A processing technology for the back cover of a foldable screen electronic device

By combining sandblasting with stacked chamfering, the problems of decreased precision and wear in laser chamfering of UTG glass sheets have been solved, improving the anti-slip performance and yield of UTG glass sheets, ensuring the strength and toughness of UTG glass sheets, and extending the service life of products.

CN119927810BActive Publication Date: 2026-11-10BIEL OPTIC HUIZHOU +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510097498.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-01-22
Publication Date
2026-11-10
Estimated Expiration
2045-01-22

AI Technical Summary

Technical Problem

Existing technologies for processing flexible ultra-thin glass (UTG) result in decreased precision in laser chamfering, leading to insufficient glass yield. Furthermore, the surface of UTG glass is prone to slippage and wear, affecting the lifespan of mobile phones.

Method used

The process combines sandblasting and stacking chamfering. Sandblasting is performed on the skirt edge by using a sandblasting fixture, followed by stacking chamfering and polishing to ensure the strength and toughness of the UTG glass sheet. Double-sided etched chamfering is used to improve the yield rate.

Benefits of technology

This improves the anti-slip properties of UTG glass sheets, reduces the risk of wear, increases the yield rate of chamfering, ensures the strength and toughness of UTG glass sheets, and extends product lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119927810B_ABST
    Figure CN119927810B_ABST
Patent Text Reader

Abstract

This invention discloses a processing technology for the back cover of a foldable screen electronic device, comprising: S1, cutting and thinning glass to obtain a UTG glass sheet to be sandblasted, the UTG glass sheet including a part to be sandblasted and a skirt surrounding the part to be sandblasted; S2, loading the UTG glass sheet into a sandblasting fixture, exposing the part to be sandblasted to the sandblasting area of ​​the sandblasting equipment, and covering the skirt with the sandblasting fixture, and sandblasting the UTG glass sheet; S3, smoothing the UTG glass sheet; S4, cutting off the skirt of the smoothed UTG glass sheet and thinning the UTG glass sheet a second time; S5, stacking the UTG glass sheets after the second thinning to obtain a glass stack; S6, using CNC machining to chamfer the edges of the glass stack and polishing the body of the glass stack; S7, splitting the polished glass stack into several UTG glass sheets, protecting both sides and etching the chamfers of the UTG glass sheets to obtain the finished product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of foldable screen glass processing technology, and in particular to a processing technology for the back cover of foldable screen electronic devices, used to achieve sandblasting of the user surface and chamfering of the edge laminations of the back cover of foldable screen electronic devices. Background Technology

[0002] Flexible ultra-thin glass (UTG) boasts advantages such as high surface hardness and screen clarity, excellent light transmission, and good wear and high-temperature resistance. It also offers a pleasant tactile experience and achieves a balance between folding performance and mechanical strength, resisting wrinkles even after repeated folding. It can be used as a back cover for foldable screen phones, meeting the bending requirements while reducing the phone's weight. However, as the thickness of flexible ultra-thin glass decreases, while its light transmission and flexibility improve and weight is reduced, its mechanical strength decreases. Any impurities and microcracks will have a serious negative impact on ultra-thin glass. Currently, the industry mainly addresses this by chamfering UTG glass to balance its strength and toughness. Traditional chamfering processes often use laser chamfering, which offers high precision, high efficiency, and non-contact processing. However, when the thickness of the UTG glass is less than 50μm, the processing precision of laser chamfering decreases significantly, resulting in insufficient glass yield. In addition, due to the high smoothness of the UTG glass surface, there is a risk of the phone slipping due to unstable grip during use, as well as wear and scratches caused by the phone coming into contact with external objects, which in turn affects the phone's lifespan. Summary of the Invention

[0003] Therefore, it is necessary to address the above-mentioned shortcomings by providing a processing technology for the back cover of foldable electronic devices that combines stacked chamfering with sandblasting to improve the strength, toughness, feel, and anti-slip properties of UTG glass, thereby preventing wear and scratches on mobile phones and improving the yield rate of sandblasting and chamfering.

