MXene / rGO / CoFe2O4 aerogel composite material and preparation method thereof
Through the preparation of MXene/rGO/CoFe2O4 aerogel composite material, the three-dimensional porous structure and magnetic filler are used to solve the problem of low electromagnetic wave absorption and thermal barrier performance, and efficient electromagnetic wave absorption and thermal barrier are achieved, suitable for aerospace, etc. field.
Patent Information
- Application Number
- CN202411283836.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-17
AI Technical Summary
The existing electromagnetic wave absorbing materials ignore the heat accumulation problem caused by electronic devices when reducing electromagnetic interference, and MXene is difficult to form a three-dimensional porous structure, resulting in low electromagnetic wave absorption and thermal barrier properties.
The preparation method of MXene/rGO/CoFe2O4 aerogel composite material was prepared by LiF-HCl etching, improved Hummer method and hydrothermal method, and three-dimensional was formed by hydrothermal method and freeze-drying technology. Porous aerogels improve the electromagnetic wave absorption and thermal barrier properties of the material.
It realizes a composite material that combines high electromagnetic wave absorption and thermal barrier, a simple and feasible preparation method, has low production costs and wide application value, and meets the needs of aerospace and other fields.
Smart Images

Figure CN119155976A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of composite material preparation, and in particular relates to a method for preparing a MXene / rGO / CoFe2O4 aerogel composite material, and also relates to the MXene / rGO / CoFe2O4 aerogel composite material. Background Art
[0002] Traditional electromagnetic wave absorbing materials focus on reducing electromagnetic interference, but ignore the problem of heat accumulation caused by electronic devices. Therefore, designing and preparing electromagnetic wave absorbing materials with strong electromagnetic wave absorption ability and high heat barrier properties is of great significance to solving this series of problems.
[0003] A large number of studies have found that adding magnetic components to aerogels to introduce magnetic losses and construct three-dimensional porous structures are key strategies to alleviate the impedance mismatch between materials and free space, which can effectively introduce more incident waves and enhance the multiple reflection and scattering effects inside the material. At the same time, its three-dimensional porous structure gives it excellent thermal barrier properties.
[0004] CoFe2O4 and Ti3C2T x (MXene) is widely used in electromagnetic wave absorption as a typical magnetic material and conductive filler. However, due to its weak gelation ability, MXene is difficult to form a three-dimensional porous structure. In recent years, constructing graphene oxide (GO) into aerogel has been proven to be an effective way to enhance gelation ability. Graphene oxide is a typical two-dimensional material. It has the characteristics of ultra-low bulk density, large specific surface area, and rich functional groups. Using graphene oxide to enhance the gelation ability of MXene and introducing the magnetic material CoFe2O4 to form an aerogel is a promising strategy. In addition, studies have shown that the three-dimensional porous structure of the composite material plays a vital role in its electromagnetic wave absorption and thermal barrier effect. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a MXene / rGO / CoFe2O4 aerogel composite material, which solves the problems of low electromagnetic wave absorption performance and low thermal barrier performance of the composite material in the prior art.
[0006] Another object of the present invention is to provide the above-mentioned MXene / rGO / CoFe2O4 aerogel composite material.
[0007] The technical solution adopted by the present invention is a method for preparing a MXene / rGO / CoFe2O4 aerogel composite material, which is specifically implemented according to the following steps:
[0008] Step 1, etching Ti3AlC2 precursor with LiF-HCl to prepare few-layer MXene powder;
[0009] Step 2, preparing rGO powder by improved Hummer method;
[0010] Step 3, preparing magnetic material CoFe2O4 powder by hydrothermal method;
[0011] Step 4: After step 3, a MXene / rGO / CoFe2O4 aerogel composite material is prepared using a hydrothermal method and freeze-drying technology.
[0012] The present invention is also characterized in that:
[0013] In step 1, the specific steps are as follows:
[0014] Step 1.1, LiF and HCl are fully mixed, and then MAX phase precursor powder is slowly added under ice bath conditions to obtain a mixture;
[0015] Step 1.2, the mixture is stirred to obtain Ti3C2T x The suspension was then repeatedly centrifuged and washed with deionized water until the pH of the solution was 7 to obtain Ti3C2T x Sediment;
[0016] Step 1.3, Ti3C2T x The precipitate was dispersed in deionized water and ultrasonically treated for 15 min to promote the delamination of multilayer MXene. Then, the centrifugation was continued for several cycles, and the supernatant was taken to obtain a few-layer MXene dispersion.
[0017] Step 1.4, the few-layer MXene dispersion obtained above is pre-frozen at -26°C, and then freeze-dried using a freeze dryer to obtain a few-layer MXene powder.
[0018] In step 2, the specific steps are as follows:
[0019] Step 2.1, dissolving P2O5, K2S2O8 and graphite in sulfuric acid under oil bath conditions, stirring for 5-7 hours and mixing evenly; the mass ratio of P2O5, K2S2O8 and graphite is 0.5-1.5:0.5-1.5:0.25-1.35;
[0020] Step 2.2, vacuum filter the mixture obtained in step 2.1, collect the precipitate, dissolve the mixture in sulfuric acid under ice bath conditions, add potassium permanganate in batches, stir for 1-3 hours after each addition, and mix well;
[0021] Step 2.3, adding deionized water and hydrogen peroxide to the solution of step 2.2, and then adding the solution into dilute hydrochloric acid, and standing for 12-24 hours; taking the lower layer of the mixed solution and placing it into water for dialysis, the dialysis time is 48-72 hours, and after the dialysis, stirring the solution for 3-5 hours;
[0022] Step 2.4, precooling the GO dispersion obtained in step 2.3, and then freeze-drying to obtain rGO powder.
