RGO / g-C3N4atAuNPs nano composite material as well as preparation method and application of rGO / g-C3N4atAuNPs nano composite material
By modifying the electrodes by using reduced graphene oxide/graphite phase carbon nitride/gold nanoparticle composite electrode materials, the complex, time-consuming and cost-effective detection of nitrite ion in the prior art is solved, and the electrochemical detection effect is achieved with high sensitivity and selectivity.
Patent Information
- Application Number
- CN202411731291.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-29
- Publication Date
- 2025-03-07
AI Technical Summary
The prior art has problems such as long recognition time, complexity and cumbersomeness, high cost, low sensitivity and insignificant recognition effect when detecting nitrite ions.
The nanocomposite material was prepared by reducing graphene oxide/graphite phase carbon nitride/gold nanoparticles (rGO/g-C3N4@AuNPs) by ultrasonic treatment and magnetic stirring, and modified on the glass carbon electrode for electrochemical detection of nitrite ions.
It realizes high sensitivity detection of nitrite ions, which has the advantages of good selectivity, simplicity and low cost, and significantly improves detection efficiency and accuracy.
Smart Images

Figure CN119569044A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a nanocomposite material, and in particular to a reduced graphene oxide / graphite phase carbon nitride / gold nanoparticle (rGO / g-C3N4@AuNPs) composite electrode material and a preparation method thereof, and application of the material in electrochemical detection of nitrite in food samples. Background Art
[0002] Nitrite (NO2 - ) is a chemical substance widely used in daily life and the food industry. In my country, nitrite is widely used in the processing of cooked meat products, fish, vegetables and other foods to extend the shelf life of food and improve the color and taste of food. However, the impact of nitrite on human health has also attracted widespread attention. Long-term exposure to excessive nitrite can cause great harm to human health. It can even have adverse effects on unborn babies. Therefore, it is very important to accurately detect nitrite ions in water. At present, there are some methods for determining NO2 - Although these methods have certain accuracy, they have problems such as complex process and high cost. On the contrary, electrochemical technology has the advantages of high sensitivity, fast response speed and easy detection.
[0003] Gold nanoparticles refer to tiny colloidal gold particles with a diameter between 0.8 and 250 nm. In electrochemical biosensors, they can be used as electrode modification materials due to their good biocompatibility and excellent conductivity. The simplest method is the sodium citrate reduction method. After the preparation, the citrate on the gold nanoparticles will also prevent them from aggregating, thereby maintaining the particle size of the gold nanoparticles for a long time.
[0004] Reduced graphene oxide (rGO) is a reduction product of graphene oxide, which retains some of the oxygen-containing functional groups of graphene oxide, making it easy to modify with other reagents and biomolecules, enhancing conductivity and thus having better electrochemical performance. Therefore, reduced graphene oxide is an ideal material for electrochemical biosensors.
[0005] Graphite carbon nitride is rich in electrons and is nucleophilic as a whole, but its conductivity is low. To use graphite carbon nitride in electrochemical sensors, it needs to be modified. Reduced graphene oxide is one of its ideal modified materials. Studies have shown that there is a synergistic effect between reduced graphene oxide and graphite carbon nitride in terms of electrochemical performance to improve the overall conductivity of the composite material. The combination of the two will further increase the specific surface area of the material and provide more sites for modifying and binding biomolecules. In addition, gold nanoparticles doped in graphite carbon nitride can shorten the electron transmission path, improve conductivity, and enhance the overall stability of the nanomaterial composite. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a reduced graphene oxide / graphitic carbon nitride / gold nanoparticle (rGO / g-C3N4@AuNPs) composite electrode material and electrochemically detecting nitrite ions thereof, so as to solve the technical problems existing in the prior art such as long and complicated recognition time, high cost, low sensitivity and unclear recognition effect.