[0004] A manufacturing process for the back cover of a foldable screen electronic device includes the following steps:

[0005] S1. Cut and thin the glass once to obtain a UTG glass sheet to be sandblasted, the UTG glass sheet including a sandblasted portion and a skirt portion surrounding the sandblasted portion;

[0006] S2. Load the UTG glass sheet into the sandblasting fixture, expose the part to be sandblasted to the sandblasting operation area of ​​the sandblasting equipment, and cover the skirt part with the sandblasting fixture to sandblast the UTG glass sheet.

[0007] S3. Smooth the UTG glass sheet;

[0008] S4. Remove the skirt edge of the smoothed UTG glass sheet and perform a second thinning of the UTG glass sheet;

[0009] S5. Stack the UTG glass sheets after secondary thinning to obtain a glass laminate;

[0010] S6. The edges of the glass laminate are chamfered using CNC machining, and the body of the glass laminate is polished.

[0011] S7. The polished glass stack is split into several UTG glass sheets, and the edges of the UTG glass sheets are protected on both sides and etched to obtain the finished product.

[0012] In one embodiment, step S1 includes:

[0013] S11. Apply protective oil to both sides of the incoming glass material;

[0014] S12. Cut and bevel the glass material to obtain a rectangular glass sheet;

[0015] S13. Polish the glass sheet and remove the protective oil from the glass sheet surface;

[0016] S14. Place the glass sheet in the etching solution and thin it to 0.07-0.08 mm to obtain a UTG glass sheet;

[0017] S15. Apply protective oil to the system surface of the UTG glass plate.

[0018] In one embodiment, the sandblasting fixture includes:

[0019] A sandblasting base includes a concave base and a convex base that are oppositely arranged and interlocked. The upper surface of the concave base has a first groove, and a mounting notch is provided on one side of the concave base adjacent to the convex base. The first groove penetrates the side of the concave base where the mounting notch is located. The upper surface of the convex base has a second groove, and a mounting protrusion that interlocks with the mounting notch is provided on one side of the convex base adjacent to the concave base. The second groove penetrates the side of the convex base where the mounting protrusion is located.

[0020] A positioning frame, comprising a first U-shaped frame embedded in a first groove and fixedly connected to a concave base, and a second U-shaped frame embedded in a second groove and fixedly connected to a convex base. The upper surface of the first U-shaped frame is higher than the upper surface of the concave base, and the upper surface of the second U-shaped frame is higher than the upper surface of the convex base. The first and second U-shaped frames together form a limiting area for accommodating a UTG glass sheet, the height of which is less than or equal to the thickness of the UTG glass sheet.

[0021] An annular cover plate is pressed and fixed on the upper surfaces of the first U-shaped frame and the second U-shaped frame. The annular cover plate forms a sandblasting shielding area above the limiting area corresponding to the skirt edge of the UTG glass sheet, and the inner ring area of ​​the annular cover plate forms a sandblasting area corresponding to the sandblasting part of the UTG glass sheet.

[0022] In one embodiment, the first groove is provided with a plurality of first positioning holes and a plurality of first sand leakage holes, and the second groove is provided with a plurality of second positioning holes and a plurality of second sand leakage holes; the first U-shaped frame is provided with a plurality of third positioning holes corresponding to each of the first positioning holes and a plurality of first sand leakage notches corresponding to each of the first sand leakage holes, and the second U-shaped frame is provided with a plurality of fourth positioning holes corresponding to each of the second positioning holes and a plurality of second sand leakage notches corresponding to each of the second sand leakage holes; the annular cover plate is provided with a plurality of fifth positioning holes corresponding to each of the third positioning holes and the fourth positioning holes; the sandblasting base further includes a plurality of first mounting screws that sequentially pass through the fifth positioning holes, the third positioning holes, and the first positioning holes to connect the annular cover plate, the first U-shaped frame, and the concave base, and a plurality of second mounting screws that sequentially pass through the fifth positioning holes, the fourth positioning holes, and the second positioning holes to connect the annular cover plate, the second U-shaped frame, and the convex base.

