Method for recovering copper from bismuth concentrate
By adopting flotation method and efficient environmentally friendly bismuth inhibitor system in bismuth concentrate, the problem of difficulty in separation of copper and bismuth in bismuth concentrate and environmental pollution is solved, and efficient recycling and sorting of copper in bismuth concentrate is achieved, improving the Copper-bismuth separation efficiency and process adaptability.
Patent Information
- Application Number
- CN202411189276.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-17
- Estimated Expiration
- 2044-08-28
AI Technical Summary
In the prior art, there are problems such as high flotation separation, environmental pollution and high equipment investment in the copper-bismuth separation process in bismuth concentrate. In particular, the adaptability of copper-bismuth mixed concentrate with low copper-bismuth high copper is insufficient, making it difficult to achieve efficient and environmental protection. Copper recycling.
Pre-de-drug and desludge were performed by flotation method, combining strong alkali and high-efficiency environmentally friendly bismuth inhibitor CD-B1, through the "coarse selection tail-selected strengthened sorting" process, using activated carbon and ethylthioamide + F6 Combining the pharmaceutical system to achieve efficient sorting and recycling of copper.
The efficiency of copper-bismuth separation and flotation is significantly improved, the separation difficulty is reduced, the copper recovery rate and process adaptability are improved, and the effective sorting and recycling of medium and low-grade copper in bismuth concentrate is achieved, and the process flow is simplified and environmentally friendly.
Smart Images

Figure CN119140264A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ore dressing, and in particular to a method for recovering copper from bismuth concentrate. Background Art
[0002] Bismuth polymetallic ore with copper content less than 0.1% in the original ore is an important associated copper resource. At present, the main mineral processing technology basically adopts the method of "sulfide ore mixed flotation-multi-metal cascade separation flotation", and copper metal is mostly enriched in bismuth concentrate (containing 2% to 3% copper). Since copper minerals (mainly chalcopyrite) and bismuth minerals (mainly bismuthinite) have good natural floatability, their flotation separation is difficult. The technical solutions are mainly divided into "copper suppression and bismuth floating" and "bismuth suppression and copper floating"; the former usually requires the addition of cyanide, which is seriously harmful to the environment and has been gradually eliminated; the latter, as the most important copper-bismuth separation method, mainly focuses on the development of efficient and environmentally friendly bismuth inhibitors, and needs to be further improved in terms of copper-bismuth separation effect and technical indicator stability.
[0003] There are certain differences in specific gravity and specific magnetic susceptibility between copper minerals and bismuth minerals. In theory, gravity separation or strong magnetic separation can be used to separate copper and bismuth. However, most copper and bismuth minerals in the -0.037mm particle size are difficult to separate well through gravity separation in practical applications. The copper and bismuth concentrate products separated by strong magnetic separation are prone to exceed the standard, the quality of copper concentrate is poor, and the investment in strong magnetic separation equipment is large.
[0004] The patent with publication number CN106238202A discloses a copper-bismuth mixed concentrate ultrasonic dispersion-magnetic separation process, which uses the "ultrasonic dispersion-magnetic separation" method to achieve good results, but there are problems such as complex procedures and ultrasonic pollution of the environment, and it is mainly suitable for copper-bismuth mixed concentrate raw materials with "high copper and low bismuth", and its adaptability to "low copper and high bismuth" bismuth-copper mixed concentrate raw materials is not clear. Therefore, it is necessary to develop a more efficient beneficiation process and a more economical and environmentally friendly bismuth inhibitor and reagent system for copper-containing bismuth concentrate, so as to significantly improve the recovery effect of low-grade copper resources associated with bismuth polymetallic ores.
[0005] In view of this, it is necessary to design an improved method for recovering copper from bismuth concentrate to solve the above problems. Summary of the invention
[0006] In view of the defects of the above-mentioned prior art, the purpose of the present invention is to provide a method for recovering copper from bismuth concentrate. Based on the difference in floatability of copper and bismuth minerals, the residual reagents of the front-end flotation operation are utilized to carry out pre-flotation desludging (drugs), improve the flotation environment of the subsequent "bismuth suppression and copper flotation" operation, and reduce the separation difficulty. The "roughing and tailing-fine strengthening sorting" process and the "strong alkali + combined reagents synergistically inhibit bismuth minerals-enhanced selective recovery of copper minerals" reagent system are adopted to achieve efficient sorting and recovery of copper, and effectively solve the technical problem of copper-bismuth separation in copper-containing bismuth concentrate.