[0007] The present invention is achieved through the following technical solution: A method for preparing a composite material, comprising the following steps:
[0008] 1) Preparation of GO / g-C3N4:
[0009] 40-60 mg (preferably 50 mg) of graphene oxide (GO) is ultrasonically treated in 50-70 mL (preferably 50 mL) of deionized water for 5-8 hours (preferably 8 hours) to obtain a graphene oxide suspension; 80-100 mg (preferably 100 mg) of graphite phase carbon nitride is ultrasonically treated in 80-100 mL (preferably 100 mL) of deionized water for 24-30 hours (preferably 24 hours), centrifuged at 3000-5000 rpm for 15-30 minutes (preferably 30 minutes), and the supernatant is collected to obtain a g-C3N4 nanosheet suspension; 5-10 mL (preferably 5 mL) of the graphene oxide suspension is ultrasonically mixed with 50-60 mL (preferably 50 mL) of the g-C3N4 nanosheet suspension for 10-12 hours (preferably 12 hours) to obtain a g-C3N4@GO suspension;
[0010] 2) Preparation of rGO / g-C3N4@AuNPs:
[0011] 150-300 μL (preferably 200 μL) of ammonia water and 20-40 μL (preferably 25 μL) of hydrazine hydrate are added to the above g-C3N4@GO suspension, ultrasonically treated for 0.5-1.5 hours, and magnetically stirred at 90-110°C for 4-6 hours (preferably 5 hours) to obtain a g-C3N4@rGO suspension; 90-110 μL (preferably 100 μL) of 0.1 M chloroauric acid solution is added to the g-C3N4@rGO suspension, ultrasonically treated for 20-30 minutes (preferably 25 minutes), and continuously stirred at 85°C; 0.8-1 mL of 0.08 M NaBH4 solution and 180-200 μL of 0.01 M sodium citrate solution were continuously stirred for 20-30 min, and centrifuged at 6000-8000 rpm for 3-5 times to obtain rGO / g-C3N4@AuNPs nanocomposite materials.
[0012] A method for detecting nitrite using rGO / g-C3N4@AuNPs nanocomposite material comprises the following steps:
[0013] 1) Preparation and electrochemical characterization of rGO / g-C3N4@AuNPs modified electrode:
[0014] The prepared rGO / g-C3N4@AuNPs nanocomposite material was dissolved in a mixture of ethanol and water, and ultrasonically treated to prepare a 1 mg / mL suspension. The rGO / g-C3N4@AuNPs suspension was then drop-coated on the surface of a glassy carbon electrode and dried to obtain a rGO / g-C3N4@AuNPs modified electrode. The electrode was immersed in a solution containing 0.1 M KCl, 5 mM [Fe(CN)6] 3- / 4- In the mixed solution, electrochemical impedance spectroscopy (EIS) and cyclic voltammetry (CV) were performed, and the rGO / g-C3N4@AuNPs modified electrode showed low electrochemical impedance value and high peak current;
[0015] 2) Electrochemical detection of nitrite ions:
[0016] The rGO / g-C3N4@AuNPs modified electrode was immersed in 2 mM NO2 - The current response signal of DPV was measured in PBS buffer with pH = 4.0 to determine the effect of NO2 - Whether there is response and response effect. It was found that rGO / g-C3N4@AuNPs modified electrode can respond to NO2 - Electrochemical detection was performed and showed high selectivity.
[0017] 3) Electrochemical detection of nitrite ions in food samples:
[0018] After simple pretreatment of the food samples, the supernatant was collected and fixed to 10 mL with 0.1 M pH = 4 PBS buffer. The rGO / g-C3N4@AuNPs modified electrode was inserted into the 0.1 M pH = 4.0 PBS buffer containing the actual sample. The NO2 in the sample was measured according to the standard addition method. - Conduct testing.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The rGO / g-C3N4@AuNPs nanocomposite prepared by the present invention, wherein rGO is an ideal material for electrochemical biosensors, and there is a synergistic effect between reduced graphene oxide and graphite phase carbon nitride in electrochemical performance that can improve the overall conductivity of the composite material, and AuNPs have excellent electrocatalytic performance and biocompatibility that can enhance the stability of the nanomaterial composite. This nanocomposite material for NO2 - The new electrochemical sensor used for detection has the characteristics of high sensitivity, good selectivity, simplicity and ease of use, and is superior to other detection methods.
[0021] (2) The NO2 - The present invention provides the electrochemical behavior of rGO / g-C3N4@AuNPs on the surface of modified electrode to detect NO2 in food samples by electrochemical method. - This will play an important role in the analysis and research of electrochemical sensors. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 SEM images, (A) g-C3N4, (B) rGO / g-C3N4, (C) rGO / g-C3N4@AuNPs, (D) TEM of rGO / g-C3N4@AuNPs.
