Bio-based full-degradable comb material and preparation method thereof

By blending PLA, PBAT and PBS, and adding modified starch, mineral powder and plant composite powder, bio-based fully degraded comb material with excellent toughness and heat resistance is prepared, solving the problems of low elongation of break and poor heat resistance of existing materials at extremely low temperatures, and achieving a combination of environmental protection, degradability and high performance.

CN119529496APending Publication Date: 2025-02-28GUANGDONG ZHONGSU DEGRADABLE MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411703768.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-26
Publication Date
2025-02-28

AI Technical Summary

Technical Problem

The existing biodegradable materials have low elongation at break and poor heat resistance at extremely low temperatures, which limits their wide application.

Method used

A biobased fully degraded comb material was prepared by blending PLA, PBAT and PBS and adding modified starch, mineral powder and plant composite powder. Modified starch is prepared by blending chitosan and starch, and has excellent tensile strength and compatibility.

Benefits of technology

It improves the toughness, heat resistance and hair flexibility of bio-based fully degraded comb materials, reduces production costs, and achieves the dual advantages of environmental protection and degradability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005154036680000051
    Figure BDA0005154036680000051
  • Figure BDA0005154036680000061
    Figure BDA0005154036680000061
  • Figure BDA0005154036680000101
    Figure BDA0005154036680000101
Patent Text Reader

Abstract

The invention discloses a bio-based fully-degradable comb material and a preparation method thereof. The comb material comprises the following raw materials in parts by weight: 55-75 parts of PLA, 5-15 parts of PBAT, 5-15 parts of PBS, 15-20 parts of modified starch, 5-15 parts of mineral powder, 4-10 parts of plant composite powder, 0.3-1 part of a lubricant and 0.5-0.8 part of a compatilizer. The bio-based fully-degradable comb material can be fully degraded into water and carbon dioxide in the natural environment, does not cause secondary pollution to the environment, and is more environment-friendly and degradable; a biological base is selected for preparing the comb, natural resources can be better recycled, and use of petroleum resources is reduced; by adding the plant powder, the hair can be effectively maintained, and the flexibility and smoothness of the hair can be improved, so that the comb is endowed with an application additional value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a bio-based fully degradable comb material and a preparation method thereof. Background Art

[0002] Most of the raw materials of traditional polymer materials come from petroleum, and the discard of non-explainable polymer material products, especially disposable packaging, will cause great harm to the environment. At the same time, the large-scale use of petroleum-based polymer materials is also a huge challenge for non-renewable petroleum resources. With the increasing pollution of plastic products to the environment, environmental protection is imminent, and many countries and regions have introduced very strict "plastic restriction" and "plastic ban" related policies. Considering environmental protection and related policies, the application of biodegradable materials will become more and more extensive, the demand will become greater and greater, and the biodegradable materials industry has a bright future.

[0003] Polylactic acid (PLA), also known as polylactide, is a polyester polymer obtained by polymerization with lactic acid as the main raw material. It is a new type of biodegradable material. Compared with traditional petroleum-based polymer materials, its raw materials are widely available and can be extracted from renewable resources such as corn and starch. After being discarded, it can be completely degraded into water and carbon dioxide under the action of microorganisms in nature without causing any pollution to the environment. It has excellent biocompatibility, high strength, high hardness and processability, and is considered to be one of the most promising biodegradable materials. However, its high brittleness, poor heat resistance, and especially its extremely low elongation at break limit its wide application.

[0004] Polybutylene adipate / terephthalate (PBAT) is a copolymer of butylene adipate and butylene terephthalate. It has good ductility and elongation at break, as well as good heat resistance and impact properties. In addition, it has excellent biodegradability and is one of the most popular and widely used biodegradable materials.

[0005] Polybutylene succinate (PBS), also known as polybutylene succinate, is a biodegradable polyester polymer material made of aliphatic dibasic acids and diols. It can be obtained from the fermentation of agricultural biomass containing glucose, cellulose, etc., or from traditional petroleum resources. In addition to being biodegradable, it also has good biocompatibility, excellent heat resistance, processability and high elongation at break. It is considered to be a type of biodegradable material with a promising future in packaging and other fields.

