Method for detecting impurity content of lanthanum-containing solid electrolyte material
Through one-step digestion method and microwave digestion technology, the cumbersome and inaccurate problems in detecting impurities of lanthanum-containing solid electrolyte materials in the prior art are solved, and more efficient and accurate detection results are achieved.
Patent Information
- Application Number
- CN202411746304.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-29
- Publication Date
- 2025-03-21
AI Technical Summary
The prior art has multiple cumbersome digestion processes when detecting impurity elements in lanthanum-containing solid electrolyte materials, which increases testing costs and safety risks, and it is difficult to accurately determine the content of impurity elements.
The one-step digestion method is used to mix the sample to be tested with a small amount of hydrochloric acid and sulfuric acid for microwave digestion to obtain a completely digested filtrate, which reduces the loss of main elements and the introduction of impurity elements, and is tested by an inductively coupled plasma emission spectrometer.
The operation steps are simplified, manpower and material consumption is reduced, the accuracy of element content is improved, and the impurity elements in the original sample can be measured within the range of error permitted.
Smart Images

Figure BDA0005166071320000121 
Figure BDA0005166071320000122 
Figure BDA0005166071320000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of detection methods, and more specifically, to a method for detecting the impurity content of a lanthanum-containing solid electrolyte material. Background Art
[0002] Solid electrolytes are the core of solid-state batteries, among which oxides, sulfides, and polymer electrolytes are the mainstream. At present, oxide electrolytes have balanced performance, and sulfides have the greatest potential. Their upstream metal raw materials mainly include zirconium, germanium, titanium, lanthanum, etc., among which lanthanum is a metallic rare earth element with abundant reserves in my country.
[0003] At present, lanthanum-containing solid electrolyte materials have attracted more and more attention from scientific researchers due to their excellent performance. They mainly include lithium lanthanum titanium oxide solid electrolyte (LLTO) and lithium lanthanum zirconium oxide solid electrolyte (LLZO). The main elements of LLTO (elements that make up the solid electrolyte, which are indispensable for the solid electrolyte) are Li, La, Ti, and O. The main elements of LLZO are Li, La, Zr, and O. According to different doping elements (elements deliberately doped to improve the performance or physical phase of the electrolyte, such as tantalum, niobium, tungsten, aluminum, antimony, and tellurium; these elements are optional for the solid electrolyte), it can further include: lithium lanthanum zirconium tantalum oxide solid electrolyte (LLZTO, doped element is Ta), lithium lanthanum zirconium niobium oxide solid electrolyte (LLZNO, doped element is Nb), lithium lanthanum zirconium tungsten oxide solid electrolyte (LLZWO, doped element is W), lithium aluminum lanthanum zirconium oxide solid electrolyte (LALZO, doped element is Al), lithium lanthanum zirconium antimony oxide solid electrolyte (LLZSO, doped element is Sb), and lithium aluminum lanthanum zirconium tellurium oxide solid electrolyte (LLZTO, doped element is Te).
[0004] Regarding the detection of various elements in lanthanum-containing solid electrolyte materials, patent CN109540874B discloses a method for detecting the content of inorganic elements in a sample of a lithium lanthanum zirconium oxygen type solid electrolyte. The detection method comprises: (1) melting the sample, adding hydrofluoric acid and filtering to obtain a filtrate and a filter residue; (2) alkali melting the filter residue, adding a hydrochloric acid solution, to obtain a filter residue solution; (3) using an inductively coupled plasma emission spectrometer to measure the content of inorganic elements in the filtrate and the filter residue solution. The detection method can detect the content of lithium, lanthanum and zirconium in a lithium lanthanum zirconium oxygen type solid electrolyte sample by an inductively coupled plasma emission spectrometer. Patent CN110931847B discloses a method for processing a solid electrolyte and a method for testing the element content in a solid electrolyte, the method comprising: (1) first contacting the solid electrolyte with an alkaline substance to obtain a first contact material, the temperature of the first contact being 500 to 1000°C; (2) second contacting the first contact material with a solvent to obtain a first contact material solution; (3) third contacting the first contact material solution with an acid to obtain a solid electrolyte solution.
[0005] However, the existing technical solutions still have the following technical problems: (1) The existing technical solutions all need to first mix the sample with a specific substance and then perform a high-temperature dissolution treatment, then add acid and other substances for digestion, filter the residue and continue digestion, and finally achieve complete digestion; the high-temperature melting of the sample requires strict temperature control, which increases the testing cost and also brings high safety risks. (2) The existing technical solutions actively introduce a large number of existing / new elements by adding a co-solvent for digestion, while the inductively coupled plasma emission spectrometer determines the type and content of each element based on the "characteristic wavelength" and "signal intensity of the characteristic wavelength" of each element in the excited state. The introduction of a large number of elements greatly increases the amount of elements with characteristic wavelengths close to the target element to be measured, and the testing equipment easily identifies these "elements with characteristic wavelengths close to the element to be measured" as target elements, which seriously interferes with the accurate determination of the content of the element to be measured. (3) The existing technical solution needs to filter and collect the filter residue. In the process of filtering with filter paper, the elements originally existing in the filter paper will inevitably be brought into the filtrate, which will affect the test results. Therefore, the existing technical solution can only determine the content of major elements such as lithium, lanthanum, and zirconium in the sample within the range of error, but it is completely unable to accurately determine the content of impurity elements in the original sample (except for the main elements and doping elements, "elements that should not appear in the sample in actual production and are of concern to the industry", including: Al, As, Ba, Ca, Cd, Cr, Cu, Fe, Hg, K, Mg, Mn, Na, Ni, Pb, Si, Zn, etc.). (4) The existing technical solution needs to collect the filtrate separately for ICP testing, and then obtain the final result through mathematical calculation, which increases the complexity of the operation. (5) In the prior art solution, when performing ICP testing, the spectrum of potassium element is generally only relatively stable at a wavelength of 766.49nm, while the emission spectrum of lanthanum element at 766.434nm is very likely to interfere with potassium element, causing the test result of K element content to be greater than the actual value, especially in the presence of high lanthanum element. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide a method for detecting the impurity content of a lanthanum-containing solid electrolyte material, which can completely digest the sample to be tested in one step to obtain a filtrate without filter residue, greatly simplifying the operation steps, and at the same time greatly reducing the loss of main elements in the digestion process, saving manpower and material resources; and, in the digestion process, microwave digestion is used, and only a small amount of hydrochloric acid and sulfuric acid are used, which greatly reduces the introduction of impurity elements, thereby reducing the mutual interference between the elements, making the determination of the element content more accurate, and without introducing a large amount of new elements, the impurity elements in the original sample can be determined within the allowable error range.