[0023] In step 2.4, the precooling temperature is -21 to -31°C, and the precooling time is 30 to 60 minutes; the freeze-drying temperature is -30 to -40°C, and the freeze-drying time is 48 to 72 hours.
[0024] In step 3, specifically:
[0025] CoCl2·6H2O, FeCl3·6H2O, urea and ascorbic acid powder are added to deionized water and stirred for 20-30 minutes to obtain a mixed solution. The mixed solution is transferred to a high-pressure reactor for hydrothermal reaction, cooled, and the precipitate is collected, centrifuged, washed, and dried to obtain CoFe2O4 powder.
[0026] The reaction temperature is 170-180°C, the reaction time is 11-13h; the mass ratio of CoCl2·6H2O, FeCl3·6H2O, urea, ascorbic acid and deionized water is 0.5-1.5:1.89-2.79:2.70-3.80:6.15-6.75:3.42-4.78.
[0027] In step 4, specifically:
[0028] Step 4.1, adding few-layer MXene powder, rGO powder, and CoFe2O4 powder into deionized water, stirring to obtain a mixed solution, transferring the mixed solution into a high-pressure reactor, performing a hydrothermal reaction, cooling, and soaking the obtained aerogel in a mixed solution of water and ethanol for hydrolysis;
[0029] Step 4.2, precooling the aerogel obtained in step 4.1, and then freeze-drying it to obtain MXene / rGO / CoFe2O4 aerogel;
[0030] The precooling temperature is -21 to -31°C, and the precooling time is 30 to 60 minutes; the freeze-drying temperature is -30 to -40°C, and the freeze-drying time is 48 to 72 hours.
[0031] In step 4.1, the stirring time is 20-30 minutes; the mass ratio of water to ethanol is 9-11:0.5-1.5; the reaction temperature is 170-180°C, the reaction time is 9-11 hours; and the soaking time is 24-48 hours.
[0032] In step 4.1, the mass ratio of few-layer MXene powder, rGO powder, CoFe2O4 powder, and deionized water is 0.5-1.5: 0.5-1.5: 0.06-0.81: 1.5-4.5.
[0033] Another technical solution adopted by the present invention is a MXene / rGO / CoFe2O4 aerogel composite material prepared by a preparation method of a MXene / rGO / CoFe2O4 aerogel composite material.
[0034] The beneficial effect of the present invention is that the method of the present invention, through the design of three-dimensional porous aerogel, introduces magnetic fillers to provide magnetic loss, and prepares a composite material with both high electromagnetic wave absorption and thermal barrier; at the same time, the preparation method is simple and feasible, has a low production cost, and is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the morphology of CoFe2O4 powder.
[0036] Figure 2 This is the morphology of the MXene / rGO / CoFe2O4 aerogel composite material of Example 4.
[0037] Figure 3 This is the XPS graph of the MXene / rGO / CoFe2O4 aerogel composite material of Example 4.
[0038] Figure 4 is a graph showing the electromagnetic wave absorption performance of the MXene / rGO / CoFe2O4 aerogel composite material of Example 1;
[0039] Figure 5 is a graph showing the electromagnetic wave absorption performance of the MXene / rGO / CoFe2O4 aerogel composite material of Example 2;
[0040] Figure 6 is a graph showing the electromagnetic wave absorption performance of the MXene / rGO / CoFe2O4 aerogel composite material of Example 3;
[0041] Figure 7 is a graph showing the electromagnetic wave absorption performance of the MXene / rGO / CoFe2O4 aerogel composite material of Example 4;
[0042] Figure 8 This is a graph showing the electromagnetic wave absorption performance of the MXene / rGO / CoFe2O4 aerogel composite material of Example 5. DETAILED DESCRIPTION
[0043] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0044] The preparation method of the MXene / rGO / CoFe2O4 aerogel composite material of the present invention is specifically implemented according to the following steps:
[0045] Step 1: Etch the Ti3AlC2 precursor with LiF-HCl to prepare a few-layer Ti3C2T x MXene powder; the specific steps are as follows:
[0046] Step 1.1, LiF and HCl are fully mixed, and then MAX phase precursor powder is slowly added under ice bath conditions to obtain a mixture;
[0047] The mass ratio of LiF, HCl and MAX phase precursor powder is 1:20:1;
[0048] Step 1.2, the mixture was stirred at 35 °C for 24 h to obtain Ti3C2T x The suspension was then repeatedly centrifuged and washed with deionized water until the pH of the solution was 7 to obtain Ti3C2T x Sediment;
[0049] During centrifugal washing, the centrifugal speed was 3500r / min;
[0050] Step 1.3, Ti3C2T x The precipitate was dispersed in deionized water and ultrasonically treated for 15 min to promote the delamination of multilayer MXene. Then, the mixture was centrifuged at 3500 r / min for 15 min, and the cycle was repeated several times. The supernatant was collected to obtain a few-layer MXene dispersion.