[0006] Melting PLA and PBAT together can effectively alleviate the brittleness of PLA, but the temperature resistance of the two after melting is low; adding PBS to the blend of PLA and PBAT, the composite material prepared by melting the three has excellent mechanical properties and heat resistance, but the compatibility between the three is poor and the cost is high. Therefore, the composite material obtained has defects such as bubbles, uneven distribution of components, and poor mechanical properties. Summary of the invention

[0007] In view of this, the purpose of the present invention is to overcome the problems existing in the prior art and provide a bio-based fully degradable comb material, which can be fully degraded into water and carbon dioxide in the natural environment, will not cause secondary pollution to the environment, and is more environmentally friendly and degradable; the use of bio-based materials to prepare combs can better recycle natural resources and reduce the use of petroleum resources; by adding plant powder, hair can be effectively maintained, the softness and smoothness of hair can be improved, thereby giving the comb added value in application

[0008] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0009] A bio-based fully degradable comb material comprises the following raw materials in parts by weight: 55-75 parts of PLA, 5-15 parts of PBAT, 5-15 parts of PBS, 15-20 parts of modified starch, 5-15 parts of mineral powder, 4-10 parts of plant composite powder, 0.3-1 parts of lubricant and 0.5-0.8 parts of compatibilizer.

[0010] The bio-based fully degradable comb material of the present invention uses PLA as a base resin. PLA has good biocompatibility and biodegradability, but poor heat resistance and impact strength. PBAT has excellent toughness, and PBS has excellent impact strength and elongation at break. PBAT and PBS are added to blend with PLA to improve the toughness and heat resistance of the bio-based fully degradable comb material. Modified starch with excellent compatibility and biodegradability is added to improve the toughness and mechanical properties of the bio-based fully degradable comb material on the one hand, and the amount of mineral powder used on the other hand, thereby improving the compatibility of the bio-based fully degradable comb material. The addition of mineral powder can improve the crystallinity of PLA, and improve the crystallization ability and heat resistance of the bio-based fully degradable comb material. The addition of plant composite powder enables the bio-based fully degradable comb material to have the additional effects of maintaining hair and improving the softness and smoothness of hair.

[0011] Preferably, the modified starch is prepared by the following steps: 1) dissolving starch in distilled water, stirring to completely dissolve, and obtaining a starch solution with a mass percentage of 3-5%; 2) dissolving chitosan in a 1-2% acetic acid solution, stirring to completely dissolve, and obtaining a chitosan solution with a mass percentage of 3-5%; 3) mixing the starch solution and the chitosan solution in a mass ratio of 3-10:2-5, and then adding a plasticizer to the mixed solution, and blending in a water bath to obtain the modified starch.

[0012] Preferably, the starch is selected from one or more of acetylated starch and hydroxypropylated starch, and the plasticizer is one or more of glycerol, sorbitol, and glucose, and the amount of the plasticizer added is 5-8% of the weight of the mixed solution. Starch is a degradable natural polymer material, and chitosan has good biocompatibility and biodegradability. Starch and chitosan are blended, and the starch and chitosan are combined in the form of chemical bonding. The prepared modified starch has excellent tensile strength, biodegradability, compatibility and mechanical properties. Adding the modified starch to the PLA base resin can promote the crystallization of the PLA base resin and effectively improve the mechanical properties of the bio-based fully degradable comb material. At the same time, starch can absorb excess oil from the hair. Adding it to the bio-based fully degradable comb material and using the prepared comb to comb the hair can make the hair fluffy, refreshing, soft and smooth.

[0013] More preferably, the starch is a mixture of acetylated starch and hydroxypropylated starch in a weight ratio of 1-5:3-5. Acetylated starch is generated by reacting starch with acetyl liver under the action of an alkaline catalyst, using acetyl groups to replace part of the hydroxyl groups in the starch. Adding acetylated starch to the PLA base resin can improve the toughness of PLA and improve the elongation at break of the bio-based fully degradable comb material; hydroxypropylated starch is generated by reacting starch with propylene oxide, using hydroxypropyl groups to destroy the hydrogen bonds in the starch, and adding hydroxypropylated starch to the PLA base resin can improve the mechanical properties of PLA. At the same time, the ether groups in the hydroxypropylated starch can react with the ester groups in the PLA to form hydrogen bonds, thereby enhancing the interfacial interaction force and improving the compatibility between the modified starch and the PLA.