[0007] The present invention provides a method for detecting the impurity content of a lanthanum-containing solid electrolyte material, comprising the following steps:
[0008] a) mixing the lanthanum-containing solid electrolyte material to be tested with an acid solution, performing a digestion reaction, and obtaining a digestion solution;
[0009] b) After diluting the digestion solution obtained in step a), the main elements and impurity elements are tested respectively by inductively coupled plasma emission spectrometer, and the test results of each element are obtained by comparing with the marking lines of each element. Finally, the impurity content of the lanthanum-containing solid electrolyte material is obtained by calculation.
[0010] Preferably, the acid solution in step a) is hydrochloric acid with a mass fraction of 36% to 38% and / or sulfuric acid with a mass fraction of 95% to 98%.
[0011] Preferably, the digestion reaction in step a) is carried out by hydrothermal reaction in a reactor or microwave reaction in a microwave digester; the temperature of the digestion reaction is 180° C. to 250° C., and the time is 0.5 h to 5 h.
[0012] Preferably, the dilution process in step b) is specifically as follows:
[0013] The digestion solution is diluted to 50±5 g with a diluent to obtain a first solution;
[0014] Take 5±0.5 g of the first solution and dilute it to 50±1 g with a diluent to obtain a second solution;
[0015] Take 20±0.5g of the first solution and dilute to 25±1g with oxalic acid to obtain a third solution;
[0016] Take 10±0.5g of the first solution, add 4±1g of a standard solution with a concentration of 1ppm, and then add a diluent to make the volume to 20±1g to obtain a fourth solution;
[0017] Take 10±0.5g of the third solution, add 4±1g of a standard solution with a concentration of 1ppm, and then add a diluent to make the volume to 20±1g to obtain a fifth solution;
[0018] Take 5±0.5 g of the third solution and dilute it to 50±1 g with a diluent to obtain a sixth solution.
[0019] Preferably, the diluent is a mixture of water and hydrochloric acid with a mass fraction of 36% to 38% in a volume ratio of 4: (0.8 to 1).
[0020] Preferably, the standard solution includes standard solutions of main elements and impurity elements with different concentrations, wherein the concentrations of the main elements are 1ppm, 2ppm, 5ppm, 10ppm, 20ppm respectively, and the concentrations of the impurity elements are 0.1ppm, 0.2ppm, 0.5ppm, 1ppm, 2ppm respectively.
[0021] Preferably, the testing conditions for the main element and the impurity element in step b) include:
[0022] For the elements Al, As, Cd, Cr, Cu, Fe, Hg, Mn, Ni, Pb, Si, and Zn, the RF power was 1–1.5 kW, the stabilization time was 14–16 s, and the observation mode was axial;
[0023] For elements Ba, Ca, K, Mg, and Na, the RF power was 1–1.5 kW, the stabilization time was 4–6 s, and the observation mode was radial;
[0024] For the elements Li, La, Zr, and Ti, the RF power was 1 to 1.5 kW, the stabilization time was 14 to 16 s, and the observation mode was radial.
[0025] Preferably, the element markings in step b) are obtained by testing standard solutions of main elements and impurity elements of different concentrations using an inductively coupled plasma emission spectrometer; the linearity of each element marking generated by the testing equipment is not less than 99.9%; the standard solution is diluted to the corresponding concentration using the same bottle of dilution solution, and the dilution solution is dilute nitric acid or dilute hydrochloric acid with a concentration range of 3% to 10%.
[0026] Preferably, the calculation in step b) adopts the following formula:
[0027] A1=a1×m2 / m1;
[0028] Among them, A1 is the impurity element content, in ppm; a1 is the impurity element test result, in ppm; m2 is the mass of the first solution, in g; m1 is the mass of the lanthanum-containing solid electrolyte material to be tested, in g.
[0029] Preferably, the step b) further comprises:
[0030] The main element content of the lanthanum-containing solid electrolyte material is calculated; the calculation adopts the following formula:
[0031] B1=b1×m2×5 / m1;
[0032] Among them, B1 is the main element content, in ppm; b1 is the main element test result, in ppm; m2 is the mass of the first solution, in g; m1 is the mass of the lanthanum-containing solid electrolyte material to be tested, in g.