[0023] In one embodiment, the sandblasting fixture further includes at least one baffle for shielding the skirt portion of the UTG glass sheet located in the sandblasting area. The baffle includes a horizontal bar straddling a concave base or a convex base, and two locking blocks oppositely arranged and fixed at both ends of the horizontal bar. The concave base has two oppositely arranged first slots on the outer side of a first groove, and the convex base has two oppositely arranged second slots on the outer side of a second groove. The two locking blocks of the baffle are embedded one-to-one into the two first slots and fixedly connected to the annular cover plate by a limiting screw passing through the annular cover plate, or the two locking blocks of the baffle are embedded one-to-one into the two second slots and fixedly connected to the annular cover plate by a limiting screw passing through the annular cover plate.

[0024] In one embodiment, step S3 includes:

[0025] S31. Remove the protective oil from the surface of the UTG glass system;

[0026] S32. Use an alkaline etching solution to etch the UTG glass sheet to smooth it out.

[0027] In one embodiment, step S5 includes:

[0028] S51. Apply adhesive between the stacked substrate and the UTG glass sheet or between two UTG glass sheets to form an adhesive-plate composition;

[0029] S52. UV light is used to cure the adhesive-board composition to form an adhesive layer;

[0030] S53. Bake the glue-board composition after the adhesive layer has cured;

[0031] S54. Repeat steps S51-S53 until a glass stack consisting of two opposing substrates and a plurality of UTG glass sheets stacked between the two substrates is formed.

[0032] In one embodiment, step S7 includes:

[0033] S71. De-adhere the glass stack so that the glass stack is separated into several UTG glass sheets;

[0034] S72. Apply a protective film to both sides of the UTG glass slide;

[0035] S73. Use alkaline etching solution to etch the edge chamfer of the UTG glass sheet;

[0036] S74. Remove the protective film from the surface of the UTG glass sheet.

[0037] In one embodiment, in step S71, the glass stack is placed in hot water to de-adhere.

[0038] In one embodiment, step S74 is followed by:

[0039] S75. Chemically strengthen the UTG glass sheet to harden it;

[0040] S76. The strengthened UTG glass sheet is placed in an alkaline etching solution for repolishing. After repolishing, the surface roughness Sa of the UTG glass sheet is less than 1 nm.

[0041] The back cover processing technology for foldable screen electronic devices implementing this invention uses a sandblasting fixture to shield the skirt of the UTG glass sheet, and removes the skirt in subsequent operations. This achieves sandblasting of the UTG glass sheet surface, improves the anti-slip performance of the glass sheet, reduces the risk of glass wear and scratches, and extends product lifespan. At the same time, it avoids the problem of glass sheet breakage caused by sandblasting particles contacting the edge of the glass sheet. Removing the skirt also reduces frame marks generated after product smoothing, which can reduce the defect rate of sandblasting. By chamfering and polishing the UTG glass sheets after stacking, burrs remaining from CNC machining of the UTG glass sheets can be removed without breaking the UTG glass sheets, ensuring the strength of the UTG glass sheets. By protecting the edges of the UTG glass sheets on both sides and etching the polished edges, the chamfering of UTG glass with a thickness of less than 40μm can be satisfied, which significantly improves the yield rate of chamfering while improving the strength and toughness of the UTG glass sheets. Attached Figure Description

[0042] Figure 1This is a flowchart of the manufacturing process of the back cover of a foldable screen electronic device in one embodiment of the present invention;

[0043] Figure 2 This is a schematic diagram of the structure of a UTG glass sheet to be sandblasted in one embodiment of the present invention;

[0044] Figure 3 This is a schematic diagram of the sandblasting fixture from one perspective in one embodiment of the present invention;

[0045] Figure 4 This is a schematic diagram of the sandblasting fixture from another perspective in one embodiment of the present invention;

[0046] Figure 5 This is an exploded view of a sandblasting fixture in one embodiment of the present invention;

[0047] Figure 6 This is a cross-sectional view of the sandblasting fixture in one direction according to one embodiment of the present invention;

[0048] Figure 7 This is a cross-sectional view of the sandblasting fixture in one direction according to one embodiment of the present invention;