[0014] Preferably, the mineral powder is selected from one or more of talc, montmorillonite, kaolin, calcium carbonate, and barium sulfate. The addition of mineral powder can reduce the production cost of bio-based fully degradable comb materials, and can also improve the processability and high temperature resistance of bio-based fully degradable comb materials. Mineral powder is an inorganic material, and the compatibility between inorganic materials and PLA base resin is poor. By adding modified starch, the compatibility between modified starch and PLA base resin is better. Modified starch can also be used as a filler to replace part of the mineral powder, thereby solving the problem of poor interface compatibility between raw materials.

[0015] Preferably, the plant composite powder is selected from one or more of angelica powder, Polygonum multiflorum powder, Platycladus orientalis leaf powder, and Gleditsia sinensis powder. More preferably, the plant composite powder is a mixture of angelica powder, Polygonum multiflorum powder, Platycladus orientalis leaf powder, and Gleditsia sinensis powder in a weight ratio of 1-5:2-8:1-5:3-5. Angelica has the effect of enhancing hair toughness and reducing hair loss; Polygonum multiflorum has the effect of nourishing hair, strengthening hair growth, and inhibiting dandruff; Platycladus orientalis leaf has the effect of relieving itching, promoting hair growth, and darkening hair; Gleditsia sinensis has the effect of deep cleansing hair and improving hair quality; the plant composite powder

[0016] Preferably, the lubricant is selected from one or more of stearic acid, pentaerythritol stearate, and ethylene bis stearamide. By adding the lubricant, the processing fluidity between the raw materials can be improved, the melting rate of the bio-based fully degradable comb material can be accelerated, and the mechanical properties of the bio-based fully degradable comb material can be improved.

[0017] Preferably, the compatibilizer is selected from one or more of maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, maleic anhydride grafted SEBS, maleic anhydride grafted PBS, and maleic anhydride grafted POE. By adding the compatibilizer, the interfacial compatibility between the mineral powder and PLA is improved, the fluidity and toughness of the bio-based fully degradable comb material are improved, and the brittleness and strength problems of the PLA base resin are solved.

[0018] The present invention also provides a method for preparing a bio-based fully degradable comb material, comprising the following steps:

[0019] (1) Adding PLA, PBAT and PBS according to weight parts into a stirring device and mixing them evenly to obtain a first mixed material for later use;

[0020] (2) adding the first mixed material, modified starch, mineral powder, plant composite powder, lubricant and compatible powder into a stirring device according to weight parts, mixing them evenly to obtain a second mixed material for standby use;

[0021] (3) adding the second mixed material into an extruder, and performing melt extrusion and granulation to obtain a bio-based fully degradable comb material.

[0022] Preferably, in step (1), the stirring rate is 150-250 r / min, and the stirring time is 2-4 min; in step (2), the stirring rate is 200-300 r / min, and the stirring time is 3-5 min.

[0023] Preferably, in step (3), the melting temperature is 160-180°C.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. Compared with ordinary plastic combs, the bio-based fully degradable comb material provided by the present invention can be completely degraded into water and carbon dioxide in the natural environment, will not cause secondary pollution to the environment, and is more environmentally friendly and degradable; the use of bio-based materials to prepare combs can better recycle natural resources and reduce the use of petroleum resources; by adding plant powder, it can effectively maintain hair and improve the softness and smoothness of hair, thereby giving the comb added value.

[0026] 2. The bio-based fully degradable comb material provided by the present invention uses PLA as the base resin, and adds PBAT and PBS for blending, which effectively improves the brittleness of the PLA base resin, so that the prepared bio-based fully degradable comb material has excellent toughness; modified starch is added, and the excellent toughness and biodegradability of the modified starch are utilized, so that the prepared bio-based fully degradable comb material has improved toughness while maintaining biodegradability; at the same time, starch can absorb oil, and the plant composite powder has the function of maintaining hair, which gives the bio-based fully degradable comb material the function of nourishing hair.