[0033] The present invention provides a method for detecting the impurity content of a lanthanum-containing solid electrolyte material, comprising the following steps: a) mixing the lanthanum-containing solid electrolyte material to be tested with an acid solution, performing a digestion reaction, and obtaining a digestion solution; b) diluting the digestion solution obtained in step a), respectively testing the main element and the impurity element using an inductively coupled plasma emission spectrometer, obtaining the test results of each element by comparing with the marking lines of each element, and finally calculating to obtain the impurity content of the lanthanum-containing solid electrolyte material. Compared with the prior art, the detection method provided by the present invention adopts specific process steps to achieve overall good interaction: the sample to be tested can be completely digested in one step to obtain a filtrate without filter residue, which greatly simplifies the operation steps, and at the same time greatly reduces the loss of the main element in the digestion process, saving manpower and material resources; and, microwave digestion is used in the digestion process, and only a small amount of hydrochloric acid and sulfuric acid are used, which greatly reduces the introduction of impurity elements, thereby reducing the mutual interference between the elements, making the determination of the element content more accurate, and not introducing a large amount of new elements, and the impurity elements in the original sample can be determined within the error allowable range.
[0034] At the same time, the present invention can not only decompose cubic phase LLZO materials, but also decompose LLTO, LLZO and various doped derivatives thereof, and is not limited to a specific phase (eg, tetragonal phase, cubic phase, rhombohedral phase, etc.).
[0035] In addition, the present invention has a relatively loose requirement on the digestion temperature range of the sample, and the required digestion temperature is also relatively low, and the digestion can be performed between 180 and 250° C.; even if the digestion tank is not tightly sealed, the harm to people caused by the volatilization and leakage of hydrochloric acid is much smaller than that of hydrofluoric acid, and the boiling point of sulfuric acid is 337° C., and the volatility is also much smaller than that of hydrofluoric acid, so the digestion process is safer; at the same time, because the digestion temperature is low, even if the digestion tank is not tightly sealed, the loss caused by the volatilization of mercury, lead, cadmium, tin, selenium, etc. is also smaller, and the test results of the content of these impurity elements are also closer to the true value.
[0036] Finally, when testing the K element content, the present invention first adds excess oxalic acid to the digested test solution to form lanthanum oxalate that is insoluble in water and most acids with the La element, and then centrifuges to remove residues to reduce the La element content in the solution; the spectral interference of the La element on the K element during ICP testing is avoided, and the accuracy of the test result is effectively guaranteed. DETAILED DESCRIPTION
[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The present invention provides a method for detecting the impurity content of a lanthanum-containing solid electrolyte material, comprising the following steps:
[0039] a) mixing the lanthanum-containing solid electrolyte material to be tested with an acid solution, performing a digestion reaction, and obtaining a digestion solution;
[0040] b) After diluting the digestion solution obtained in step a), the main elements and impurity elements are tested respectively by inductively coupled plasma emission spectrometer, and the test results of each element are obtained by comparing with the marking lines of each element. Finally, the impurity content of the lanthanum-containing solid electrolyte material is obtained by calculation.
[0041] The present invention first mixes the lanthanum-containing solid electrolyte material to be tested with an acid solution, performs a digestion reaction, and obtains a digestion solution. In the present invention, the lanthanum-containing solid electrolyte material to be tested can be not only a cubic phase LLZO material, but also LLTO, LLZO and various doped derivatives thereof, and is not limited to a specific physical phase (such as: tetragonal phase, cubic phase, rhombohedral phase, etc.); the present invention has no special restrictions on the source of the lanthanum-containing solid electrolyte material to be tested, and commercially available products or self-made products familiar to those skilled in the art can be used. In the present invention, the mass of the lanthanum-containing solid electrolyte material to be tested is recorded, denoted as m1.
[0042] In the present invention, the acid solution is preferably hydrochloric acid with a mass fraction of 36% to 38% and / or sulfuric acid with a mass fraction of 95% to 98%. The present invention has no special restriction on the source of the acid solution, and commercially available products known to those skilled in the art can be used.
[0043] For materials such as LLTO, LLZO and their various doped derivatives, because the main elements such as lithium, lanthanum, zirconium, titanium, etc. do not react with hydrochloric acid or sulfuric acid to form precipitates that are difficult to dissolve in acid (i.e., insoluble substances), hydrochloric acid or sulfuric acid, while destroying the main structure of the above materials, react with these main elements to form substances that are easily soluble in acid (i.e., "soluble substances", as opposed to "insoluble substances"; Note: insoluble substances are not completely insoluble in acid, but their solubility in acid is very small). As for the impurity elements in these materials, on the one hand, most of the elements can also react with hydrochloric acid or sulfuric acid to form soluble substances that are easily soluble in acid; on the other hand, although some of the existing elements will react with hydrochloric acid and sulfuric acid to form substances that are difficult to dissolve in acid, because the content is extremely small, it is far from reaching the upper limit of solubility in acid, so it can also be completely dissolved in acid (special note: in the enterprise, for the above samples, the requirements for the content of impurity elements are very low, far from reaching the upper limit of its solubility in acid. If it is found that there is precipitation in the digestion solution and the subsequent diluted solution after the sample is digested, it means that the content of impurity elements in this material exceeds the standard and can be directly judged as unqualified). In addition, some elements (such as titanium) are easily hydrolyzed in water or dilute acid, so a higher concentration of acid (the diluent in the subsequent steps) is used to dilute and fix the volume. In the present invention, the same bottle of acid or diluent is always used for digestion and dilution, which reduces the introduction of impurities.