[0049] Figure 8 This is a schematic cross-sectional view of the glass stack in one embodiment of the present invention;

[0050] Figure 9 This is a flowchart illustrating the manufacturing process of the back cover of a foldable screen electronic device in one embodiment of the present invention. Detailed Implementation

[0051] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0052] Please combine Figure 1-9 This invention discloses a processing technology for the back cover of a foldable screen electronic device. This processing technology is used to achieve sandblasting of the user surface and chamfering of the edge laminations of the back cover of the foldable screen electronic device, particularly for the processing of glass back covers for Apple mobile phones (iPhones) or tablets (iPads). Specifically, the processing technology includes the following steps:

[0053] S1. Cut and thin the glass in one step to obtain a UTG glass sheet 10 to be sandblasted. The UTG glass sheet includes a sandblasted portion 101 and a skirt portion 102 surrounding the sandblasted portion 101 (the structure of the UTG glass sheet is as follows). Figure 2(As shown).

[0054] Furthermore, step S1 includes:

[0055] S11. Apply protective oil to both sides of the incoming glass material.

[0056] In this embodiment, the glass material processed is Corning Gorilla Glass 7418, a type of non-grinding glass. In other embodiments, other commercially available types of non-grinding glass can also be used. Specifically, a protective oil is applied to both sides of the glass material via screen printing to prevent damage to the glass surface in subsequent processes. The protective oil used is acid-resistant protective ink of type 4500PN. The thickness of the acid-resistant protective ink coating on one side of the glass is 15-25 μm. The screen printing stencil used is type 77T. After the acid-resistant protective ink is applied, the glass surface is continuously heated at 175-185℃ for 3 minutes to dry the acid-resistant protective ink. Subsequently, the glass surface is continuously heated at 175-185℃ for 30 minutes to cure the acid-resistant protective ink.

[0057] S12. Cut and bevel the glass material to obtain a rectangular glass sheet.

[0058] Specifically, the large sheet of glass is first cut into smaller pieces to facilitate subsequent production processes. During the cutting process, diamond grinding wheels are used to cut the glass to a depth of 0.005-0.01mm, with a cutting pressure of 1-2MPa and a feed rate of 35000-60000mm / min. Subsequently, a CNC machine is used to machine the shape and chamfer of the cut glass, roughly shaping it to the customer's desired form. The shaping and chamfering process involves rough cutting followed by finish cutting. During both rough and finish cutting, the spindle speed is 28000-32000rpm, the rough cutting wheel is a 400# grit wheel with a feed rate of 80mm / min, and the finish cutting wheel is an 800# grit wheel with a feed rate of 130mm / min.

[0059] S13. Polish the glass sheet and remove the protective oil from the glass sheet surface.

[0060] Specifically, the glass sheet is first polished using a pig bristle brush to remove sharp edges or burrs generated during CNC machining, preventing scratches, breakage, and other defects in subsequent processes. During polishing, the pig bristles on the brush are 15-30mm long, the polishing speed is 1750-1850 rpm for the long side and 400-500 rpm for the short side. The polished glass sheet is then placed in an alkaline solution to remove the protective oil from its surface, minimizing the impact of the protective ink layer on the precision of the UTG glass thinning process. To remove the protective oil, the glass sheet is immersed in an 8-10% NaOH solution at 78-82℃ for 14-16 minutes to remove the protective ink layer from the glass sheet's surface.

[0061] S14. Place the glass sheet in the etching solution and thin it to 0.07-0.08 mm (i.e. 70-80 μm) to obtain a UTG glass sheet.

[0062] Specifically, first, weigh 45 kg of water using an electronic scale, then add 5 kg of NaG and 50 kg of NaOH in batches while stirring until the NaG and NaOH are completely dissolved, thus preparing a mixed solution with a mass fraction of 50% NaOH and 5% NaG, which is the etching solution. Then, place the glass slide in the etching solution and chemically thin the glass slide at a temperature of 115-125℃ until the thickness of the glass slide is reduced to 0.07-0.08 mm, thus achieving a single thinning of the glass slide.