[0027] 3. The preparation method of the bio-based fully degradable comb material provided by the present invention has simple steps, is easy to operate, has low raw material cost, is easily available, and can be industrialized for production. DETAILED DESCRIPTION

[0028] In order to facilitate understanding by those skilled in the art, the present invention is further described below with reference to the embodiments, but the contents mentioned in the embodiments are not intended to limit the present invention.

[0029] The main raw materials used in the embodiments of the present invention are from:

[0030]

[0031]

[0032] Example 1

[0033] A bio-based fully degradable comb material comprises the following raw materials in parts by weight: 55 parts of PLA, 5 parts of PBAT, 5 parts of PBS, 15 parts of modified starch, 5 parts of mineral powder, 4 parts of plant composite powder, 0.3 parts of lubricant and 0.5 parts of compatibilizer.

[0034] The modified starch is prepared by the following steps: 1) dissolving starch in distilled water, stirring to completely dissolve, and obtaining a starch solution with a mass percentage of 3%; 2) dissolving chitosan in a 1% acetic acid solution, stirring to completely dissolve, and obtaining a chitosan solution with a mass percentage of 3%; 3) mixing the starch solution and the chitosan solution in a mass ratio of 3:2, then adding a plasticizer to the mixed solution, and blending them in a water bath to obtain the modified starch.

[0035] The starch is a mixture of acetylated starch and hydroxypropylated starch in a weight ratio of 1:3, and the plasticizer is glycerol. The amount of the plasticizer added is 5% of the weight of the mixed solution.

[0036] The mineral powder is talcum powder.

[0037] The plant composite powder is a mixture of angelica powder, polygonum multiflorum powder, arborvitae leaf powder and sapodilla powder in a weight ratio of 1:2:1:3.

[0038] The lubricant is stearic acid.

[0039] The compatibilizer is maleic anhydride grafted polyethylene.

[0040] The method for preparing the above-mentioned bio-based fully degradable comb material comprises the following steps:

[0041] (1) Adding PLA, PBAT and PBS according to weight into a stirring device, mixing evenly to obtain a first mixed material for later use;

[0042] (2) adding the first mixed material, modified starch, mineral powder, plant composite powder, lubricant and compatible powder into a stirring device according to weight parts, mixing them evenly to obtain a second mixed material for standby use;

[0043] (3) adding the second mixed material into an extruder, and performing melt extrusion and granulation to obtain a bio-based fully degradable comb material.

[0044] In the step (1), the stirring rate is 150 r / min and the stirring time is 2 min; in the step (2), the stirring rate is 200 r / min and the stirring time is 3 min.

[0045] In the step (3), the melting temperature is 160°C.

[0046] Example 2

[0047] A bio-based fully degradable comb material comprises the following raw materials in parts by weight: 75 parts of PLA, 15 parts of PBAT, 15 parts of PBS, 20 parts of modified starch, 15 parts of mineral powder, 10 parts of plant composite powder, 1 part of lubricant and 0.8 parts of compatibilizer.

[0048] The modified starch is prepared by the following steps: 1) dissolving starch in distilled water, stirring to completely dissolve, and obtaining a starch solution with a mass percentage of 5%; 2) dissolving chitosan in a 2% acetic acid solution, stirring to completely dissolve, and obtaining a chitosan solution with a mass percentage of 5%; 3) mixing the starch solution and the chitosan solution in a mass ratio of 10:5, and then adding a plasticizer to the mixed solution, and blending them in a water bath to obtain the modified starch.

[0049] The starch is a mixture of acetylated starch and hydroxypropylated starch in a weight ratio of 5:5, and the plasticizer is sorbitol, and the added amount of the plasticizer is 8% of the weight of the mixed solution.

[0050] The mineral powder is selected from montmorillonite.

[0051] The plant composite powder is a mixture of angelica powder, polygonum multiflorum powder, arborvitae leaf powder and sapodilla powder in a weight ratio of 5:8:5:5.

[0052] The lubricant is pentaerythritol stearate.

[0053] The compatibilizer is maleic anhydride grafted polypropylene.

[0054] The method for preparing the above-mentioned bio-based fully degradable comb material comprises the following steps:

[0055] (1) Adding PLA, PBAT and PBS according to weight parts into a stirring device and mixing them evenly to obtain a first mixed material for later use;

[0056] (2) adding the first mixed material, modified starch, mineral powder, plant composite powder, lubricant and compatible powder into a stirring device according to weight parts, mixing them evenly to obtain a second mixed material for standby use;

[0057] (3) adding the second mixed material into an extruder, and performing melt extrusion and granulation to obtain a bio-based fully degradable comb material.