[0044] In the present invention, the digestion reaction is preferably a hydrothermal reaction in a reactor or a microwave reaction in a microwave digester; wherein the hydrothermal reaction in a reactor is to mix the lanthanum-containing solid electrolyte material to be tested with an acid solution and then add it to a polytetrafluoroethylene digestion tank, and then put the digestion tank into a reactor for conventional hydrothermal reaction; the microwave reaction in a microwave digester is to mix the lanthanum-containing solid electrolyte material to be tested with an acid solution and then add it to a polytetrafluoroethylene digestion tank, and then put the digestion tank into a microwave digester for microwave hydrothermal reaction. For reactor digestion, hydrochloric acid can be directly used for digestion because the temperature of the solution in the digestion tank is increased by external heating under a high pressure environment (the digestion tube is tightly sealed); for microwave digestion, microwave digestion directly heats the substance through the two effects of molecular polarization and ion conduction, prompting the surface layer of the solid sample to break quickly, generating a new surface and solvent interaction, and completely decomposing the sample within a few minutes. Using only hydrochloric acid, the solution cannot be raised to the corresponding temperature, so it is necessary to add some sulfuric acid to raise the solution to the corresponding temperature.
[0045] In the present invention, the temperature of the digestion reaction is preferably 180° C. to 250° C., and the time is preferably 0.5 h to 5 h.
[0046] After the digestion reaction is completed, the digestion tank is taken out and opened, and the powder sample is completely digested into a clear and transparent liquid to obtain a digestion solution.
[0047] After obtaining the digestion solution, the present invention dilutes the obtained digestion solution, and uses an inductively coupled plasma emission spectrometer to test the main elements and impurity elements respectively, and obtains the test results of each element by comparing with the marking lines of each element, and finally obtains the impurity content of the lanthanum-containing solid electrolyte material through calculation.
[0048] In the present invention, the dilution process is preferably specifically as follows:
[0049] The digestion solution is diluted to 50±5 g with a diluent to obtain a first solution;
[0050] Take 5±0.5 g of the first solution and dilute it to 50±1 g with a diluent to obtain a second solution;
[0051] Take 20±0.5g of the first solution and dilute to 25±1g with oxalic acid to obtain a third solution;
[0052] Take 10±0.5g of the first solution, add 4±1g of a standard solution with a concentration of 1ppm, and then add a diluent to make the volume to 20±1g to obtain a fourth solution;
[0053] Take 10±0.5g of the third solution, add 4±1g of a standard solution with a concentration of 1ppm, and then add a diluent to make the volume to 20±1g to obtain a fifth solution;
[0054] Take 5±0.5 g of the third solution and dilute it to 50±1 g with a diluent to obtain a sixth solution.
[0055] In a preferred embodiment of the present invention, the above process is specifically performed as follows:
[0056] Pour the digestion solution into centrifuge tube 1, add diluent to make up to 50.00±5.00g (accurate to the second decimal place, the solution at this time is a mixed solution of "digestion solution and diluent", recorded as the first solution); record the mass m2 of the first solution at this time (unit: g, accurate to the second decimal place).
[0057] Then, take out 5.00±0.50g (accurate to the second decimal place) of the first solution from centrifuge tube 1 and add it to centrifuge tube 2. In centrifuge tube 2, add the diluent to make the volume up to 50.00±1.00g (accurate to the second decimal place, the mixed solution at this time is recorded as the second solution).
[0058] Then, take out 20.00±0.50g (accurate to the second decimal place) of the first solution from centrifuge tube 1 and add it to centrifuge tube 3. In centrifuge tube 3, add oxalic acid to make the volume to 25.00±1.00g (accurate to the second decimal place, the mixed solution at this time is recorded as the third solution).
[0059] Then, take out 10.00±0.50g (accurate to the second decimal place) of the first solution from centrifuge tube 1 and add it to centrifuge tube 4. In centrifuge tube 4, add 4g of the standard solution with a concentration of 1ppm, and then add the diluent to make up the volume to 20.00±1.00g (accurate to the second decimal place, the mixed solution at this time is recorded as the fourth).
[0060] Then, 10.00±0.50g (accurate to the second decimal place) of the third solution is taken out from centrifuge tube 3 and added to centrifuge tube 5. In centrifuge tube 5, 4g of the standard solution with a concentration of 1ppm is added, and then the diluent is added to make the volume to 20.00±1.00g (accurate to the second decimal place, and the mixed solution at this time is recorded as the fifth solution)
[0061] Finally, take out 5.00±0.50g (accurate to the second decimal place) of the third solution from centrifuge tube 3 and add it to centrifuge tube 6. In centrifuge tube 6, add diluent to make the volume up to 50.00±1.00g (accurate to the second decimal place, the mixed solution at this time is recorded as the sixth solution).
[0062] In the present invention, the diluent is preferably a mixture of water and hydrochloric acid with a mass fraction of 36% to 38% in a volume ratio of 4: (0.8 to 1).
[0063] In the present invention, the standard solution includes standard solutions of main elements and impurity elements of different concentrations, wherein the concentrations of main elements (including but not limited to Li, La, Zr, Ti and other elements in the prepared standard solution) are 1ppm, 2ppm, 5ppm, 10ppm, 20ppm, respectively, and the concentrations of impurity elements (including but not limited to Al, As, Ba, Ca, Cd, Cr, Cu, Fe, Hg, K, Mg, Mn, Na, Ni, Pb, Si, Zn and other elements in the prepared standard solution) are 0.1ppm, 0.2ppm, 0.5ppm, 1ppm, 2ppm, respectively. The present invention prepares the above-mentioned series of standard solutions of different concentrations, which are also used for making marking lines of inductively coupled plasma emission spectrometer.