[0063] S15. Apply protective oil to the system surface of the UTG glass plate.

[0064] For glass sheets etched to 0.07-0.08 mm using alkaline etching, a protective oil is screen-printed on the entire surface to prevent damage to the surface in subsequent processes. In this embodiment, the protective oil used is acid-resistant protective ink of model 4500PN. The thickness of the acid-resistant protective ink coating on one side of the glass is 15-25 μm. The screen printing stencil used is model 77T. After the acid-resistant protective ink is applied, the glass surface is continuously heated at 175-185℃ for 3 minutes to dry the acid-resistant protective ink. Subsequently, the glass surface is continuously heated at 175-185℃ for 30 minutes to cure the acid-resistant protective ink.

[0065] It should be noted that the length of the UTG glass sheet to be sandblasted, obtained after processes such as cutting, thinning, and applying protective oil, must be 30mm greater than the length of the finished product, and the width of the UTG glass sheet to be sandblasted must be 30mm greater than the width of the finished product. The area on the UTG glass sheet corresponding to the finished product forms the sandblasting portion 101. The width of the sandblasting portion 101 is 16-20mm smaller than the width of the UTG glass sheet to be sandblasted, and the length of the sandblasting portion 101 is 16-20mm smaller than the length of the UTG glass sheet to be sandblasted. The area extending beyond the edge of the finished product forms a skirt 102. During lamination, a 2mm section needs to be removed from one side. This removed section is also the sandblasting area. Therefore, the length of the sandblasting section 101 needs to be 4.028-4.032mm longer than the finished product length, and the width of the sandblasting section 101 needs to be 4.028-4.032mm wider than the finished product width. This avoids the problem of un-sandblasted areas on the product due to processing errors, ensuring that the user surface of the final product is sandblasted. The excess dimensions will be removed in subsequent processes such as CNC machining, surface etching, chamfer etching, and repolishing after lamination. During sandblasting, the skirt 102 is shielded so that the sandblasting equipment only sandblasts the sandblasting section 101 of the glass sheet, avoiding the problem of glass breakage caused by sand particles directly hitting the edge of the UTG glass sheet during sandblasting, thereby reducing the defect rate of the sandblasting operation.

[0066] S2. Load the UTG glass sheet into the sandblasting fixture 20, so that the part to be sandblasted 101 is exposed to the sandblasting operation area of ​​the sandblasting equipment, and make the sandblasting fixture 20 cover the skirt part 102 to sandblast the UTG glass sheet.

[0067] Please combine Figure 2-7The sandblasting fixture 20 includes a sandblasting base 100, a positioning frame 200, and an annular cover plate 300. The sandblasting base 100 includes a concave base 110 and a convex base 120 that are arranged opposite to each other and engaged. The upper surface of the concave base 110 is provided with a first groove 111, and a mounting notch 112 is provided on one side of the concave base 110 adjacent to the convex base 120. The first groove 111 penetrates the side of the concave base 110 where the mounting notch 112 is located. The upper surface of the convex base 120 is provided with a second groove 121, and a mounting protrusion 122 that engages with the mounting notch 112 is provided on one side of the convex base 120 adjacent to the concave base 110. The second groove 121 penetrates the side of the convex base 120 where the mounting protrusion 122 is located. The positioning frame 200 includes a first U-shaped frame 210 embedded in a first groove 111 and fixedly connected to a concave base 110, and a second U-shaped frame 220 embedded in a second groove 121 and fixedly connected to a convex base 120. The upper surface of the first U-shaped frame 210 is higher than the upper surface of the concave base 110, and the upper surface of the second U-shaped frame 220 is higher than the upper surface of the convex base 120. The first U-shaped frame 210 and the second U-shaped frame 220 together form a limiting area 230 for accommodating a UTG glass sheet. The height of the limiting area 230 is less than or equal to the thickness of the UTG glass sheet. The annular cover plate 300 presses against and fixes the upper surfaces of the first U-shaped frame 210 and the second U-shaped frame 220. The annular cover plate 300 forms a sandblasting shielding area corresponding to the skirt 102 of the UTG glass sheet above the limiting area 230. The inner ring area of ​​the annular cover plate 300 forms a sandblasting area corresponding to the sandblasting part 101 of the UTG glass sheet. The sandblasting shielding area can prevent the edge of the glass sheet from being placed in the sandblasting area of ​​the annular cover plate 300, and prevent the glass sheet from breaking due to the impact of sand particles on the edge of the glass sheet. Preferably, in this embodiment, the groove depth of the first groove 111 and the second groove 121 is 4mm, the thickness of the first U-shaped frame 210 and the second U-shaped frame 220 is 5mm, and the height of the limiting area 230 is 1mm. Since the thickness of the UTG glass sheet to be sandblasted is 0.07-0.08mm, the height of the limiting area 230 not only satisfies the limiting of the UTG glass sheet, preventing the UTG glass sheet 10 to be sandblasted from being crushed when the annular cover plate 300 is closed, but also allows the UTG glass sheet to be removed from the sandblasting base 100 by the positioning frame 200 after the UTG glass sheet sandblasting is completed, so as to prevent the UTG glass sheet from breaking when it is picked up. In addition, the shape of the first groove 111 is adapted to the shape of the first U-shaped frame 210, and the shape of the second groove 121 corresponds to the shape of the second U-shaped frame 220. That is to say, the first groove 111 and the second groove 121 are both U-shaped structures to prevent the positioning frame 200 from shaking on the sandblasting base 100.