[0023] Figure 2 Infrared spectra of GO, g-C3N4, rGO / g-C3N4, and rGO / g-C3N4@AuNPs.
[0024] Figure 3 XPS graphs: (A) XPS graph of rGO / g-C3N4@AuNPs; (B) XPS graphs of GO, (C) rGO / g-C3N4, (D) C1s of rGO / g-C3N4@AuNPs and (E) Au4f;
[0025] Figure 4 For bare glassy carbon electrode, rGO modified electrode, rGO / g-C3N4 modified electrode, rGO / g-C3N4@AuNPs modified electrode in [Fe(CN)6] 3- / 4- Electrochemical impedance spectroscopy (A), cyclic voltammogram (B) and its electrochemical performance in NO2 - Differential pulse voltammogram in solution (C).
[0026] Figure 5 Cyclic voltammograms at different scan rates (A) (the inset is its linear graph) and differential pulse voltammograms at different pH (B), enrichment time (C), and modification volume (D).
[0027] Figure 6 For different concentrations of NO2 - The detected DPV graph (A) and its linear graph (B).
[0028] Figure 7 When there is an interfering substance, rGO / g-C3N4@AuNPs has a strong affinity for NO2 - Current response diagram. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below with reference to the examples, but the examples do not limit the protection scope of the present invention.
[0030] Embodiment 1:
[0031] A method for preparing a rGO / g-C3N4@AuNPs nanocomposite material comprises the following steps:
[0032] 1) Preparation of GO / g-C3N4:
[0033] 50 mg of graphene oxide (GO) was ultrasonically treated in 50 mL of deionized water for 8 hours to obtain a graphene oxide suspension; 100 mg of graphite phase carbon nitride was ultrasonically treated in 100 mL of deionized water for 24 hours, centrifuged at 5000 rpm for 30 minutes, and the supernatant was collected to obtain a g-C3N4 nanosheet suspension. 5 mL of the graphene oxide suspension was ultrasonically mixed with 50 mL of the g-C3N4 nanosheet suspension for 12 hours to obtain a g-C3N4@GO suspension;
[0034] 2) Preparation of rGO / g-C3N4@AuNPs:
[0035] 200 μL of ammonia water and 25 μL of hydrazine hydrate were added to the above g-C3N4@GO suspension, ultrasonically treated for 1 hour, and magnetically stirred at 100°C for 5 hours to obtain g-C3N4@rGO suspension; 100 μL of 0.1 M chloroauric acid solution was added to the g-C3N4@rGO suspension, ultrasonically treated for 25 minutes, and continuously stirred at 85°C; 1 mL of 0.08 M NaBH4 solution and 200 μL of 0.01 M sodium citrate solution were quickly injected and continuously stirred for 25 minutes, and centrifuged at 8000 rpm for 3 times to obtain rGOg-C3N4@AuNPs nanocomposite material.
[0036] A method for detecting nitrite using rGO / g-C3N4@AuNPs nanocomposite material comprises the following steps:
[0037] 1) Preparation and electrochemical characterization of rGO / g-C3N4@AuNPs modified electrode:
[0038] The prepared rGO / g-C3N4@AuNPs nanocomposite material was dissolved in a mixture of ethanol and water and ultrasonically treated to prepare a 1 mg / mL suspension. The rGO / g-C3N4@AuNPs suspension was then drop-coated on the surface of a glassy carbon electrode and dried to obtain a rGO / g-C3N4@AuNPs modified electrode. The electrode was immersed in a solution containing 0.1 M KCl, 5 mM [Fe(CN)6] 3- / 4- In the mixed solution, electrochemical impedance spectroscopy (EIS) and cyclic voltammetry (CV) were performed, and the rGO / g-C3N4@AuNPs modified electrode showed low electrochemical impedance value and high peak current;
[0039] 2) Electrochemical detection of nitrite ions:
[0040] The rGO / g-C3N4@AuNPs modified electrode was immersed in 2 mM NO2 - The current response signal of DPV was measured in PBS buffer solution with pH = 4.0 to determine the effect of NO2 - Whether there is response and the effect of response. It was found that rGO / g-C3N4@AuNPs modified electrode can respond to NO2 - Electrochemical detection was performed and showed high selectivity.