[0064] In the present invention, the test conditions for the main element and the impurity element respectively preferably include:
[0065] For the elements Al, As, Cd, Cr, Cu, Fe, Hg, Mn, Ni, Pb, Si, and Zn, the RF power is preferably 1 to 1.5 kW, the stabilization time is preferably 14 to 16 s, and the observation mode is preferably axial;
[0066] For elements Ba, Ca, K, Mg, and Na, the RF power is preferably 1 to 1.5 kW, the stabilization time is preferably 4 to 6 s, and the observation mode is preferably radial;
[0067] For the elements Li, La, Zr, and Ti, the RF power is preferably 1 to 1.5 kW, the stabilization time is preferably 14 to 16 s, and the observation mode is preferably radial.
[0068] In a preferred embodiment of the present invention, the content of impurity elements in the third solution is measured by inductively coupled plasma emission spectrometer, and the content of main elements in the second solution is measured; wherein:
[0069] For impurity elements:
[0070] When the element to be determined is Al, the detection wavelength is 396.152nm, or 237.312nm;
[0071] When the element to be determined is As, the detection wavelength is 193.696nm, or 197.198nm;
[0072] When the element to be determined is Ba, the detection wavelength is 455.403nm, or 233.527nm;
[0073] When the element to be determined is Ca, the detection wavelength is 396.847nm, or 317.933nm;
[0074] When the element to be determined is Cd, the detection wavelength is 214.439nm, or 226.502nm;
[0075] When the element to be determined is Cr, the detection wavelength is 267.716nm, or 205.56nm;
[0076] When the element to be determined is Cu, the detection wavelength is 327.395nm, or 213.598nm;
[0077] When the element to be determined is Fe, the detection wavelength is 238.204nm, or 259.94nm;
[0078] When the element to be determined is Hg, the detection wavelength is 184.887nm, or 253.652nm;
[0079] When the element to be determined is K, the detection wavelength is 766.491 nm and FACT calibration is used;
[0080] When the element to be determined is Mg, the detection wavelength is 279.553nm, or 280.27nm;
[0081] When the element to be determined is Mn, the detection wavelength is 257.610nm, or 259.372nm;
[0082] When the element to be determined is Na, the detection wavelength is 589.592nm, or 588.995nm;
[0083] When the element to be determined is Ni, the detection wavelength is 231.604nm, or 216.555nm;
[0084] When the element to be determined is Pb, the detection wavelength is 220.353nm;
[0085] When the element to be determined is Si, the detection wavelength is 251.611nm, or 250.69nm;
[0086] When the element to be determined is Zn, the detection wavelength is 213.857nm, or 202.548nm;
[0087] For the main element:
[0088] When the element to be determined is Li, the detection wavelength is 460.289nm, or 610.365nm, or 670.783nm;
[0089] When the element to be determined is La, the detection wavelength is 333.749nm, or 379.477nm, or 408.671nm;
[0090] When the element to be determined is Ti, the detection wavelength is 334.941nm, or 336.122nm, or 337.280nm;
[0091] When the element to be determined is Zr, the detection wavelength is 343.823 nm, or 339.198 nm.
[0092] In the present invention, the element markings are preferably obtained by testing the standard solutions of the main elements and impurity elements with different concentrations using an inductively coupled plasma emission spectrometer; the linearity of each element marking generated by the testing equipment is preferably not less than 99.9%; the standard solution is preferably diluted to the corresponding concentration using the same bottle of dilution solution, and the dilution solution is preferably dilute nitric acid or dilute hydrochloric acid with a concentration range of 3% to 10%.
[0093] By comparing with the marking lines of each element, the test results of each element are obtained, including: the test result a1 of the impurity element and the test result b1 of the main element; on this basis, the calculation preferably adopts the following formula:
[0094] A1=a1×m2 / m1;
[0095] Among them, A1 is the impurity element content, in ppm; a1 is the impurity element test result, in ppm; m2 is the mass of the first solution, in g; m1 is the mass of the lanthanum-containing solid electrolyte material to be tested, in g.
[0096] In a preferred embodiment of the present invention, assuming that the test result of the content of a certain impurity element in the first solution is a1 (unit: ppm, accurate to the second decimal place), then the content A1 (unit: ppm, accurate to the second decimal place) of the impurity element in the unit mass of lanthanum-containing solid electrolyte material can be obtained by the above calculation formula; the same is true for other impurity elements to obtain the impurity element content of the lanthanum-containing solid electrolyte material.
[0097] In the present invention, the step b) preferably further comprises:
[0098] The main element content of the lanthanum-containing solid electrolyte material is calculated; the calculation preferably adopts the following formula:
[0099] B1=b1×m2×5 / m1;
[0100] Among them, B1 is the main element content, in ppm; b1 is the main element test result, in ppm; m2 is the mass of the first solution, in g; m1 is the mass of the lanthanum-containing solid electrolyte material to be tested, in g.
[0101] In a preferred embodiment of the present invention, assuming that the test result of the content of a certain main element in the second solution is b1 (unit: ppm, accurate to the second decimal place), the content B1 (unit: ppm, accurate to the second decimal place) of the main element in the unit mass of lanthanum-containing solid electrolyte material can be obtained by the above calculation formula; the same is true for other main elements to obtain the main element content of the lanthanum-containing solid electrolyte material.