[0068] In this embodiment, the sandblasting base 100 is designed with a snap-fit ​​connection between a concave base 110 and a convex base 120. After the UTG glass sheet is sandblasted, the snap-fit ​​connection between the concave base 110 and the convex base 120 is disassembled, allowing the concave base 110 and the convex base 120 to separate. Then, the positioning frame 200 is pushed, causing the positioning frame 200 to slide the UTG glass sheet off the sandblasting base 100. This avoids the problem of breakage of the sandblasted UTG glass sheet caused by handling it by hand or using a suction pen. During the assembly of the sandblasting fixture 20, the concave base 110 and the convex base 120 need to be assembled with the first U-shaped frame 210 and the second U-shaped frame 220 respectively before being spliced. During the disassembly of the sandblasting fixture 20, the process is exactly the opposite: the convex base 120 and the concave base 110 need to be disassembled first, and then each component installed on the concave base 110 and the convex base 120 needs to be disassembled one by one. The specific process is as follows:

[0069] 1) Clean the concave base 110 and the convex base 120.

[0070] 2) Assemble the positioning frame 200, and embed the first U-shaped frame 210 and the second U-shaped frame 220 into the first groove 111 of the concave base 110 and the second groove 121 of the convex base 120 respectively, ensuring that the outer edge of the short side of the first U-shaped frame 210 abuts against the inner edge of the short side of the concave base 110, and the outer edge of the short side of the second U-shaped frame 220 abuts against the inner edge of the short side of the convex base 120.

[0071] 3) Slide the UTG glass sheet along the upper surface of the concave base 110 into the first U-shaped frame 210, ensuring that the outer edge of the UTG glass sheet, which is adapted to the short side of the sandblasting fixture 20, abuts against the inner edge of the first U-shaped frame 210; or slide the UTG glass sheet along the upper surface of the convex base 120 into the second U-shaped frame 220, ensuring that the outer edge of the UTG glass sheet, which is adapted to the short side of the sandblasting fixture 20, abuts against the inner edge of the second U-shaped frame 220.

[0072] 4) The convex base 120 and the concave base 110 are spliced ​​together so that the UTG glass sheet is located between the first U-shaped frame 210 and the second U-shaped frame 220.

[0073] 5) Cover the annular cover plate 300, ensuring that the mounting parts on the annular cover plate 300 are aligned with the mounting parts on the first U-shaped frame 210, the second U-shaped frame 220, the concave base 110, and the convex base 120, and fix the annular cover plate 300, the first U-shaped frame 210, the second U-shaped frame 220, the concave base 110, and the convex base 120 together.