[0051] Step 1.4, the few-layer MXene dispersion obtained above is pre-frozen at -26°C, and then freeze-dried using a freeze dryer to obtain a few-layer MXene powder;
[0052] Step 2, preparing rGO powder by improved Hummer method; the specific steps are as follows:
[0053] Step 2.1, in an oil bath, dissolve phosphorus pentoxide (P2O5), potassium persulfate (K2S2O8), and graphite in sulfuric acid, stir for 5-7 hours, and mix well;
[0054] The mass ratio of P2O5, K2S2O8 and graphite is 0.5-1.5:0.5-1.5:0.25-1.35.
[0055] Step 2.2, vacuum filter the mixture obtained in step 2.1, collect the precipitate, dissolve the mixture in sulfuric acid under ice bath conditions, add potassium permanganate (KMnO4) in batches, stir for 1-3 hours after each addition, and mix well;
[0056] Step 2.3, adding deionized water and hydrogen peroxide (H2O2) to the solution of step 2.2 to remove KMnO4, then adding the solution into dilute hydrochloric acid and standing for 12-24 hours; taking the lower layer of the mixed solution and placing it into water for dialysis for 48-72 hours, and after dialysis, stirring the solution at high speed for 3-5 hours at a stirring rate of 2000-3000 r / min;
[0057] Step 2.4, precooling the GO dispersion obtained in step 2.3, and then freeze-drying to obtain rGO powder;
[0058] The precooling temperature is -21~-31℃, and the precooling time is 30-60min;
[0059] The freeze drying temperature is -30 to -40°C and the freeze drying time is 48 to 72 hours;
[0060] Step 3, preparing magnetic material CoFe2O4 powder by hydrothermal method; specifically:
[0061] Add CoCl2·6H2O, FeCl3·6H2O, urea and ascorbic acid powder into deionized water, stir for 20-30 minutes to obtain a mixed solution, transfer the mixed solution into a high-pressure reactor, perform a hydrothermal reaction at a reaction temperature of 170-180°C and a reaction time of 11-13 hours; then cool naturally to room temperature, collect the precipitate, wash by centrifugation at a centrifugal speed of 8000 r / min, and dry to obtain CoFe2O4 powder;
[0062] The mass ratio of CoCl2·6H2O, FeCl3·6H2O, urea, ascorbic acid, and deionized water is 0.5-1.5: 1.89-2.79: 2.70-3.80: 6.15-6.75: 3.42-4.78;
[0063] Step 4, after step 3, using a hydrothermal method and freeze drying technology to prepare a MXene / rGO / CoFe2O4 aerogel composite material; specifically:
[0064] Step 4.1, adding few-layer MXene powder, rGO powder, and CoFe2O4 powder to deionized water, stirring for 20-30 minutes to obtain a mixed solution, transferring the mixed solution to a high-pressure reactor for hydrothermal reaction at a reaction temperature of 170-180°C for a reaction time of 9-11 hours; naturally cooling to room temperature, soaking the obtained aerogel in a mixed solution of water and ethanol for 24-48 hours for hydrolysis to remove excess ions;
[0065] The mass ratio of water to ethanol is 9-11:0.5-1.5;
[0066] The mass ratio of few-layer MXene powder, rGO powder, CoFe2O4 powder, and deionized water is 0.5-1.5: 0.5-1.5: 0.06-0.81: 1.5-4.5;
[0067] Step 4.2, precooling the aerogel obtained in step 4.1, and then freeze-drying it to obtain MXene / rGO / CoFe2O4 aerogel.
[0068] The precooling temperature is -21~-31℃, and the precooling time is 30-60min;
[0069] The freeze-drying temperature is -30 to -40°C, and the freeze-drying time is 48 to 72 hours.
[0070] The mechanism of action of the method of the present invention is: using a MXene / rGO / CoFe2O4 aerogel composite material with a magnetic three-dimensional porous structure, when an electromagnetic wave enters, the electromagnetic wave is easy to enter the interior of the material due to the optimization of impedance matching between the magnetic component and the porous structure. Subsequently, the incident electromagnetic wave attenuates the incident wave through multiple reflections and scattering in the porous structure. In addition, CoFe2O4 provides magnetic loss, which improves the magnetic loss capacity of the electromagnetic wave. Moreover, a large number of effective interfaces are obtained in the aerogel formed by MXene and rGO, which triggers interface polarization and dipole polarization, improves impedance matching, increases dielectric loss, and further produces a stronger electromagnetic wave loss capacity, thereby obtaining a relatively excellent electromagnetic wave absorption performance.
[0071] The MXene / rGO / CoFe2O4 aerogel composite material with high electromagnetic wave absorption performance prepared by the present invention using a hydrothermal method and a freeze-drying method has a safe and environmentally friendly preparation process, a simple preparation process and low cost, and has wide practicality and promotion value; and the MXene / rGO / CoFe2O4 aerogel composite material has excellent electromagnetic wave absorption performance and can meet the application requirements of aerospace, electronic packaging and other fields.
[0072] Example 1
[0073] The preparation method of the MXene / rGO / CoFe2O4 aerogel composite material of the present invention comprises the following specific steps:
[0074] Step 1: Prepare few-layer Ti3C2T by etching Ti3AlC2 precursor with LiF-HCl x MXene powder, the specific steps are as follows:
[0075] Step 1.1, 1 g LiF was thoroughly mixed with 20 mL 9 mol / L HCl, and then 1 g MAX phase precursor powder was slowly added under ice bath conditions;
[0076] Step 1.2, the above mixture was stirred at 35 °C for 24 h to obtain Ti3C2T x The suspension was washed repeatedly with deionized water until the pH was 7 and centrifuged at 3500 r / min;
[0077] Step 1.3, Ti3C2T x The precipitate was dispersed in 100 ml of deionized water and ultrasonically treated for 20 min to promote the delamination of multilayer MXene. Then, the precipitate was centrifuged at 3500 r / min for 5 min, and the cycle was repeated several times. The supernatant was collected to obtain a MXene dispersion.