[0102] The present invention provides a method for detecting the impurity content of a lanthanum-containing solid electrolyte material, comprising the following steps: a) mixing the lanthanum-containing solid electrolyte material to be tested with an acid solution, performing a digestion reaction, and obtaining a digestion solution; b) diluting the digestion solution obtained in step a), respectively testing the main element and the impurity element using an inductively coupled plasma emission spectrometer, obtaining the test results of each element by comparing with the marking lines of each element, and finally calculating to obtain the impurity content of the lanthanum-containing solid electrolyte material. Compared with the prior art, the detection method provided by the present invention adopts specific process steps to achieve overall good interaction: the sample to be tested can be completely digested in one step to obtain a filtrate without filter residue, which greatly simplifies the operation steps, and at the same time greatly reduces the loss of the main element in the digestion process, saving manpower and material resources; and, microwave digestion is used in the digestion process, and only a small amount of hydrochloric acid and sulfuric acid are used, which greatly reduces the introduction of impurity elements, thereby reducing the mutual interference between the elements, making the determination of the element content more accurate, and not introducing a large amount of new elements, and the impurity elements in the original sample can be determined within the error allowable range.
[0103] At the same time, the present invention can not only decompose cubic phase LLZO materials, but also decompose LLTO, LLZO and various doped derivatives thereof, and is not limited to a specific phase (eg, tetragonal phase, cubic phase, rhombohedral phase, etc.).
[0104] In addition, the present invention has a relatively loose requirement on the digestion temperature range of the sample, and the required digestion temperature is also relatively low, and the digestion can be performed between 180 and 250° C.; even if the digestion tank is not tightly sealed, the harm to people caused by the volatilization and leakage of hydrochloric acid is much smaller than that of hydrofluoric acid, and the boiling point of sulfuric acid is 337° C., and the volatility is also much smaller than that of hydrofluoric acid, so the digestion process is safer; at the same time, because the digestion temperature is low, even if the digestion tank is not tightly sealed, the loss caused by the volatilization of mercury, lead, cadmium, tin, selenium, etc. is also smaller, and the test results of the content of these impurity elements are also closer to the true value.
[0105] Finally, when testing the K element content, the present invention first adds excess oxalic acid to the digested test solution to form lanthanum oxalate that is insoluble in water and most acids with the La element, and then centrifuges to remove residues to reduce the La element content in the solution; the spectral interference of the La element on the K element during ICP testing is avoided, and the accuracy of the test result is effectively guaranteed.
[0106] In order to further illustrate the present invention, the following examples are used for detailed description. In the following examples of the present invention, solution B: ultrapure water and hydrochloric acid with a mass fraction of 36% to 38% are used to prepare a certain concentration of diluted hydrochloric acid (i.e., solution B); the preparation rule of solution B is as follows: 4 volumes of ultrapure water are mixed with 0.8 to 1 volume of hydrochloric acid; then solution A is poured into a centrifuge tube, and solution B is added to make up the volume to obtain a mixed solution of solution A and solution B (solution C).
[0107] Example 1
[0108] Take a known sample Li 0.5 La 0.5 TO3, weigh 0.1142g of LLTO powder sample with an analytical balance, put it into a digestion tank, add 10mL of hydrochloric acid with a mass fraction of 36% to 38% with a pipette, put the digestion tank into the reactor, heat it at 220℃ for 4 hours, take out and open the digestion tank, the sample is completely digested into a clear and transparent liquid (solution A), and the solution B mentioned above is used to make the volume to 50.01g (solution C).
[0109] Take 5.01 g of liquid from solution C, add solution B to make up to 50.01 g (solution D); take out 20.00±0.50 g (accurate to the second decimal place) of solution C from solution C, add oxalic acid to make up to 25.00±1.00 g (accurate to the second decimal place, the mixed solution at this time is recorded as solution E). Take out 10.00±0.50g (accurate to the second decimal place) of solution C from solution C, add 4g of standard solution with a concentration of 1ppm, and then add solution B to make up the volume to 20.00±1.00g (accurate to the second decimal place, the mixed solution at this time is recorded as solution F); take out 10.00±0.50g (accurate to the second decimal place) of solution E from solution E, add 4g of standard solution with a concentration of 1ppm, and then add solution B to make up the volume to 20.00±1.00g (accurate to the second decimal place, the mixed solution at this time is recorded as solution G); take out 5.00±0.50g (accurate to the second decimal place) of solution E from solution E, add solution B to make up the volume to 50.00±1.00g (accurate to the second decimal place, the mixed solution at this time is recorded as solution H).
[0110] According to the above requirements, 3% dilute nitric acid is used to prepare standard solutions containing "Li, La, Ti elements, concentrations of 1ppm, 2ppm, 5ppm, 10ppm, 20ppm" and "Al, As, Ba, Ca, Cd, Cr, Cu, Fe, Hg, K, Mg, Mn, Na, Ni, Pb, Si, Zn, concentrations of 0.1ppm, 0.2ppm, 0.5ppm, 1ppm, 2ppm" respectively. The main element marking lines and impurity element marking lines with a linearity of not less than 99.9% are respectively produced on the inductively coupled plasma spectrometer. The corresponding test conditions of the inductively coupled plasma emission spectrometer are set according to the above requirements.