[0074] Furthermore, in this design, a limiting block is provided at the end of the mounting protrusion 122. The width of the limiting block is greater than the width of the mounting protrusion 122. The connection between the limiting block and the mounting protrusion 122 is provided with an arc transition part. The width difference between the limiting block and the mounting protrusion 122 is between 1-2mm. Correspondingly, a limiting groove adapted to the shape of the limiting block is provided in the mounting notch 112. In this way, through the mutual constraint of the limiting block and the limiting groove, it is convenient to disassemble the concave base 110 and the convex base 120, while avoiding displacement between the concave base 110 and the convex base 120 when the annular cover plate 300 is installed, thereby reducing the assembly difficulty of the sandblasting fixture 20.

[0075] Furthermore, in one embodiment, the first groove 111 is provided with a plurality of first positioning holes 113 and a plurality of first sand-leaking holes 114, and the second groove 121 is provided with a plurality of second positioning holes 123 and a plurality of second sand-leaking holes 124; the first U-shaped frame 210 is provided with a plurality of third positioning holes 211 corresponding to each of the first positioning holes 113 and a plurality of first sand-leaking notches 212 corresponding to each of the first sand-leaking holes 114, and the second U-shaped frame 220 is provided with a plurality of fourth positioning holes 221 corresponding to each of the second positioning holes 123 and a plurality of second sand-leaking notches corresponding to each of the second sand-leaking holes 124. 222; The annular cover plate 300 has a plurality of fifth positioning holes 310 corresponding to the third positioning holes 211 and the fourth positioning holes 221; The sandblasting base 100 also includes a plurality of first mounting screws 320 that pass through the fifth positioning holes 310, the third positioning holes 211, and the first positioning holes 113 in sequence to connect the annular cover plate 300, the first U-shaped frame 210, and the concave base 110, and a plurality of second mounting screws 330 that pass through the fifth positioning holes 310, the fourth positioning holes 221, and the second positioning holes 123 in sequence to connect the annular cover plate 300, the second U-shaped frame 220, and the convex base 120. In this embodiment, after the UTG glass sheet is loaded and the components of the sandblasting fixture 20 are assembled, the annular cover plate 300, the first U-shaped frame 210 and the concave base 110 are fixed by the first mounting screw 320, and the annular cover plate 300, the second U-shaped frame 220 and the convex base 120 are fixed by the second mounting screw 330. This can prevent the relative movement of the positions of the sandblasting base 100, the positioning frame 200 and the annular cover plate 300 during the sandblasting process, which could lead to the problem of poor sandblasting position of the UTG glass sheet, thus ensuring the sandblasting quality of the UTG glass sheet. In this solution, by opening a first sand-leaking notch 212 on the first U-shaped frame 210, a second sand-leaking notch 222 on the second U-shaped frame 220, a first sand-leaking hole 114 on the concave base 110, and a second sand-leaking hole 124 on the convex base 120, the sand-water mixture sprayed during the sandblasting process can flow in a timely manner into the sandblasting pipe through the aforementioned sand-leaking notches and holes for circulation, avoiding the optical defects of the sandblasted glass caused by the sand-water mixture covering the glass sheet surface. Further preferably, in this embodiment, multiple first positioning holes 113 and multiple first sand-leaking holes 114 are evenly distributed within the first groove 111, multiple second positioning holes 123 and multiple second sand-leaking holes 124 are evenly distributed within the second groove 121, multiple third positioning holes 211 and multiple first sand-leaking notches 212 are evenly distributed on the first U-shaped frame 210, and multiple fourth positioning holes 221 and multiple second sand-leaking notches 222 are evenly distributed on the second U-shaped frame 220.