[0007] To achieve the above object, the present invention provides a method for recovering copper from bismuth concentrate, comprising the following steps:
[0008] S1. The initial bismuth concentrate is slurried to a pulp concentration of 15 to 20%, and the initial bismuth concentrate is de-doped and deslued by flotation. The removed mud at the bottom of the flotation tank is the first bismuth concentrate, and the foam product is obtained at the top;
[0009] S2. Adding a de-agent, a pH adjuster, a bismuth inhibitor, a copper collector and a frother to the foam product obtained in step S1 in sequence, and performing rough separation of copper and bismuth to obtain a rougher concentrate and a rougher tailing, wherein the rougher tailing is a second bismuth concentrate;
[0010] S3. Adding a pH adjuster, a bismuth inhibitor and a copper collector to the rougher concentrate obtained in step S2 in sequence, and performing fine and rough separation of copper and bismuth to obtain a fine and rougher concentrate and a fine and rougher tailings;
[0011] S4. Adding a pH adjuster and a bismuth inhibitor to the rougher concentrate obtained in step S3 in sequence to perform a first concentration operation to obtain a first concentrated concentrate and a first concentrated tailings; adding a pH adjuster and a bismuth inhibitor to the first concentrated concentrate in sequence to perform a second concentration operation to obtain a copper concentrate and a second concentrated tailings, and returning the second concentrated tailings to the first concentration operation;
[0012] S5. Add a copper collector to the fine and rough tailings obtained in step S3 to perform a first scavenging operation to obtain a first scavenging concentrate and a first scavenging tailing; add a copper collector to the first scavenging tailings to perform a second scavenging operation to obtain a second scavenging concentrate and a second scavenging tailing, wherein the second scavenging tailing is a third bismuth concentrate; return the second scavenging concentrate to the first scavenging operation;
[0013] S6. The tailings from the first concentration in step S4 and the concentrate from the first scavenging in step S5 are combined and returned to the fine and rough separation operation in step S3.
[0014] As a further improvement of the present invention, the de-drug agent is activated carbon, the pH adjuster is calcium oxide, the bismuth inhibitor is CD-B1, the copper collector is ethiocarbamate, and the foaming agent is F6.
[0015] As a further improvement of the present invention, in step S2, the dosage of the de-drug agent is 1000-4000 g / t; the dosage of the pH adjuster is 10000-20000 g / t; the dosage of the bismuth inhibitor is 2000-8000 g / t; the dosage of the copper collector is 50-200 g / t, and the dosage of the foaming agent is 10-50 g / t.
[0016] As a further improvement of the present invention, in step S3, the amount of the pH adjuster is 6000-8000 g / t, the amount of the bismuth inhibitor is 1000-5000 g / t, and the amount of the copper collector is 10-100 g / t.
[0017] As a further improvement of the present invention, in step S4, the amount of pH adjuster added in the first concentrating operation is 2000-6000 g / t, and the amount of bismuth inhibitor added is 500-2000 g / t.
[0018] Furthermore, the amount of pH adjuster added in the second concentration operation is 1000-3000 g / t, and the amount of bismuth inhibitor added is 100-1000 g / t.
[0019] As a further improvement of the present invention, in step S5, the amount of copper collector added in the first scavenging operation is 10-50 g / t, and the amount of copper collector added in the second scavenging operation is 5-20 g / t.
[0020] As a further improvement of the present invention, the copper content in the initial bismuth concentrate is 2-3%, and the bismuth content is 30-35%.
[0021] As a further improvement of the present invention, the CD-B1 is obtained by mixing and compounding sodium metabisulfite, sodium sulfite, sodium carboxymethyl cellulose and sodium starch phosphate in mass percentages of 20-30%: 20-25%: 30-40%: 10-15%.
[0022] As a further improvement of the present invention, the F6 is obtained by mixing terpene alcohol, isobutanol and isopentanol in a mass percentage of 50-60%: 10-20%: 25-35%.