[0111] The test results are as follows:
[0112] Main elements:
[0113]
[0114] It can be seen from the table that: (1) the relative standard deviations (RSDs) of the solution tests are all less than 2%, indicating that the ICP-OES test results are highly stable; (2) the measured contents of Li, La, and Ti are very close to the theoretical values of known samples; (3) the La element detected in solution H is significantly reduced, indicating that the La element has been effectively removed.
[0115] Impurity elements:
[0116]
[0117]
[0118] It can be seen from the table that: (1) the relative standard deviation (RSD) of the solution test is less than 1%, indicating that the ICP-OES test results are highly stable; (2) except for potassium, the impurity content test results in solution D are about 1.25 times that in solution E, indicating that the addition of HF does not affect the test results of other impurities; (3) the potassium content test results in solution E are significantly lower than those in solution D. Analysis of the original ICP data spectrum shows that there is obvious lanthanum spectral interference in the potassium detection in solution D, which makes the test results biased; (4) The spiked recovery rates of solution D and solution E also show that the spiked recovery rate of potassium in the solution after HF removal of La is closer to 100%, and the test results are more accurate.
[0119] Example 2
[0120] Take the known sample Li7La3Zr2O 12 , weigh 0.1153 g of LLZO sample with an analytical balance, put it into a microwave digestion tank, add 5 ml of 36% to 38% hydrochloric acid and 5 ml of 95% to 98% sulfuric acid with a pipette, put the digestion tank into a microwave digestion instrument, heat it at 200°C for 0.5 hour, take out and open the digestion tank, the sample is completely digested into a clear and transparent liquid (solution A), and the volume is adjusted to 51.13 g (solution C) with the solution B mentioned above.
[0121] Take 5.07g of liquid from solution C, add solution B to make up to 50.01g (solution D); take out 20.00±0.50g (accurate to the second decimal place) of solution C from solution C, add oxalic acid to make up to 25.00±1.00g (accurate to the second decimal place, the mixed solution at this time is recorded as solution E). Take out 10.00±0.50g (accurate to the second decimal place) of solution C from solution C, add 4g of standard solution with a concentration of 1ppm, and then add solution B to make up the volume to 20.00±1.00g (accurate to the second decimal place, the mixed solution at this time is recorded as solution F); take out 10.00±0.50g (accurate to the second decimal place) of solution E from solution E, add 4g of standard solution with a concentration of 1ppm, and then add solution B to make up the volume to 20.00±1.00g (accurate to the second decimal place, the mixed solution at this time is recorded as solution G); take out 5.00±0.50g (accurate to the second decimal place) of solution E from solution E, add solution B to make up the volume to 50.00±1.00g (accurate to the second decimal place, the mixed solution at this time is recorded as solution H).
[0122] According to the above requirements, use 3% dilute nitric acid to prepare standard solutions containing "Li, La, Zr elements, concentrations of 1ppm, 2ppm, 5ppm, 10ppm, 20ppm" and "Al, As, Ba, Ca, Cd, Cr, Cu, Fe, Hg, K, Mg, Mn, Na, Ni, Pb, Si, Zn, concentrations of 0.1ppm, 0.2ppm, 0.5ppm, 1ppm, 2ppm" respectively. On the inductively coupled plasma spectrometer, make the main element markings and impurity element markings with a linearity of not less than 99.9% respectively. Set the corresponding test conditions of the inductively coupled plasma emission spectrometer according to the above requirements.
[0123] The test results are as follows:
[0124] Main elements:
[0125]
[0126] It can be seen from the table that: (1) the relative standard deviations (RSDs) of the solution tests are all less than 2%, indicating that the ICP-OES test results are highly stable; (2) the measured contents of Li, La, and Zr are very close to the theoretical values of known samples; (3) the La element detected in solution H is significantly reduced, indicating that the La element has been effectively removed.
[0127] Impurity elements:
[0128]
[0129] It can be seen from the table that: (1) the relative standard deviation (RSD) of the solution test is less than 1%, indicating that the ICP-OES test results are highly stable; (2) except for potassium, the impurity content test results in solution D are about 1.25 times that in solution E, indicating that the addition of HF does not affect the test results of other impurities; (3) the potassium content test results in solution E are significantly lower than those in solution D. Analysis of the original ICP data spectrum shows that there is obvious lanthanum spectral interference in the potassium detection in solution D, which makes the test results biased; (4) The spiked recovery rates of solution D and solution E also show that the spiked recovery rate of K in the solution after HF removal of La is closer to 100%, and the test results are more accurate.
[0130] In summary, the method for detecting the impurity content of the lanthanum-containing solid electrolyte material provided by the present invention can not only completely eliminate the lithium lanthanum zirconium oxide type solid electrolyte mentioned in the prior art scheme disclosed in the background technology (including: the substance in various phases; the derivatives of the substance "in various phases formed after various doping"), but also completely eliminate the lithium lanthanum titanium oxide type solid electrolyte (including: the substance in various phases; the derivatives of the substance "in various phases formed after various doping"); while the prior art scheme disclosed in the background technology cannot completely eliminate the cubic phase lithium lanthanum zirconium oxide type solid electrolyte, therefore, the cubic phase derivatives formed by various doping of the substance (lithium lanthanum zirconium oxide type solid electrolyte) cannot be completely eliminated; at the same time, the prior art scheme disclosed in the background technology cannot even eliminate the lithium lanthanum titanium oxide type solid electrolyte. Moreover, the present invention enables the inductively coupled plasma spectrometer to more accurately determine the main elements in the corresponding solid electrolyte, and can also accurately determine the doping elements and impurity elements therein (because the doping element content is low, it can be measured together with the impurity elements in the determination), while the prior art solution disclosed in the background technology can only determine the main elements. For the determination of impurity elements, because the digestion steps of the prior art solution disclosed in the background technology are too cumbersome, a large number of impurity elements are artificially introduced into the original sample, resulting in the prior art solution disclosed in the background technology being completely inaccurate in determining the impurity elements in the original sample, and having no determination significance. Finally, the present invention greatly simplifies the digestion steps, saving a lot of manpower and material resources; at the same time, because the digestion steps are greatly simplified, the impurity elements artificially introduced into the original sample are greatly reduced, making it possible to accurately determine the impurity elements in the original sample. In addition, the present invention uses oxalic acid to treat the digested solution, so that oxalic acid combines with the La element in the solution to generate lanthanum fluoride that is insoluble in water and most acids, thereby greatly reducing the interference of the lanthanum element on the potassium element test, and greatly improving the accuracy of the test results of the potassium element.