[0041] 3) Electrochemical detection of nitrite ions in food samples:
[0042] For tap water samples, they were filtered with a 0.45 μm membrane before analysis to remove micron-sized particle impurities.
[0043] For food samples such as spinach, ham and milk, the following pretreatments were performed: (1) 15 g of fresh spinach sample was weighed and mashed into a paste, filtered with a 0.45 μm filter membrane, and the spinach juice was retained and stored in a container for later use; (2) 5.0 g of ham sample was weighed and mashed into a paste, and then 0.5 g was taken and mixed with 5 mL of ultrapure water at 50-80°C for 30 minutes by ultrasound, and then the mixture was centrifuged at 5000 rpm at 4°C for 10 minutes, and then 10 mL of 5 g / L zinc acetate was added to treat the supernatant to precipitate protein. After 30 minutes, the mixture was centrifuged at 8000 rpm and the supernatant was collected for later use; (3) 15 mL of milk was taken, 8 mL of 5 g / L zinc acetate was added at 4°C, and after 30 minutes, the mixture was centrifuged at 10000 rpm and stored in a container for later use.
[0044] After simple pretreatment of the food samples, the supernatant was collected and fixed to 10 mL with 0.1 M pH = 4 PBS buffer. The rGO / g-C3N4@AuNPs modified electrode was inserted into the 0.1 M pH = 4.0 PBS buffer containing the actual sample. The NO2 in the sample was measured according to the standard addition method. - Conduct testing.
[0045] Embodiment 2:
[0046] A method for preparing a rGO / g-C3N4@AuNPs nanocomposite material comprises the following steps:
[0047] 1) Preparation of GO / g-C3N4:
[0048] 40 mg of graphene oxide (GO) was ultrasonically treated in 60 mL of deionized water for 5 hours to obtain a graphene oxide suspension; 80 mg of graphite phase carbon nitride was ultrasonically treated in 80 mL of deionized water for 26 hours, centrifuged at 3000 rpm for 15 minutes, and the supernatant was collected to obtain a g-C3N4 nanosheet suspension; 5 mL of the graphene oxide suspension was ultrasonically mixed with 55 mL of the g-C3N4 nanosheet suspension for 10 hours to obtain a g-C3N4@GO suspension;
[0049] 2) Preparation of rGO / g-C3N4@AuNPs:
[0050] 150 μL of ammonia water and 20 μL of hydrazine hydrate were added to the above g-C3N4@GO suspension, ultrasonically treated for 0.5 h, and magnetically stirred at 100 °C for 4 h to obtain g-C3N4@rGO suspension; 90 μL of 0.1 M chloroauric acid solution was added to the g-C3N4@rGO suspension, ultrasonically treated for 20 min, and continuously stirred at 85 °C; 0.8 mL of 0.08 M NaBH4 solution and 180 μL of 0.01 M sodium citrate solution were quickly injected and stirred continuously for 20 min, and centrifuged twice at 6000 rpm to obtain rGOg-C3N4@AuNPs nanocomposite material.
[0051] 3) Preparation and electrochemical characterization of rGO / g-C3N4@AuNPs modified electrode, same as Example 1.
[0052] 4) Electrochemical detection of nitrite ions in food samples:
[0053] First, food samples were prepared by the following steps: tap water samples were filtered with a 0.45 μm membrane before analysis to remove micron-sized particulate impurities. Food samples such as spinach, ham sausage and milk were purchased and pretreated as follows: (1) 10.0 g of fresh spinach sample was weighed and mashed into a paste, filtered with a 0.45 μm filter membrane, and the spinach juice was retained and stored in a container for later use; (2) 6.0 g of ham sausage sample was weighed and mashed into a paste, and then 0.6 g was taken and mixed with 6 mL of ultrapure water under ultrasonic conditions at 50-80°C for 20-30 minutes, and then the mixture was centrifuged at 4000 rpm for 8 minutes at 4°C, and then 9 mL of 5 g / L zinc acetate was added to treat the supernatant to precipitate protein. After 18 minutes, the supernatant was centrifuged at 90000 rpm and the supernatant was collected for later use; (3) 10 mL of milk was taken, 9 mL of 5 g / L zinc acetate was added at 4°C, and after 15 minutes, the supernatant was centrifuged at 90000 rpm and stored in a container for later use. Finally, the supernatant of the three pre-treated samples was fixed to 10 mL with 0.1 M PBS buffer (pH=4).