[0078] In step 1.4, the few-layer MXene dispersion obtained above is pre-frozen at -26°C for 12 hours and then freeze-dried for 48 hours to obtain the few-layer MXene powder.
[0079] Step 2: Prepare GO powder by improving the Hummer method. The specific steps are as follows:
[0080] Step 2.1, in an oil bath, dissolve phosphorus pentoxide (P2O5), potassium persulfate (K2S2O8), and graphite in sulfuric acid, stir for 6 hours, and mix well;
[0081] The mass ratio of P2O5, K2S2O8 and graphite is 1:1:0.75.
[0082] Step 2.2, vacuum filter the mixture, collect the precipitate, dissolve the mixture in sulfuric acid under ice bath conditions, add 9g potassium permanganate (KMnO 4 ), stir for 2h and mix well;
[0083] Step 2.3, add deionized water and hydrogen peroxide (H2O2) to the solution to remove KMnO4. Add the solution to dilute hydrochloric acid and let stand for 12 hours; take the lower layer of the mixed solution and put it into water for dialysis for 48 hours. Stir the solution at high speed for 5 hours;
[0084] Step 2.4, the GO dispersion obtained above was precooled at -26°C for 30 min, and then freeze-dried at -30°C for 48 h using a freeze dryer to obtain GO powder.
[0085] Step 3, preparing magnetic material CoFe2O4 powder by hydrothermal method, specifically:
[0086] Add CoCl2·6H2O, FeCl3·6H2O, urea and ascorbic acid powder into deionized water and stir for 30 minutes to obtain a mixed solution. Transfer the mixed solution to a high-pressure reactor and keep it at 170°C for 12 hours. Then cool it naturally to room temperature. Collect the precipitate, wash and dry it to obtain CoFe2O4 powder;
[0087] The mass ratio of CoCl2·6H2O, FeCl3·6H2O, urea and ascorbic acid is 1:2.29:3.30:6.45.
[0088] Step 4, after step 3, using a hydrothermal method and freeze drying technology to prepare a MXene / rGO / CoFe2O4 aerogel composite material; specifically:
[0089] Step 4.1, add 0.03g MXene, 0.03g rGO, and 0.006g CoFe2O4 powder into deionized water and stir for 30min to obtain a mixed solution. Move the mixed solution into a high-pressure reactor, keep it at 180℃ for 10h, and then cool it naturally to room temperature; soak the obtained aerogel in a mixed solution of water and ethanol for 24h for hydrolysis to remove excess ions; the mass ratio of water to ethanol is 10:1.
[0090] Step 4.2, the aerogel obtained above was pre-frozen at -26°C for 12 hours, and then freeze-dried at -30°C for 48 hours using a freeze dryer to obtain MXene / rGO / CoFe2O4 aerogel; the loading amount of CoFe2O4 in the aerogel was 10wt%;
[0091] like Figure 4 As shown, the minimum reflection loss of the MXene / rGO / CoFe2O4 aerogel composite material prepared in Example 1 is -7.8 dB at 2.50 mm-4.50 mm.
[0092] Example 2
[0093] The preparation method of the MXene / rGO / CoFe2O4 aerogel composite material of the present invention comprises the following specific steps:
[0094] Step 1: Prepare few-layer Ti3C2T by etching Ti3AlC2 precursor with LiF-HCl xMXene powder, the specific steps are as follows:
[0095] Step 1.1, 1 g LiF was thoroughly mixed with 20 mL 9 mol / L HCl, and then 1 g MAX phase precursor powder was slowly added under ice bath conditions;
[0096] Step 1.2, the above mixture was stirred at 35 °C for 24 h to obtain Ti3C2T x The suspension was washed repeatedly with deionized water until the pH was 7 and centrifuged at 3500 r / min;
[0097] Step 1.3, Ti3C2T x The precipitate was dispersed in 100 ml of deionized water and ultrasonically treated for 20 min to promote the delamination of multilayer MXene. Then, the precipitate was centrifuged at 3500 r / min for 5 min, and the cycle was repeated several times. The supernatant was collected to obtain a MXene dispersion.
[0098] In step 1.4, the few-layer MXene dispersion obtained above is pre-frozen at -26°C for 12 hours and then freeze-dried for 48 hours to obtain the few-layer MXene powder.
[0099] Step 2: Prepare GO powder by improving the Hummer method. The specific steps are as follows:
[0100] Step 2.1, dissolve phosphorus pentoxide (P2O5), potassium persulfate (K2S2O8) and graphite in sulfuric acid under oil bath conditions. Stir for 6 hours to mix well;
[0101] The mass ratio of P2O5, K2S2O8 and graphite is 1:1:0.75.