[0058] In the step (1), the stirring rate is 250 r / min and the stirring time is 4 min; in the step (2), the stirring rate is 300 r / min and the stirring time is 5 min.

[0059] In the step (3), the melting temperature is 180°C.

[0060] Example 3

[0061] A bio-based fully degradable comb material comprises the following raw materials in parts by weight: 65 parts of PLA, 10 parts of PBAT, 10 parts of PBS, 18 parts of modified starch, 10 parts of mineral powder, 7 parts of plant composite powder, 0.6 parts of lubricant and 0.7 parts of compatibilizer.

[0062] The modified starch is prepared by the following steps: 1) dissolving starch in distilled water, stirring to completely dissolve, and obtaining a starch solution with a mass percentage of 4%; 2) dissolving chitosan in a 1.5% acetic acid solution, stirring to completely dissolve, and obtaining a chitosan solution with a mass percentage of 4%; 3) mixing the starch solution and the chitosan solution in a mass ratio of 7:4, then adding a plasticizer to the mixed solution, and blending them in a water bath to obtain the modified starch.

[0063] The starch in this embodiment is a mixture of acetylated starch and hydroxypropylated starch in a weight ratio of 3:4, and the plasticizer is glucose, and the amount of the plasticizer added is 6% of the weight of the mixed solution.

[0064] The mineral powder is kaolin.

[0065] The plant composite powder is a mixture of angelica powder, polygonum multiflorum powder, arborvitae leaf powder and sapodilla powder in a weight ratio of 3:5:3:4.

[0066] The lubricant is ethylene bis stearamide.

[0067] The compatibilizer is maleic anhydride grafted SEBS.

[0068] The method for preparing the above-mentioned bio-based fully degradable comb material comprises the following steps:

[0069] (1) Adding PLA, PBAT and PBS according to weight into a stirring device, mixing evenly to obtain a first mixed material for later use;

[0070] (2) adding the first mixed material, modified starch, mineral powder, plant composite powder, lubricant and compatible powder into a stirring device according to weight parts, mixing them evenly to obtain a second mixed material for standby use;

[0071] (3) adding the second mixed material into an extruder, and performing melt extrusion and granulation to obtain a bio-based fully degradable comb material.

[0072] In the step (1), the stirring rate is 200 r / min and the stirring time is 3 min; in the step (2), the stirring rate is 250 r / min and the stirring time is 4 min.

[0073] In the step (3), the melting temperature is 170°C.

[0074] Example 4

[0075] The difference between this embodiment and embodiment 3 is that the starch in this embodiment is acetylated starch.

[0076] Example 5

[0077] The difference between this embodiment and embodiment 3 is that the starch in this embodiment is hydroxypropylated starch.

[0078] Comparative Example 1

[0079] The difference between this comparative example and Example 3 is that no PBS is added in this comparative example.

[0080] Comparative Example 2

[0081] The difference between this comparative example and Example 3 is that PBAT is not added in this comparative example.

[0082] Comparative Example 3

[0083] The difference between this comparative example and Example 3 is that the starch in this comparative example is not modified by chitosan.

[0084] The bio-based fully degradable comb materials prepared in Examples 1-5 and Comparative Examples 1-3 were subjected to performance tests:

[0085] 1. Density: The density of the bio-based fully degradable comb materials prepared in Examples 1-5 and Comparative Examples 1-3 was measured according to ASTM D792, and the test results are recorded in Table 1 below;

[0086] 2. Melt index: The melt index of the bio-based fully degradable comb materials prepared in Examples 1-5 and Comparative Examples 1-3 was measured according to ASTM D1238, and the test results are recorded in Table 1 below;

[0087] 3. Tensile strength: The tensile strength of the bio-based fully degradable comb materials prepared in Examples 1-5 and Comparative Examples 1-3 was measured according to ASTM D638, and the test results are recorded in Table 1 below;

[0088] 4. Elongation: The elongation of the bio-based fully degradable comb materials prepared in Examples 1-5 and Comparative Examples 1-3 was measured according to ASTM D638, and the test results are recorded in Table 1 below;

[0089] 5. Notched impact strength: The notched impact strength of the bio-based fully degradable comb materials prepared in Examples 1-5 and Comparative Examples 1-3 was measured according to ASTM D256. The test results are recorded in Table 1.