[0054] After simple pretreatment of the food samples, the supernatant was collected and fixed to 10 mL with 0.1 M pH = 4 PBS buffer. The rGO / g-C3N4@AuNPs modified electrode was inserted into the 0.1 M pH = 4.0 PBS buffer containing the actual sample. The NO2 in the sample was measured according to the standard addition method. - Conduct testing.
[0055] Embodiment 3:
[0056] A method for preparing a rGO / g-C3N4@AuNPs nanocomposite material comprises the following steps:
[0057] 1) Preparation of GO / g-C3N4:
[0058] 60 mg of graphene oxide (GO) was ultrasonically treated in 70 mL of deionized water for 6 hours to obtain a graphene oxide suspension; 90 mg of graphite carbon nitride was ultrasonically treated in 90 mL of deionized water for 28 hours, centrifuged at 4000 rpm for 25 minutes, and the supernatant was collected to obtain a g-C3N4 nanosheet suspension; 10 mL of the graphene oxide suspension was ultrasonically mixed with 60 mL of the g-C3N4 nanosheet suspension for 1 hour to obtain a g-C3N4@GO suspension;
[0059] 2) Preparation of rGO / g-C3N4@AuNPs:
[0060] 200 μL of ammonia water and 35 μL of hydrazine hydrate were added to the above g-C3N4@GO suspension, ultrasonically treated for 0.8 h, and magnetically stirred at 100 °C for 5 h to obtain g-C3N4@rGO suspension; 110 μL of 0.1 M chloroauric acid solution was added to the g-C3N4@rGO suspension, ultrasonically treated for 30 min, and continuously stirred at 85 °C; 0.9 mL of 0.08 M NaBH4 solution and 190 μL of 0.01 M sodium citrate solution were quickly injected and continuously stirred for 30 min, and centrifuged at 7000 rpm for 3 times to obtain rGO / g-C3N4@AuNPs nanocomposite material.
[0061] 3) Preparation and electrochemical characterization of rGO / g-C3N4@AuNPs modified electrode, same as Example 1.
[0062] 4) Electrochemical detection of nitrite ions in food samples:
[0063] First, food samples were prepared by the following steps: tap water samples were filtered with a 0.45 μm membrane before analysis to remove micron-sized particulate impurities. Food samples such as spinach, ham sausage and milk were purchased and pretreated as follows: (1) 20.0 g of fresh spinach sample was weighed and mashed into a paste, filtered with a 0.45 μm filter membrane, and the spinach juice was retained and stored in a container for later use; (2) 5.0 g of ham sausage sample was weighed and mashed into a paste, and then 0.5 g was taken and mixed with 5 mL of ultrapure water at 80°C for 30 minutes by ultrasonication, and then the mixture was centrifuged at 6000 rpm at 4°C for 10 minutes, and then 10 mL of 5 g / L zinc acetate was added to treat the supernatant to precipitate protein. After 20 minutes, the mixture was centrifuged at 80000 rpm and the supernatant was collected for later use; (3) 20 mL of milk was taken, 10 mL of 5 g / L zinc acetate was added at 4°C, and after 20 minutes, the mixture was centrifuged at 80000 rpm and stored in a container for later use. Finally, the supernatant of the three pre-treated samples was fixed to 10 mL with 0.1 M PBS buffer (pH=4).
[0064] After simple pretreatment of the food samples, the supernatant was collected and fixed to 10 mL with 0.1 M pH = 4 PBS buffer. The rGO / g-C3N4@AuNPs modified electrode was inserted into the 0.1 M pH = 4.0 PBS buffer containing the actual sample. The NO2 in the sample was measured according to the standard addition method. - Conduct testing.