[0102] Step 2.2, vacuum filter the mixture and collect the precipitate. Dissolve the mixture in sulfuric acid under ice bath conditions, add 9 g potassium permanganate (KMnO 4 ), stir for 2h and mix well;
[0103] Step 2.3, deionized water and hydrogen peroxide (H2O2) are added to the solution to remove KMnO4, and the solution is added to dilute hydrochloric acid and allowed to stand for 12 hours; the lower layer of the mixed solution is taken and dialyzed in water for 48 hours, and the solution is stirred at high speed for 5 hours;
[0104] Step 2.4, after precooling the GO dispersion obtained above, freeze-dry it using a freeze dryer to obtain GO powder.
[0105] The precooling temperature is -25℃ and the precooling time is 40min;
[0106] The freeze drying temperature was -35°C and the freeze drying time was 50h;
[0107] Step 3, preparing magnetic material CoFe2O4 powder by hydrothermal method, specifically:
[0108] Add 0.048g CoCl2·6H2O, 0.11g FeCl3·6H2O, 0.31g urea, and 0.158g ascorbic acid powder into deionized water and stir for 30 minutes to obtain a mixed solution. Transfer the mixed solution to a high-pressure reactor, keep it at 170°C for 12 hours, and then cool it naturally to room temperature. Collect the precipitate, wash it by centrifugation, and dry it to obtain CoFe2O4 powder;
[0109] Step 4, after step 3, using a hydrothermal method and freeze drying technology to prepare a MXene / rGO / CoFe2O4 aerogel composite material; specifically:
[0110] Step 4.1, add 0.03g MXene, 0.03g rGO, and 0.018g CoFe2O4 powder into deionized water and stir for 30min to obtain a mixed solution. Move the mixed solution into a high-pressure reactor, keep it at 180℃ for 10h, and then cool it naturally to room temperature; soak the obtained aerogel in a mixed solution of water and ethanol for 24h for hydrolysis to remove excess ions; the mass ratio of water to ethanol is 10:1.
[0111] Step 4.2, the aerogel obtained above was pre-frozen at -26°C for 12 hours, and then freeze-dried at -33°C for 48 hours using a freeze dryer to obtain MXene / rGO / CoFe2O4 aerogel. The loading amount of CoFe2O4 in the aerogel was 30 wt%.
[0112] like Figure 5 As shown, the minimum reflection loss of the MXene / rGO / CoFe2O4 aerogel composite material prepared in Example 2 is -8.1 dB at 2.50 mm-4.50 mm.
[0113] Example 3
[0114] The preparation method of the MXene / rGO / CoFe2O4 aerogel composite material of the present invention comprises the following specific steps:
[0115] Step 1: Prepare few-layer Ti3C2T by etching Ti3AlC2 precursor with LiF-HCl x MXene powder, the specific steps are as follows:
[0116] Step 1.1, 1 g LiF was thoroughly mixed with 20 mL 9 mol / L HCl, and then 1 g MAX phase precursor powder was slowly added under ice bath conditions;
[0117] Step 1.2, the above mixture was stirred at 35 °C for 24 h to obtain Ti3C2T x The suspension was washed repeatedly with deionized water until the pH was 7 and centrifuged at 3500 r / min;
[0118] Step 1.3, Ti3C2T x The precipitate was dispersed in 100 ml of deionized water and ultrasonically treated for 20 min to promote the delamination of multilayer MXene. Then, the precipitate was centrifuged at 3500 r / min for 5 min, and the cycle was repeated several times. The supernatant was collected to obtain a MXene dispersion.
[0119] In step 1.4, the few-layer MXene dispersion obtained above is pre-frozen at -26°C for 12 hours and then freeze-dried for 48 hours to obtain the few-layer MXene powder.
[0120] Step 2: Prepare GO powder by improving the Hummer method. The specific steps are as follows:
[0121] Step 2.1, in an oil bath, dissolve phosphorus pentoxide (P2O5), potassium persulfate (K2S2O8), and graphite in sulfuric acid, stir for 6 hours, and mix well;
[0122] The mass ratio of P2O5, K2S2O8 and graphite is 1:1:0.75.
[0123] Step 2.2, vacuum filter the mixture and collect the precipitate. Dissolve the mixture in sulfuric acid under ice bath conditions, add 9 g potassium permanganate (KMnO 4 ). Stir for 2h to mix well;
[0124] Step 2.3, add deionized water and hydrogen peroxide (H2O2) to the solution to remove KMnO4. Add the solution to dilute hydrochloric acid and let stand for 12 hours; take the lower layer of the mixed solution and put it into water for dialysis for 48 hours. Stir the solution at high speed for 5 hours;
[0125] Step 2.5, precooling the GO dispersion obtained above, and freeze-drying it using a freeze dryer to obtain GO powder;
[0126] The precooling temperature is -30℃ and the precooling time is 50min;
[0127] The freeze-drying temperature was -36°C and the freeze-drying time was 65h;
[0128] Step 3, preparing magnetic material CoFe2O4 powder by hydrothermal method, specifically:
[0129] Add 0.048g CoCl2·6H2O, 0.11g FeCl3·6H2O, 0.31g urea, and 0.158g ascorbic acid powder into deionized water and stir for 30 minutes to obtain a mixed solution. Transfer the mixed solution to a high-pressure reactor and keep it at 170°C for 12 hours. Then cool it naturally to room temperature. Collect the precipitate, wash it by centrifugation, and dry it to obtain CoFe2O4 powder;
[0130] Step 4, after step 3, using a hydrothermal method and freeze drying technology to prepare a MXene / rGO / CoFe2O4 aerogel composite material; specifically:
[0131] Step 4.1, add 0.03g MXene, 0.03g rGO, and 0.03g CoFe2O4 powder into deionized water and stir for 30min to obtain a mixed solution. Move the mixed solution into a high-pressure reactor and keep it at 180℃ for 10h. Then cool it naturally to room temperature; soak the obtained aerogel in a mixed solution of water and ethanol for 24h for hydrolysis to remove excess ions; the mass ratio of water to ethanol is 10:1.