[0023] The beneficial effects of the present invention are:
[0024] 1. The present invention provides a method for recovering copper from bismuth concentrate, wherein water is added to the initial bismuth concentrate for slurry preparation, and no additional reagent is added. The initial bismuth concentrate is de-doped (mud) by flotation method using the residual collector and other reagents from the front-end flotation operation, and the residue at the bottom of the flotation tank is the removed mud; for the foam product obtained by flotation, a copper-bismuth separation roughing selection is performed, and the obtained roughing concentrate is subjected to a copper-bismuth separation fine-roughing selection to obtain a fine-roughing concentrate and a fine-roughing tailing; the fine-roughing concentrate is subjected to two closed-circuit selections to obtain a copper concentrate, and the fine-roughing tailing is subjected to two closed-circuit sweeping selections to obtain a tailing. The present invention adopts measures such as "flotation de-doping (mud), strong alkali + high-efficiency and environmentally friendly bismuth inhibitor CD-B1 combination to inhibit bismuth minerals, and enhanced selective recovery of copper minerals" for copper-bismuth concentrate, significantly improving the copper-bismuth separation flotation environment, improving the flotation efficiency of "bismuth suppression and copper flotation", and realizing the effective sorting and recovery of low-grade copper in bismuth concentrate.
[0025] 2. Based on the characteristics of copper-bismuth concentrate, the present invention effectively utilizes the residual reagent effect of the front-end flotation operation and the initial floatability difference of copper and bismuth minerals, and uses the capture and frothing effect of the residual reagent system to pre-float and remove the reagent (mud), pre-enrich most of the copper (accounting for about 90% of the total copper metal) and discard part of the bismuth (accounting for about 30% of the total bismuth metal), creating conditions for the subsequent "bismuth suppression and copper floating" to achieve good indicators.
[0026] 3. Under the premise of ensuring the recovery rate of copper ore dressing, the present invention adopts the process flow of "roughing and tailing-concentrating and enhanced sorting" to quickly discharge most of the bismuth minerals in the roughing operation of copper-bismuth separation, thereby achieving the sorting purpose of "early discard and early collection", and at the same time effectively reducing the circulation volume of middling ore, significantly improving the operating efficiency of "suppressing bismuth and floating copper", and improving the adaptability and stability of the process.
[0027] 4. The present invention uses activated carbon for secondary enhanced drug removal, CD-B1 high-efficiency and environmentally friendly bismuth inhibitor and calcium oxide form a high-alkali inhibition system, and ethionamide + F6 combined capture foaming system effectively expands the floatability difference between copper and bismuth minerals, achieves efficient inhibition of bismuth minerals and highly selective recovery of copper minerals, and provides key support for "inhibiting bismuth and floating copper".
[0028] 5. The present invention effectively solves the problem of difficulty in recovering copper from copper-bismuth concentrates. The process is streamlined and reliable, and the reagent system is efficient and environmentally friendly, providing a new and effective method for the recovery of similar associated copper resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A flow chart of a method for recovering copper from bismuth concentrate provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.
[0032] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0033] The present invention provides a method for recovering copper from bismuth concentrate, comprising the following steps:
[0034] S1. The initial bismuth concentrate is slurried to a pulp concentration of 15-20%, and the initial bismuth concentrate is de-doped and de-sludged by flotation. The removed mud at the bottom of the flotation tank is the first bismuth concentrate, and the foam product is obtained at the top.
[0035] Specifically, the initial bismuth concentrate is slurried with clean water without adding any other reagents, and the initial bismuth concentrate is de-doped (mud) by flotation method using the residual collectors and other reagents from the front-end flotation operation. The residual collectors and other reagents from the front-end flotation operation are common bismuth and copper flotation reagents, which are one or a combination of xanthate, black medicine, sulfur-nitrogen, thiocarbamate, hydrocarbon oil, pine oil, etc.
[0036] In terms of mass percentage, the copper content in the initial bismuth concentrate is 2-3% (mainly chalcopyrite), and the bismuth content is 30-35% (mainly bismuthinite).
[0037] S2. Add a de-agent, a pH adjuster, a bismuth inhibitor, a copper collector and a frother to the foam product obtained in step S1 in sequence, and perform rough separation of copper and bismuth to obtain a rougher concentrate and a rougher tailings, wherein the rougher tailings are the second bismuth concentrate.