[0065] The nanocomposite material prepared in Example 1 is characterized and analyzed as follows:
[0066] Figure 1 For SEM images, Figure 1 A can clearly show that g-C3N4 is a multilayer flake structure and is amorphous overall; Figure 1 B shows a large number of independent ultrathin nanosheet structures of g-C3N4@rGO; Figure 1 C can clearly see that the spherical AuNPs are evenly dispersed on the surface of rGO / g-C3N4, and no obvious aggregation occurs, which indicates that AuNPs are successfully modified on the surface of rGO / g-C3N4; from TEM ( Figure 1 D) It can be further observed that the rGO / g-C3N4@AuNPs nanomaterial has obvious wrinkles, and the spherical AuNPs are evenly dispersed on the surface of rGO / g-C3N4, proving that AuNPs are successfully modified on the rGO / g-C3N4 composite material.
[0067] Figure 2 Infrared spectrum, 3435cm in GO curve -1 and 1642cm -1The absorption peaks at 1726 cm-1 correspond to the stretching vibrations of OH and C=C, respectively. -1 The band in the spectrum corresponds to the stretching peak of C=O. Compared with GO, the disappearance of the C=O peak in the rGO / g-C3N4 and rGO / g-C3N4@AuNPs curves indicates that GO is successfully reduced to rGO; g-C3N4 at 1245cm -1 The peak at 810 cm-1 is attributed to the stretching vibration of the aromatic CN heterocycle. In addition, rGO / g-C3N4 and rGO / g-C3N4@AuNPs retain the characteristic peaks of GO and g-C3N4, and the peak at 810 cm-1 is attributed to the stretching vibration of the aromatic CN heterocycle. -1 The sharp absorption band at the g-C3N4 nanosheet is due to the stretching vibration of the triazine structural unit.
[0068] Figure 3 This is the XPS spectrum. Figure 3 A full spectrum shows that all three materials have C, N, and O elements, and the content of N in rGO / g-C3N4 is higher than that in GO. This is because g-C3N4 nanosheets are modified on the surface of graphene oxide (GO) through π-π interaction. Compared with GO, the O1s peak of rGO / g-C3N4 decreases, indicating the successful reduction of GO; the presence of Au element indicates that Au nanoparticles are successfully modified on the surface of rGO / g-C3N4. Figure 3 B can find four types of carbon bonds: C=C / CC (284.8 eV), CO (287.08 eV), C=O (288.78 eV) and OC=O (290.98 eV); Figure 3 C and D are the C1s spectra of rGO / g-C3N4 and rGO / g-C3N4@AuNPs, respectively. Compared with GO, the peak at 285.68 eV (CN) indicates the successful combination of g-C3N4 and GO; Figure 3 Au4f in E 5 / 2 (87.67 eV) and Au4f 7 / 2 (84.00 eV), confirming the successful preparation of rGO / g-C3N4@AuNPs composites.
[0069] Figure 4 For bare glassy carbon electrode, rGO modified electrode, rGO / g-C3N4 modified electrode, rGO / g-C3N4@AuNPs modified electrode in 5mM [Fe(CN)6] 3- / 4- Electrochemical impedance spectroscopy, cyclic voltammograms and their effects on NO2 - Differential pulse voltammogram in solution. Figure 4 As shown in A, the impedance curve includes a semicircle in the high-frequency region and a linear curve in the low-frequency region, which correspond to the electron transfer impedance (R et) and the diffusion resistance of the electrolyte in the modified layer. It was found that the semicircle diameter of rGO / g-C3N4@AuNPs / GCE was the smallest, indicating that the charge transfer resistance between the electrode surface and the electrolyte solution was the smallest. Figure 4 B is GO, rGO / g-C3N4 and rGO / g-C3N4@AuNPs modified electrodes in the presence of 5 mM [Fe(CN)6] 3- / 4- CV graph of the mixed solution. The peak current of the CV curve rGO / g-C3N4@AuNPs / GCE>rGO / g-C3N4 / GCE>rGO / GCE>bare / GCE indicates that rGO / g-C3N4@AuNPs / GCE has a higher electron transfer efficiency, proving the improvement of the conductive properties of the composite material. Figure 4 C is the NO2 concentration of 2mM for different modified electrodes - The cyclic voltammetric response diagram shows that rGO / g-C3N4@AuNPs / GCE has the best electrochemical performance and can convert NO2 - Therefore, the constructed rGO / g-C3N4@AuNPs / GCE can be used for NO2 - effective detection.