[0132] Step 4.2, the aerogel obtained above was pre-frozen at -26°C for 12 hours, and then freeze-dried at -40°C for 48 hours using a freeze dryer to obtain MXene / rGO / CoFe2O4 aerogel. The loading amount of CoFe2O4 in the aerogel was 50wt%.
[0133] like Figure 6 As shown, the minimum reflection loss of the MXene / rGO / CoFe2O4 aerogel composite material prepared in Example 3 is -8.3 dB at 2.50 mm-4.50 mm.
[0134] Example 4
[0135] The preparation method of the MXene / rGO / CoFe2O4 aerogel composite material of the present invention comprises the following specific steps:
[0136] Step 1: Prepare few-layer Ti3C2T by etching Ti3AlC2 precursor with LiF-HCl x MXene powder, the specific steps are as follows:
[0137] Step 1.1, 1 g LiF was thoroughly mixed with 20 mL 9 mol / L HCl, and then 1 g MAX phase precursor powder was slowly added under ice bath conditions;
[0138] Step 1.2, the above mixture was stirred at 35 °C for 24 h to obtain Ti3C2T xThe suspension was washed repeatedly with deionized water until the pH was 7 and centrifuged at 3500 r / min;
[0139] Step 1.3, Ti3C2T x The precipitate was dispersed in 100 ml of deionized water and ultrasonically treated for 20 min to promote the delamination of multilayer MXene. Then, the precipitate was centrifuged at 3500 r / min for 5 min, and the cycle was repeated several times. The supernatant was collected to obtain a MXene dispersion.
[0140] In step 1.4, the few-layer MXene dispersion obtained above is pre-frozen at -26°C for 12 hours and then freeze-dried for 48 hours to obtain the few-layer MXene powder.
[0141] Step 2: Prepare GO powder by improving the Hummer method. The specific steps are as follows:
[0142] Step 2.1, in an oil bath, dissolve phosphorus pentoxide (P2O5), potassium persulfate (K2S2O8), and graphite in sulfuric acid, stir for 6 hours, and mix well;
[0143] The mass ratio of P2O5, K2S2O8 and graphite is 1:1:0.75.
[0144] Step 2.2, vacuum filter the mixture and collect the precipitate. Dissolve the mixture in sulfuric acid under ice bath conditions, add 9 g potassium permanganate (KMnO 4 ). Stir for 2h to mix well;
[0145] Step 2.3, add deionized water and hydrogen peroxide (H2O2) to the solution to remove KMnO4, add the solution to dilute hydrochloric acid, and let it stand for 12 hours; take the lower layer of the mixed solution and put it into water for dialysis for 48 hours. Stir the solution at high speed for 5 hours;
[0146] Step 2.4, the GO dispersion obtained above was pre-frozen at -26°C, and then freeze-dried using a freeze dryer to obtain GO powder.
[0147] Step 3, preparing magnetic material CoFe2O4 powder by hydrothermal method, specifically:
[0148] Add 0.048g CoCl2·6H2O, 0.11g FeCl3·6H2O, 0.31g urea, and 0.158g ascorbic acid powder into deionized water and stir for 30 minutes to obtain a mixed solution. Transfer the mixed solution to a high-pressure reactor and keep it at 170°C for 12 hours. Then cool it naturally to room temperature. Collect the precipitate, wash it by centrifugation, and dry it to obtain CoFe2O4 powder;
[0149] Step 4, after step 3, using a hydrothermal method and freeze drying technology to prepare a MXene / rGO / CoFe2O4 aerogel composite material; specifically:
[0150] Step 4.1, add 0.03g MXene, 0.03g rGO, and 0.042g CoFe2O4 powder into deionized water and stir for 30min to obtain a mixed solution. Move the mixed solution into a high-pressure reactor and keep it at 180℃ for 10h. Then cool it naturally to room temperature; soak the obtained aerogel in a mixed solution of water and ethanol for 24h for hydrolysis to remove excess ions; the mass ratio of water to ethanol is 10:1.
[0151] Step 4.2, the aerogel obtained above was pre-frozen at -26°C for 12 hours, and then freeze-dried at -40°C for 48 hours using a freeze dryer to obtain MXene / rGO / CoFe2O4 aerogel. The loading amount of CoFe2O4 in the aerogel was 70wt%;
[0152] Figure 1 and Figure 2 The morphology of the CoFe2O4 powder and the MXene / rGO / CoFe2O4 aerogel composite material of Example 4 are shown in Figure 2. Figure 1 and Figure 2 The successful preparation of CoFe2O4 and MXene / rGO / CoFe2O4 aerogel can be observed. Figure 2 The rich pore structure of the aerogel and the large loading of CoFe2O4 can be observed. Figure 3 This is the XPS graph of the MXene / rGO / CoFe2O4 aerogel composite. It can be observed that the MXene / rGO / CoFe2O4 aerogel was successfully prepared. The Ti 2p and F1s of MXene and the Fe 2p and Co 2p of CoFe2O4 can be clearly observed from the XPS graph of the MXene / rGO / CoFe2O4 aerogel.