[0038] Specifically, the deagent is activated carbon, and the dosage is 1000-4000 g / t; the pH adjuster is calcium oxide, and the dosage is 10000-20000 g / t; the bismuth inhibitor is CD-B1, and the dosage is 2000-8000 g / t; the copper collector is ethiocarbamate, and the dosage is 50-200 g / t; the foaming agent is F6, and the dosage is 10-50 g / t.
[0039] CD-B1 is an environmentally friendly and efficient bismuth inhibitor composed of inorganic substances and high molecular organic substances, which is specifically prepared by mixing sodium pyrosulfite, sodium sulfite, sodium carboxymethyl cellulose and sodium starch phosphate in a mass percentage of 20-30%: 20-25%: 30-40%: 10-15%.
[0040] F6 is a highly selective foaming agent composed of a variety of alcohol substances, specifically a mixture of terpene alcohol, isobutyl alcohol and isopentanol in the mass percentages of 50-60%: 10-20%: 25-35%.
[0041] S3. Adding a pH adjuster, a bismuth inhibitor and a copper collector to the rougher concentrate obtained in step S2 in sequence, and performing fine and rougher separation of copper and bismuth to obtain a fine and rougher concentrate and a fine and rougher tailings.
[0042] Specifically, the amount of the pH adjuster is 6000-8000 g / t, the amount of the bismuth inhibitor is 1000-5000 g / t, and the amount of the copper collector is 10-100 g / t.
[0043] S4. The first beneficiation operation is performed by sequentially adding a pH adjuster and a bismuth inhibitor to the rougher beneficiated concentrate obtained in step S3 to obtain a first beneficiated concentrate and a first beneficiated tailings; the second beneficiation operation is performed by sequentially adding a pH adjuster and a bismuth inhibitor to the first beneficiated concentrate to obtain a copper concentrate and a second beneficiated tailings, and the second beneficiated tailings are returned to the first beneficiation operation.
[0044] Specifically, the amount of pH adjuster added in the first beneficiation operation is 2000-6000 g / t, and the amount of bismuth inhibitor added is 500-2000 g / t. The amount of pH adjuster added in the second beneficiation operation is 1000-3000 g / t, and the amount of bismuth inhibitor added is 100-1000 g / t.
[0045] S5. Add a copper collector to the fine-rough tailings obtained in step S3 to perform a first scavenging operation to obtain a first scavenging concentrate and a first scavenging tailings; add a copper collector to the first scavenging tailings to perform a second scavenging operation to obtain a second scavenging concentrate and a second scavenging tailings, wherein the second scavenging tailings is a third bismuth concentrate; return the second scavenging concentrate to the first scavenging operation.
[0046] Specifically, the amount of copper collector added in the first scavenging operation is 10-50 g / t, and the amount of copper collector added in the second scavenging operation is 5-20 g / t.
[0047] S6. The tailings from the first concentration in step S4 and the concentrate from the first scavenging in step S5 are combined and returned to the fine and rough separation operation in step S3.
[0048] The method for recovering copper from bismuth concentrate provided by the present invention is described below with reference to specific embodiments.
[0049] Example 1
[0050] Example 1 provides a method for recovering copper from bismuth concentrate, such as Figure 1 As shown, the following steps are included:
[0051] S1. The initial bismuth concentrate is slurried with clean water to a pulp concentration of 15%, and no additional reagents are added. The initial bismuth concentrate is de-doped (mud) by using the collector and other reagents remaining in the front-end flotation operation, and the residue at the bottom of the flotation tank is the removed mud, i.e., the first bismuth concentrate ( Figure 1 In the figure, it is represented as bismuth concentrate 1);
[0052] S2. The froth product obtained by flotation in step S1 is sequentially added with activated carbon 2000 g / t as a de-agent, calcium oxide 15000 g / t as a pH adjuster, CD-B1 5000 g / t as a bismuth inhibitor, 100 g / t as a copper collector, and 30 g / t as a frother F6 to perform rough separation of copper and bismuth to obtain a rough concentrate and tailings 1, wherein the tailings 1 is the second bismuth concentrate ( Figure 1 In the figure, it is represented as bismuth concentrate 2); CD-B1 is prepared by mixing sodium pyrosulfite, sodium sulfite, sodium carboxymethyl cellulose and sodium starch phosphate in a mass percentage of 25%:25%:35%:15%; F6 is prepared by mixing terpene alcohol, isobutyl alcohol and isopentanol in a mass percentage of 55%:15%:30%;