[0090] Table 1 Performance test results of bio-based fully degradable comb materials

[0091]

[0092]

[0093] It can be seen from Table 1 that the bio-based fully degradable comb materials prepared in Examples 1-5 have excellent mechanical properties, with a tensile strength of 52.22-63.24 MPa, an elongation of 75-95%, and a notched impact strength of 7.1-8.2 J / m; this indicates that the present invention uses PLA as a base resin, adds PBS, PBAT and modified starch to modify PLA, improves the brittleness and poor heat resistance of PLA, and makes the prepared bio-based fully degradable comb material have good toughness, the brittle fracture of the PLA base resin is transformed into a tough fracture, and the elongation and notched impact strength of the bio-based fully degradable comb material are improved.

[0094] By comparing Example 3, Example 4 and Example 5, it can be seen that Example 3 uses a compound acetylated starch and hydroxypropylated starch, Example 4 uses a single acetylated starch, and Example 5 uses a single hydroxypropylated starch. The toughness, elongation and notched impact strength of the bio-based fully degradable comb material prepared in Example 3 are better than those of the bio-based fully degradable comb materials prepared in Example 4 and Example 5; it shows that the present invention uses a compound acetylated starch and hydroxypropylated starch, the acetylated starch can improve the ductility of the PLA base resin, and the hydroxypropylated starch can improve the elongation at break of the PLA base resin. The combination of the two starches can ultimately improve the comprehensive performance of the PLA base resin, and ultimately the prepared bio-based fully degradable comb material has excellent toughness, elongation and notched impact strength.

[0095] By comparing Example 3 and Comparative Example 1, it can be seen that the bio-based fully degradable comb material prepared in Comparative Example 1 does not add PBS, and the mechanical properties such as toughness and tensile strength of the prepared bio-based fully degradable comb material are greatly reduced; because the PBS main chain contains a large number of non-polar methylene structures and ester bonds, it has good compatibility, can reduce the intermolecular interaction force between PLA and PBAT, and improve the tensile strength of the bio-based fully degradable comb material. At the same time, PBS is a crystalline substance, and the crystal agglomeration of PBS will show separation phenomenon, indicating that the addition of PBS can reduce the elongation at break and notched impact strength of the bio-based fully degradable comb material.

[0096] By comparing Example 3 and Comparative Example 2, it can be seen that the bio-based fully degradable comb material prepared in Comparative Example 2 does not add PBAT, which greatly reduces the mechanical properties of the bio-based fully degradable comb material, such as toughness, elongation and notched impact strength; because PBAT and PLA are both highly polar polymers, PBAT and PLA have similar compatibility, PBAT and PLA have good compatibility, and PBAT has good ductility and elongation at break. The addition of PBAT can effectively alleviate the brittleness of the PLA base resin, so that the prepared bio-based fully degradable comb material has good toughness, elongation and notched impact strength.

[0097] From the comparison between Comparative Example 1 and Comparative Example 2, it can be seen that the addition of PBS and PBAT to the bio-based fully degradable comb material can improve the toughness of the PLA base resin, so that the toughness, elongation and notched impact strength of the prepared bio-based fully degradable comb material are increased; PBS is a weakly polar copolyester, and PBAT is a triblock strongly polar copolyester. The melting point of PBS is quite different from that of PLA, and the melting point of PBAT is close to that of PLA. According to similar compatibility, PLA and PBAT have good compatibility, and PLA and PBS have poor compatibility. In addition, PBAT has flexible segments and benzene ring groups on its molecular chain, and the volume of the benzene ring is large. When PBAT is added to blend with PLA, PBAT is embedded in the PLA molecular chain, which increases the space of the PLA molecular chain and makes it easier for PLA molecules to move. Therefore, compared with the addition of PBS to toughen PLA, the addition of PBAT to toughen PLA, the tensile strength, elongation and notched impact strength of the prepared bio-based fully degradable comb material have a larger change range.