[0153] like Figure 7 As shown, the minimum reflection loss of the MXene / rGO / CoFe2O4 aerogel composite material prepared in Example 4 is -71.0 dB at 2.50 mm-4.50 mm.
[0154] Example 5
[0155] The preparation method of the MXene / rGO / CoFe2O4 aerogel composite material of the present invention comprises the following specific steps:
[0156] Step 1: Prepare few-layer Ti3C2T by etching Ti3AlC2 precursor with LiF-HCl xMXene powder, the specific steps are as follows:
[0157] Step 1.1, 1 g LiF was thoroughly mixed with 20 mL 9 mol / L HCl, and then 1 g MAX phase precursor powder was slowly added under ice bath conditions;
[0158] Step 1.2, the above mixture was stirred at 35 °C for 24 h to obtain Ti3C2T x The suspension was washed repeatedly with deionized water until the pH was 7 and centrifuged at 3500 r / min;
[0159] Step 1.3, Ti3C2T x The precipitate was dispersed in 100 ml of deionized water and ultrasonically treated for 20 min to promote the delamination of multilayer MXene. Then, the precipitate was centrifuged at 3500 r / min for 5 min, and the cycle was repeated several times. The supernatant was collected to obtain a MXene dispersion.
[0160] In step 1.4, the few-layer MXene dispersion obtained above is pre-frozen at -26°C for 12 hours and then freeze-dried for 48 hours to obtain the few-layer MXene powder.
[0161] Step 2: Prepare GO powder by improving the Hummer method. The specific steps are as follows:
[0162] Step 2.1, dissolve phosphorus pentoxide (P2O5), potassium persulfate (K2S2O8) and graphite in sulfuric acid under oil bath conditions. Stir for 6 hours to mix well;
[0163] The mass ratio of P2O5, K2S2O8 and graphite is 1:1:0.75.
[0164] Step 2.2, vacuum filter the mixture and collect the precipitate. Dissolve the mixture in sulfuric acid under ice bath conditions, add 9 g potassium permanganate (KMnO 4 ). Stir for 2h to mix well;
[0165] Step 2.3, add deionized water and hydrogen peroxide (H2O2) to the solution to remove KMnO4. Add the solution to dilute hydrochloric acid and let stand for 12 hours; take the lower layer of the mixed solution and put it into water for dialysis for 48 hours. Stir the solution at high speed for 5 hours;
[0166] Step 2.4, after precooling the GO dispersion obtained above, freeze-dry it using a freeze dryer to obtain GO powder.
[0167] The precooling temperature is -31°C and the precooling time is 60 minutes;
[0168] The freeze-drying temperature was -40°C and the freeze-drying time was 72h;
[0169] Step 3, preparing magnetic material CoFe2O4 powder by hydrothermal method, specifically:
[0170] Add 0.048g CoCl2·6H2O, 0.11g FeCl3·6H2O, 0.31g urea, and 0.158g ascorbic acid powder into deionized water and stir for 30 minutes to obtain a mixed solution. Transfer the mixed solution to a high-pressure reactor and keep it at 170°C for 12 hours. Then cool it naturally to room temperature. Collect the precipitate, wash it by centrifugation, and dry it to obtain CoFe2O4 powder;
[0171] Step 4, after step 3, using a hydrothermal method and freeze drying technology to prepare a MXene / rGO / CoFe2O4 aerogel composite material; specifically:
[0172] Step 4.1, add 0.03g MXene, 0.03g rGO, and 0.054g CoFe2O4 powder into deionized water and stir for 30min to obtain a mixed solution. Move the mixed solution into a high-pressure reactor and keep it at 180℃ for 10h. Then cool it naturally to room temperature; soak the obtained aerogel in a mixed solution of water and ethanol for 24h for hydrolysis to remove excess ions; the mass ratio of water to ethanol is 10:1.
[0173] Step 4.2, the aerogel obtained above was pre-frozen at -26°C for 12 hours, and then freeze-dried at -30°C for 48 hours using a freeze dryer to obtain MXene / rGO / CoFe2O4 aerogel. The loading amount of CoFe2O4 in the aerogel was 90wt%.
[0174] like Figure 8 As shown, the minimum reflection loss of the MXene / rGO / CoFe2O4 aerogel composite material prepared in Example 5 is -17.5 dB at 2.50 mm-4.50 mm.
[0175] In summary, with the increase of CoFe2O4 content in aerogel, the electromagnetic wave absorption performance shows a trend of first increasing and then decreasing. MXene / rGO / CoFe2O4 aerogel composites show excellent electromagnetic wave absorption performance.
[0176] In the method of the present invention, a MXene / rGO / CoFe2O4 aerogel composite material is prepared. The unique design of the three-dimensional porous structure of the composite material and the effect of the magnetic component improve the impedance matching, making it easier for electromagnetic waves to enter, and multiple reflections and scattering occur in the porous structure. The incident wave is attenuated by the magnetic loss of CoFe2O4 and the interface polarization and dipole polarization induced by a large number of effective interfaces, thereby obtaining excellent electromagnetic shielding performance. When the content of CoFe2O4 in the prepared composite material in the MXene / rGO aerogel is 70wt%, the minimum reflection loss is -71.0dB. This provides a feasible solution for making materials with excellent electromagnetic wave absorption performance.