[0053] S3. For the rougher concentrate obtained in step S2, calcium oxide 7000 g / t, bismuth inhibitor CD-B12000 g / t, and ethiocarbamate 60 g / t are sequentially added to perform copper-bismuth separation and roughing to obtain a rougher concentrate and a rougher tailings;
[0054] S4. For the rougher concentrate obtained in step S3, copper concentrate is obtained by two closed-circuit concentrations. 4000g / t of calcium oxide and 1000g / t of bismuth inhibitor CD-B1 are added in the concentration operation 1; 2000g / t of calcium oxide and 500g / t of bismuth inhibitor CD-B1 are added in the concentration operation 2, and the tailings of the concentration operation 2 are returned to the concentration operation 1;
[0055] S5. For the fine and rough tailings obtained in step S3, tailings 2 are obtained after two closed-circuit sweeps, i.e., the third bismuth concentrate ( Figure 1 In the figure, it is represented as bismuth concentrate 3). 30 g / t of ethylthiocarbamate is added to scavenging operation 1, 10 g / t of ethylthiocarbamate is added to scavenging operation 2, and the concentrate of scavenging operation 2 is returned to scavenging operation 1;
[0056] S6. The tailings from the concentration operation 1 in step S4 and the concentrate from the scavenging operation 1 in step S5 are combined and returned to the fine and rough separation operation in step S3.
[0057] The experimental data obtained in this example are shown in Table 1.
[0058] Table 1 Example 1 Test results
[0059]
[0060]
[0061] Comparative Example 1
[0062] Comparative Example 1 provides a method for recovering copper from bismuth concentrate. Compared with Example 1, the only difference is that there is no flotation de-drug (mud) operation in step S1, and other experimental parameters and conditions are basically the same as those in Example 1, which will not be repeated here. The experimental data obtained are shown in Table 2, and it can be seen that the copper recovery effect is poor, and bismuth is lost more in the copper concentrate, which indicates that the flotation de-drug (mud) step plays a key role in the process of recovering copper from bismuth concentrate. The flotation de-drug (mud) operation is not performed, and impurities and fine mud are not effectively removed, which affects the flotation effect of copper; bismuth and other valuable metals may not be effectively separated due to the interference of fine mud, resulting in the loss of bismuth in the copper concentrate.
[0063] Table 2 Comparative Example 1 Test Results
[0064]
[0065] Comparative Example 2
[0066] Comparative Example 2 provides a method for recovering copper from bismuth concentrate. Compared with Example 1, the only difference is that CD-B1 is not added in step S2, step S3 and step S4, and other experimental parameters and conditions are basically the same as those in Example 1, which will not be repeated here. The experimental data obtained are shown in Table 3, which shows that the copper recovery effect is poor and bismuth is lost more in copper concentrate. Due to the lack of CD-B1, bismuth minerals are not effectively suppressed, resulting in bismuth minerals being recovered together with copper minerals during flotation, increasing the loss of bismuth in copper concentrate. The mixing of bismuth minerals and copper minerals causes a decrease in flotation selectivity, thereby affecting the recovery rate of copper.
[0067] Table 3 Comparative Example 2 Test Results
[0068]
[0069] In summary, the present invention adopts measures such as "flotation removal of drugs (mud), strong alkali + high-efficiency and environmentally friendly bismuth inhibitor CD-B1 combination to inhibit bismuth minerals, and enhanced selective recovery of copper minerals" for copper-bismuth concentrate, which significantly improves the copper-bismuth separation flotation environment, improves the "bismuth-suppressing copper flotation" flotation efficiency, and realizes the effective sorting and recovery of low-grade copper in bismuth concentrate.