[0131] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for detecting the impurity content of a lanthanum-containing solid electrolyte material, comprising the following steps: a) mixing the lanthanum-containing solid electrolyte material to be tested with an acid solution, performing a digestion reaction, and obtaining a digestion solution; b) After diluting the digestion solution obtained in step a), the main elements and impurity elements are tested respectively by inductively coupled plasma emission spectrometer, and the test results of each element are obtained by comparing with the marking lines of each element. Finally, the impurity content of the lanthanum-containing solid electrolyte material is obtained by calculation.
2. The detection method according to claim 1, characterized in that: The acid solution in step a) is hydrochloric acid with a mass fraction of 36% to 38% and / or sulfuric acid with a mass fraction of 95% to 98%.
3. The detection method according to claim 1, characterized in that: The digestion reaction in step a) is carried out by hydrothermal reaction in a reaction kettle or microwave reaction in a microwave digestion instrument; the temperature of the digestion reaction is 180° C. to 250° C., and the time is 0.5 h to 5 h.
4. The detection method according to claim 1, characterized in that: The dilution process in step b) is specifically as follows: The digestion solution is diluted to 50±5 g with a diluent to obtain a first solution; Take 5±0.5 g of the first solution and dilute it to 50±1 g with a diluent to obtain a second solution; Take 20±0.5g of the first solution and dilute to 25±1g with oxalic acid to obtain a third solution; Take 10±0.5g of the first solution, add 4±1g of a standard solution with a concentration of 1ppm, and then add a diluent to make the volume to 20±1g to obtain a fourth solution; Take 10±0.5g of the third solution, add 4±1g of a standard solution with a concentration of 1ppm, and then add a diluent to make the volume to 20±1g to obtain a fifth solution; Take 5±0.5 g of the third solution and dilute it to 50±1 g with a diluent to obtain a sixth solution.
5. The detection method according to claim 4, characterized in that: The diluent is prepared by mixing water with a volume ratio of 4:(0.8-1) and hydrochloric acid with a mass fraction of 36%-38%.
6. The detection method according to claim 4, characterized in that: The standard solution includes standard solutions of main elements and impurity elements with different concentrations, wherein the concentrations of the main elements are 1ppm, 2ppm, 5ppm, 10ppm, and 20ppm, respectively, and the concentrations of the impurity elements are 0.1ppm, 0.2ppm, 0.5ppm, 1ppm, and 2ppm, respectively.
7. The detection method according to claim 1, characterized in that: The test conditions for the main element and the impurity element in step b) include: For the elements Al, As, Cd, Cr, Cu, Fe, Hg, Mn, Ni, Pb, Si, and Zn, the RF power was 1–1.5 kW, the stabilization time was 14–16 s, and the observation mode was axial; For elements Ba, Ca, K, Mg, and Na, the RF power was 1–1.5 kW, the stabilization time was 4–6 s, and the observation mode was radial; For the elements Li, La, Zr, and Ti, the RF power was 1 to 1.5 kW, the stabilization time was 14 to 16 s, and the observation mode was radial.
8. The detection method according to claim 1, characterized in that: The element markings in step b) are obtained by testing standard solutions of main elements and impurity elements with different concentrations using an inductively coupled plasma emission spectrometer; the linearity of each element marking generated by the testing equipment is not less than 99.9%; the standard solution is diluted to the corresponding concentration using the same bottle of dilution solution, and the dilution solution is dilute nitric acid or dilute hydrochloric acid with a concentration range of 3% to 10%.
9. The detection method according to claim 1, characterized in that: The calculation in step b) uses the following formula: A1=a1×m2 / m1; Among them, A1 is the impurity element content, in ppm; a1 is the impurity element test result, in ppm; m2 is the mass of the first solution, in g; m1 is the mass of the lanthanum-containing solid electrolyte material to be tested, in g.
10. The detection method according to any one of claims 1 to 9, characterized in that: The step b) further comprises: The main element content of the lanthanum-containing solid electrolyte material is calculated; the calculation adopts the following formula: B1=b1×m2×5 / m1; Among them, B1 is the main element content, in ppm; b1 is the main element test result, in ppm; m2 is the mass of the first solution, in g; m1 is the mass of the lanthanum-containing solid electrolyte material to be tested, in g.
Citation Information
Patent Citations
Method for determining the inorganic element content in samples of lithium lanthanum zirconium oxide solid electrolyte
CN109540874B
A method for processing solid electrolytes and a method for testing the elemental content in solid electrolytes.