Claims
1. A method for preparing a MXene / rGO / CoFe2O4 aerogel composite material, characterized in that: Follow the steps below to implement it: Step 1, etching Ti3AlC2 precursor with LiF-HCl to prepare few-layer MXene powder; Step 2, preparing rGO powder by improved Hummer method; Step 3, preparing magnetic material CoFe2O4 powder by hydrothermal method; Step 4: After step 3, a MXene / rGO / CoFe2O4 aerogel composite material is prepared using a hydrothermal method and freeze-drying technology.
2. The method for preparing the MXene / rGO / CoFe2O4 aerogel composite material according to claim 1, characterized in that: In step 1, the specific steps are as follows: Step 1.1, LiF and HCl are fully mixed, and then MAX phase precursor powder is slowly added under ice bath conditions to obtain a mixture; Step 1.2, the mixture is stirred to obtain Ti3C2T x The suspension was then repeatedly centrifuged and washed with deionized water until the pH of the solution was 7 to obtain Ti3C2T x Sediment; Step 1.3, Ti3C2T x The precipitate was dispersed in deionized water and ultrasonically treated for 15 min to promote the delamination of multilayer MXene. Then, the centrifugation was continued for several cycles, and the supernatant was taken to obtain a few-layer MXene dispersion. Step 1.4, the few-layer MXene dispersion obtained above is pre-frozen at -26°C, and then freeze-dried using a freeze dryer to obtain a few-layer MXene powder.
3. The method for preparing the MXene / rGO / CoFe2O4 aerogel composite material according to claim 1, characterized in that: In step 2, the specific steps are as follows: Step 2.1, dissolving P2O5, K2S2O8 and graphite in sulfuric acid under oil bath conditions, stirring for 5-7 hours and mixing evenly; the mass ratio of P2O5, K2S2O8 and graphite is 0.5-1.5:0.5-1.5:0.25-1.35; Step 2.2, vacuum filter the mixture obtained in step 2.1, collect the precipitate, dissolve the mixture in sulfuric acid under ice bath conditions, add potassium permanganate in batches, stir for 1-3 hours after each addition, and mix well; Step 2.3, adding deionized water and hydrogen peroxide to the solution of step 2.2, and then adding the solution into dilute hydrochloric acid, and standing for 12-24 hours; taking the lower layer of the mixed solution and placing it into water for dialysis, the dialysis time is 48-72 hours, and after the dialysis, stirring the solution for 3-5 hours; Step 2.4, precooling the GO dispersion obtained in step 2.3, and then freeze-drying to obtain rGO powder.
4. The method for preparing the MXene / rGO / CoFe2O4 aerogel composite material according to claim 3, characterized in that: In the step 2.4, the precooling temperature is -21 to -31°C, and the precooling time is 30 to 60 minutes; the freeze-drying temperature is -30 to -40°C, and the freeze-drying time is 48 to 72 hours.
5. The method for preparing the MXene / rGO / CoFe2O4 aerogel composite material according to claim 1, characterized in that: In the step 3, specifically: CoCl2·6H2O, FeCl3·6H2O, urea and ascorbic acid powder are added to deionized water and stirred for 20-30 minutes to obtain a mixed solution. The mixed solution is transferred to a high-pressure reactor for hydrothermal reaction, cooled, and the precipitate is collected, centrifuged, washed, and dried to obtain CoFe2O4 powder.
6. The method for preparing the MXene / rGO / CoFe2O4 aerogel composite material according to claim 5, characterized in that: The reaction temperature is 170-180°C, the reaction time is 11-13h; the mass ratio of CoCl2·6H2O, FeCl3·6H2O, urea, ascorbic acid and deionized water is 0.5-1.5:1.89-2.79:2.70-3.80:6.15-6.75:3.42-4.
78.
7. The method for preparing the MXene / rGO / CoFe2O4 aerogel composite material according to claim 1, characterized in that: In the step 4, specifically: Step 4.1, adding few-layer MXene powder, rGO powder, and CoFe2O4 powder into deionized water, stirring to obtain a mixed solution, transferring the mixed solution into a high-pressure reactor, performing a hydrothermal reaction, cooling, and soaking the obtained aerogel in a mixed solution of water and ethanol for hydrolysis; Step 4.2, precooling the aerogel obtained in step 4.1, and then freeze-drying it to obtain MXene / rGO / CoFe2O4 aerogel; The precooling temperature is -21 to -31°C, and the precooling time is 30 to 60 minutes; the freeze-drying temperature is -30 to -40°C, and the freeze-drying time is 48 to 72 hours.
8. The method for preparing the MXene / rGO / CoFe2O4 aerogel composite material according to claim 7, characterized in that: In the step 4.1, the stirring time is 20-30 minutes; the mass ratio of water to ethanol is 9-11:0.5-1.5; the reaction temperature is 170-180° C., the reaction time is 9-11 hours; and the soaking time is 24-48 hours.
9. The method for preparing the MXene / rGO / CoFe2O4 aerogel composite material according to claim 7, characterized in that: In the step 4.1, the mass ratio of the few-layer MXene powder, rGO powder, CoFe2O4 powder and deionized water is 0.5-1.5: 0.5-1.5: 0.06-0.81: 1.5-4.
5.
10. The MXene / rGO / CoFe2O4 aerogel composite material prepared by the method for preparing the MXene / rGO / CoFe2O4 aerogel composite material according to any one of claims 1 to 9.
Citation Information
Cited By
MXene-based electromagnetic wave absorbing material and preparation method thereof
CN120230512A