[0070] Figure 5 Figure 2 shows the effect of rGO / g-C3N4@AuNPs / GCE on NO2 at different scanning rates. - CV response diagram and differential pulse voltammograms at different pH (B), enrichment time (C), and modification volume (D). Figure 5 As can be seen from A, NO2 - There is only one strong oxidation peak in the CV curve, and no reduction peak, indicating that NO2 - The reaction on the electrode surface is irreversible. At the same time, as the scan rate increases, the electrochemical response signal also gradually increases, and the peak current is in the range of 10 to 200 mV / s and is related to the scan rate v 1 / 2 It shows a good linear positive correlation, indicating that NO2 - The electron transfer reaction on rGO / g-C3N4@AuNPs / GCE is a typical diffusion-controlled process. Figure 5 B, 5C, and 5D are the results of NO2 - From the test results, it can be seen that pH = 4 is the optimal pH value, 1 minute is the optimal enrichment time, and 6 μL is the optimal modification amount.
[0071] Figure 6 Under the optimal experimental conditions, rGO / g-C3N4@AuNPs / GCE reacted with different concentrations of NO2 - DPV response diagram, Figure 6 NO2 in A- The peak current increases with the increase of concentration, and the i value shows a strong concentration dependence and a good linear relationship in the concentration range of 1μM-6mM ( Figure 6 B), its linear regression equation is p (μA)=0.000411C(μM)+0.2312(R 2 =0.998), and its detection limit (LODs) was 0.097 μM.
[0072] Figure 7 To detect NO2 - Interference determination. Figure 7 As shown, the first addition of NO2 - , the current increases, and then K is added + , Cu 2+ and Zn 2+ , the current does not change; add NO2 again - , the current increases, then SO4 is added 2- 、NO3 - and F - , the current does not change, continue to add NO2 - , the current increases, then add Glu and DA, the current does not change, then add NO2 - , the current increases again. This indicates that rGO / g-C3N4@AuNPs / GCE has a strong influence on K + , Cu 2+ 、Zn 2+ 、SO4 2- 、NO3 - 、F - , Glu and DA had no response, that is, the presence of these substances did not affect the GO / g-C3N4@AuNPs / GCE to NO2 - Detection.
[0073] Table 1 shows the practicality test of rGO / g-C3N4@AuNPs / GCE sensor in actual samples. Using the standard addition method, rGO / g-C3N4@AuNPs / GCE was placed in different concentrations of NO2 - After calculation, NO2 - The recovery rates were 94.6%-105.23% and the standard deviations were 2.05%-4.22%, confirming that rGO / g-C3N4@AuNPs / GCE can be used for NO2 - effective detection.
[0074] Table 1. NO2 in actual samples determined by rGO / g-C3N4@AuNPs / GCE -
[0075]
[0076] The embodiments described above are only descriptions of the preferred implementation modes of the present invention, and are not intended to limit the concept and protection scope of the present invention. Without departing from the design concept of the present invention, ordinary engineers and technicians in this field may make various modifications and improvements to the technical solutions of this aspect, which shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing rGO / g-C3N4@AuNPs nanocomposite material, characterized in that: The following steps are involved: 1) Preparation of GO / g-C3N4: 40-60 mg of graphene oxide (GO) was ultrasonically treated in 50-70 mL of deionized water for 5-8 hours to obtain a graphene oxide suspension; 80-100 mg of graphite phase carbon nitride was ultrasonically treated in 80-100 mL of deionized water for 24-30 hours, centrifuged at 3000-5000 rpm for 15-30 minutes, and the supernatant was collected to obtain a g-C3N4 nanosheet suspension; 5-10 mL of the graphene oxide suspension was ultrasonically mixed with 50-60 mL of the g-C3N4 nanosheet suspension for 10-12 hours to obtain a g-C3N4@GO suspension; 2) Preparation of rGO / g-C3N4@AuNPs: 150-300 μL of ammonia water and 20-40 μL of hydrazine hydrate were added to the above g-C3N4@GO suspension, ultrasonically treated for 0.5-1.5 hours, and magnetically stirred at 90-110°C for 4-6 hours to obtain a g-C3N4@rGO suspension; 90-110 μL of 0.1M chloroauric acid solution was added to the g-C3N4@rGO suspension, ultrasonically treated for 20-30 minutes, and continuously stirred at 85°C; 0.8-1mL of 0.08M NaBH4 solution and 180-200 μL of 0.01M sodium citrate solution were quickly injected and continuously stirred for 20-30 minutes, and centrifuged at 6000-8000 rpm for 3-5 times to obtain rGO / g-C3N4@AuNPs nanocomposite material.