[0070] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for recovering copper from bismuth concentrate, characterized in that: The following steps are involved: S1. The initial bismuth concentrate is slurried to a pulp concentration of 15 to 20%, and the initial bismuth concentrate is de-doped and deslued by flotation. The removed mud at the bottom of the flotation tank is the first bismuth concentrate, and the foam product is obtained at the top; S2. Adding a de-agent, a pH adjuster, a bismuth inhibitor, a copper collector and a frother to the foam product obtained in step S1 in sequence, and performing rough separation of copper and bismuth to obtain a rougher concentrate and a rougher tailing, wherein the rougher tailing is a second bismuth concentrate; S3. Adding a pH adjuster, a bismuth inhibitor and a copper collector to the rougher concentrate obtained in step S2 in sequence, and performing fine and rough separation of copper and bismuth to obtain a fine and rougher concentrate and a fine and rougher tailings; S4. Adding a pH adjuster and a bismuth inhibitor to the rougher concentrate obtained in step S3 in sequence to perform a first concentration operation to obtain a first concentrated concentrate and a first concentrated tailings; adding a pH adjuster and a bismuth inhibitor to the first concentrated concentrate in sequence to perform a second concentration operation to obtain a copper concentrate and a second concentrated tailings, and returning the second concentrated tailings to the first concentration operation; S5. Add a copper collector to the fine and rough tailings obtained in step S3 to perform a first scavenging operation to obtain a first scavenging concentrate and a first scavenging tailing; add a copper collector to the first scavenging tailings to perform a second scavenging operation to obtain a second scavenging concentrate and a second scavenging tailing, wherein the second scavenging tailing is a third bismuth concentrate; return the second scavenging concentrate to the first scavenging operation; S6. The tailings from the first concentration in step S4 and the concentrate from the first scavenging in step S5 are combined and returned to the fine and rough separation operation in step S3.
2. The method for recovering copper from bismuth concentrate according to claim 1, characterized in that: The de-drug agent is activated carbon, the pH adjuster is calcium oxide, the bismuth inhibitor is CD-B1, the copper collector is ethiocarbamate, and the foaming agent is F6.
3. The method for recovering copper from bismuth concentrate according to claim 2, characterized in that: In step S2, the dosage of the de-agent is 1000-4000 g / t; the dosage of the pH adjuster is 10000-20000 g / t; the dosage of the bismuth inhibitor is 2000-8000 g / t; the dosage of the copper collector is 50-200 g / t, and the dosage of the foaming agent is 10-50 g / t.
4. The method for recovering copper from bismuth concentrate according to claim 2, characterized in that: In step S3, the pH adjuster is used in an amount of 6000-8000 g / t, the bismuth inhibitor is used in an amount of 1000-5000 g / t, and the copper collector is used in an amount of 10-100 g / t.
5. The method for recovering copper from bismuth concentrate according to claim 2, characterized in that: In step S4, the amount of pH adjuster added in the first concentrating operation is 2000-6000 g / t, and the amount of bismuth inhibitor added is 500-2000 g / t.
6. The method for recovering copper from bismuth concentrate according to claim 5, characterized in that: The amount of pH adjuster added in the second concentration operation is 1000-3000 g / t, and the amount of bismuth inhibitor added is 100-1000 g / t.
7. The method for recovering copper from bismuth concentrate according to claim 2, characterized in that: In step S5, the amount of copper collector added in the first scavenging operation is 10-50 g / t, and the amount of copper collector added in the second scavenging operation is 5-20 g / t.
8. The method for recovering copper from bismuth concentrate according to claim 1, characterized in that: The initial bismuth concentrate contains 2-3% copper and 30-35% bismuth.
9. The method for recovering copper from bismuth concentrate according to claim 2, characterized in that: The CD-B1 is prepared by mixing sodium pyrosulfite, sodium sulfite, sodium carboxymethyl cellulose and sodium starch phosphate in a mass percentage of 20-30%: 20-25%: 30-40%: 10-15%.
10. The method for recovering copper from bismuth concentrate according to claim 2, characterized in that: The F6 is prepared by mixing terpene alcohol, isobutyl alcohol and isopentanol in a mass percentage of 50-60%: 10-20%: 25-35%.
Citation Information
Patent Citations
Ultrasonic dispersing-magnetic separating separation technique for copper-bismuth mixed concentrate ore
CN106238202A
Separation method for bismuth-molybdenum-copper-sulfide mixed concentrate
CN101537388A
Separation method for copper bismuth bulk concentrates
CN103240166A
Method for recovering valuable metal from sulfide ore-contained tungsten rough concentrate
CN105498948A
Bismuth sulfide mineral inhibiting agent and application thereof
CN108620240A
Cited By
Method for carrying out closed-loop reagent removal flotation on rare earth by utilizing backwater
CN119747101A
Sorting method of arsenopyrite-containing copper sulphide ore
CN120023008A