[0098] By comparing Example 3 and Comparative Example 3, it can be seen that the starch in the bio-based fully degradable comb material prepared in Comparative Example 3 has not been modified with chitosan, and the toughness and other mechanical properties of the prepared bio-based fully degradable comb material are reduced; this indicates that the present invention uses chitosan and starch for blending, and the starch and chitosan are combined in the form of chemical bonding. The prepared modified starch has excellent tensile strength, biodegradability, compatibility and mechanical properties. Adding the modified starch to the PLA base resin can promote the crystallization of the PLA base resin and effectively improve the mechanical properties of the bio-based fully degradable comb material.

[0099] The bio-based fully degradable comb material prepared in Examples 1-5 was made into a comb by foaming molding, and 10 subjects were invited to use the prepared bio-based fully degradable comb. All the subjects had problems with greasy and frizzy hair to varying degrees; among them, 8 subjects believed that the bio-based fully degradable comb was comfortable to hold, the material was not easy to deform or break, the combed hair did not generate static electricity, and the hair was not easy to pull.

[0100] The technical solutions provided by the embodiments of the present invention are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the embodiments of the present invention. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present invention. At the same time, for those skilled in the art, according to the embodiments of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A bio-based fully degradable comb material, characterized by: The invention comprises the following raw materials in parts by weight: 55-75 parts of PLA, 5-15 parts of PBAT, 5-15 parts of PBS, 15-20 parts of modified starch, 5-15 parts of mineral powder, 4-10 parts of plant composite powder, 0.3-1 parts of lubricant and 0.5-0.8 parts of compatibilizer.

2. The bio-based fully degradable comb material according to claim 1, characterized in that: The modified starch is prepared by the following steps: 1) dissolving starch in distilled water, stirring to completely dissolve, and obtaining a starch solution with a mass percentage of 3-5%; 2) dissolving chitosan in an acetic acid solution with a mass percentage of 1-2%, stirring to completely dissolve, and obtaining a chitosan solution with a mass percentage of 3-5%; 3) mixing the starch solution and the chitosan solution in a mass ratio of 3-10:2-5, and then adding a plasticizer to the mixed solution, blending in a water bath condition, and obtaining the modified starch.

3. The bio-based fully degradable comb material according to claim 1, characterized in that: The starch is selected from one or more of acetylated starch and hydroxypropylated starch, the plasticizer is one or more of glycerol, sorbitol and glucose, and the added amount of the plasticizer is 5-8% of the weight of the mixed solution.

4. The bio-based fully degradable comb material according to claim 2, characterized in that: The mineral powder is selected from one or more of talc, montmorillonite, kaolin, calcium carbonate and barium sulfate.

5. The bio-based fully degradable comb material according to claim 1, characterized in that: The plant composite powder is selected from one or more of angelica powder, polygonum multiflorum powder, arborvitae leaf powder and sapodilla powder.

6. The bio-based fully degradable comb material according to claim 1, characterized in that: The lubricant is selected from one or more of stearic acid, pentaerythritol stearate, and ethylene bisstearamide.

7. The bio-based fully degradable comb material according to claim 1, characterized in that: The compatibilizer is selected from one or more of maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, maleic anhydride grafted SEBS, maleic anhydride grafted PBS, and maleic anhydride grafted POE.

8. A method for preparing a bio-based fully degradable comb material according to any one of claims 1 to 7, characterized in that: The steps include: (1) Adding PLA, PBAT and PBS according to weight into a stirring device, mixing evenly to obtain a first mixed material for later use; (2) adding the first mixed material, modified starch, mineral powder, plant composite powder, lubricant and compatible powder into a stirring device according to weight parts, mixing them evenly to obtain a second mixed material for standby use; (3) adding the second mixed material into an extruder, and performing melt extrusion and granulation to obtain a bio-based fully degradable comb material.

9. The method for preparing a bio-based fully degradable comb material according to claim 8, characterized in that: In the step (1), the stirring rate is 150-250 r / min, and the stirring time is 2-4 min; in the step (2), the stirring rate is 200-300 r / min, and the stirring time is 3-5 min.

10. The method for preparing a bio-based fully degradable comb material according to claim 8, characterized in that: In the step (3), the melting temperature is 160-180°C.