that it had excellent water resistance. Specifically, a water immersion test in distilled water for 72 hours was performed, and as a result, it was confirmed that the color of the distilled water did not change and the stability of the material was maintained.

[0055] The sintering aid according to this embodiment and the solid electrolyte including the same have such water resistance, so that even if water flows into the all-solid-state battery, the performance of the battery will not be reduced, and stable and excellent performance can be maintained.

[0056] The present invention has been described above using specific matters such as specific constituent elements and limited embodiments, but the above embodiments are only provided to help a more comprehensive understanding of the present invention, and the present invention is not limited thereto. Anyone with ordinary skills in the technical field to which the present invention belongs can make various modifications and deformations from such descriptions.

[0057] Therefore, the concept of the present invention should not be limited to the embodiments described above, and all scopes equivalent to or equivalent to the claims should fall within the scope of the concept of the present invention.

Claims

1. A solid electrolyte for an all-solid-state battery, comprising a solid electrolyte having a sodium superion conductor crystal structure and a sintering aid, The sintering aid is formed of an oxide including Li, Te, and Zr.

2. The solid electrolyte for all-solid-state batteries according to claim 1, wherein The sintering aid is made of Li2CO3, TeO2 and ZrO2.

3. The solid electrolyte for all-solid-state batteries according to claim 1, wherein The sintering aid comprises 24-30 mol% of Li2O, 67-75 mol% of TeO2 and 1-4 mol% of ZrO2.

4. The solid electrolyte for all-solid-state batteries according to claim 1, wherein The ionic conductivity at room temperature is 2.01×10 -7 to about 1.02×10 -5 S / cm.

5. The solid electrolyte for all-solid-state battery according to claim 1, wherein The solid electrolyte with a sodium superion conductor type crystal structure is a LAGP solid electrolyte or a LATP solid electrolyte.

6. A sintering aid for a solid electrolyte for an all-solid-state battery, which is formed from an oxide containing Li, Te and Zr.

7. The sintering aid according to claim 6, which is made of Li2CO3, TeO2 and ZrO2.

8. The sintering aid according to claim 6, comprising 24-30 mol% of Li2O, 67-75 mol% of TeO2 and 1-4 mol% of ZrO2.