2. The method for preparing a rGO / g-C3N4@AuNPs nanocomposite material according to claim 1, characterized in that: In the step 1), the graphene oxide is ultrasonically treated in deionized water for 8 hours.
3. The method for preparing a rGO / g-C3N4@AuNPs nanocomposite material according to claim 1, characterized in that: In the step 1), the graphite phase carbon nitride is ultrasonically treated in deionized water for 24 hours.
4. The method for preparing a rGO / g-C3N4@AuNPs nanocomposite material according to claim 1, characterized in that: The centrifugal speed in step 1) is 5000 rpm / min, and the centrifugal time is 30 minutes.
5. The method for preparing a rGO / g-C3N4@AuNPs nanocomposite material according to claim 1, characterized in that: In the step 1), the ultrasonic mixing time of the graphene oxide suspension and the g-C3N4 nanosheet suspension is 12 hours.
6. The method for preparing a rGO / g-C3N4@AuNPs nanocomposite material according to claim 1, characterized in that: The mass concentration of ammonia water in step 2) is 25%.
7. The method for preparing a rGO / g-C3N4@AuNPs nanocomposite material according to claim 1, characterized in that: In the step 2), ammonia water and hydrazine hydrate are added to the g-C3N4@GO suspension, the ultrasonic treatment time is 1 hour, and magnetic stirring is performed at 100° C. for 5 hours.
8. The rGO / g-C3N4@AuNPs nanocomposite material prepared according to any one of claims 1 to 7.
9. Use of the rGO / g-C3N4@AuNPs nanocomposite material according to claim 8 in electrochemical detection of nitrite.
10. A method for electrochemical detection of nitrite using rGO / g-C3N4@AuNPs nanocomposite materials, characterized in that: The following steps are involved: 1) Preparation and electrochemical characterization of rGO / g-C3N4@AuNPs modified electrode: The rGO / g-C3N4@AuNPs nanocomposite material according to claim 8 is dissolved in a mixture of ethanol and water and subjected to ultrasonic treatment to prepare a 1 mg / mL suspension; the rGO / g-C3N4@AuNPs suspension is drop-coated on the surface of a glassy carbon electrode (GCE) and dried to obtain a rGO / g-C3N4@AuNPs modified electrode; the rGO / g-C3N4@AuNPs modified electrode is immersed in a solution containing 0.1M KCl, 5mM [Fe(CN)6] 3- / 4- In the mixed solution, electrochemical impedance spectroscopy (EIS) and cyclic voltammetry (CV) were performed to characterize the rGO / g-C3N4@AuNPs modified electrode, which showed a low electrochemical impedance value and a high peak current value; 2) Electrochemical detection of nitrite ions: The rGO / g-C3N4@AuNPs modified electrode was immersed in 2 mM NO2 - The differential pulse voltammetry (DPV) test was carried out in a PBS buffer solution with a pH of 4.
0. The current response signal of the DPV was measured to determine the effect of NO2 - Whether there is response and the effect of response; the experiment found that rGO / g-C3N4@AuNPs modified electrode can successfully react with NO2 - Electrochemical detection was performed and showed high selectivity; 3) Electrochemical detection of nitrite ions in food samples: After pretreatment of the food samples, the supernatant was collected and fixed to 10 mL with 0.1 M pH = 4 PBS buffer. The rGO / g-C3N4@AuNPs modified electrode was inserted into the 0.1 M pH = 4.0 PBS buffer containing the actual sample. The NO2 in the sample was measured according to the standard addition method. - Conduct testing.
Citation Information
Patent Citations
Preparation method of graphite olefince modified electrochemical sensor electrode
CN102645468A
Preparation of three-dimensional graphene nano composite material and method for chirally recognizing tryptophan (Trp)
CN107764886A
Device for detecting nitrite by using nanogold graphene modified electrochemical method
CN109187678A
g-C3N4 nanosheet / graphene oxide composite material and preparation method and application thereof
CN110980666A
Nanocomposite electrochemical sensor, construction method and application of nanocomposite electrochemical sensor in detection of nitrite ions and iodide ions