[0076] In one embodiment, the sandblasting fixture 20 further includes at least one baffle 400 for shielding the skirt portion 102 of the UTG glass sheet located in the sandblasting area. The baffle 400 includes a horizontal bar 410 spanning a concave base 110 or a convex base 120, and two locking blocks 420 oppositely arranged and fixed at both ends of the horizontal bar 410. The concave base 110 has two oppositely arranged first slots 115 on the outer side of the first groove 111, and the convex base 120 has two oppositely arranged second slots 125 on the outer side of the second groove 121. The two locking blocks 420 of the baffle 400 are embedded one-to-one into the two first slots 115 and fixedly connected to the annular cover plate 300 by a limiting screw passing through the annular cover plate 300, or the two locking blocks 420 of the baffle 400 are embedded one-to-one into the two second slots 125 and fixedly connected to the annular cover plate 300 by a limiting screw 500 passing through the annular cover plate 300. Preferably, the depth of the first slot 115 and the second slot 125 is 10mm, so as to increase the mating area between the stop bar 400 and the concave base 110 or the convex base 120, prevent the stop bar 400 from sliding out of the first slot 115 or the second slot 125 under strong pulling, and improve the reliability of the first slot 115 and the second slot 125 in limiting the stop bar 400. During the assembly of the sandblasting fixture 20, after the annular cover plate 300 is fixedly connected to the sandblasting base 100 and the positioning frame 200, the locking block 420 of the baffle 400 is inserted into the first locking groove 115 or the second locking groove 125. The baffle 400 is moved so that it slides to the position of the skirt part 102 on the UTG glass sheet that is not covered by the annular cover plate 300 and the limiting screw 500 is locked. This fixes the baffle 400 on the sandblasting base 100, so as to prevent the baffle 400 from moving relative to the sandblasting base 100 when subjected to horizontal force, which would cause the edge of the UTG glass sheet to be directly impacted by sand particles and break.

[0077] It should be noted that in this embodiment, by setting a baffle 400 on the sandblasting base 100, the sandblasting of UTG glass of different sizes can be met, avoiding the scrapping of the sandblasting fixture due to changes in the size of the sandblasted UTG glass, thereby reducing the development cycle and saving costs. That is to say, when the size of the glass sheet to be sandblasted is smaller than the size of the sandblasting area, the sandblasting fixture can still be used to clamp the glass sheet, and the baffle 400 can be used to shield the skirt 102 of the glass sheet located in the sandblasting area to prevent the edge of the glass sheet from breaking under the impact of sand particles; when the sandblasting fixture 20 includes one or more baffles 400, an appropriate number of baffles 400 can be selected and their positions adjusted according to the size of the skirt of different glass sheets to be sandblasted, so as to ensure that the baffles 400 effectively shield the skirt of the glass sheet. In addition, in this solution, the weight of the sandblasting fixture 20 is greater than that of the traditional one-piece sandblasting base 100. This can avoid the problem of uneven sandblasting of the product caused by the sandblasting base 100 running at an inconsistent speed on the sandblasting machine slide rail under the action of non-vertical force when the weight of the sandblasting base 100 is insufficient.

[0078] In the sandblasting operation of UTG glass sheets, the UTG glass sheets are clamped into the sandblasting fixture 20 and fed into the sandblasting equipment. The sandblasting parameters of the sandblasting equipment are set, including a sandblasting pressure of 0.3-0.35MPa, a distance between the nozzle and the substrate (UTG glass sheet) of 215-235mm, and an angle between the nozzle and the substrate of 88-92°. The conveying speed of the sandblasting fixture 20 on the sandblasting equipment is 0.15-0.25m / mins. White corundum abrasive is used for sandblasting, with a particle diameter D50 of 19-21um, a sand-to-water ratio of 1:3, and a sand-to-water stirring frequency of 40Hz. Then, the UTG glass sheets are sandblasted.

[0079] S3. Smooth the UTG glass sheet to eliminate the bending problem of the sandblasted surface (user side) caused by the inability to release the stress on the sandblasted surface during the sandblasting process. This facilitates the production and processing of the UTG glass sheet in subsequent processes and eliminates the impact on the yield of subsequent processes such as glass sheet cutting.

[0080] Step S3 includes:

[0081] S31. Remove the protective oil from the UTG glass system surface to avoid affecting subsequent processes. To remove the protective oil, place the glass sheet in a NaOH solution with a mass fraction of 5-8% and a temperature of 80-90℃ for 8-12 minutes to remove the protective ink layer from the glass system surface.

[0082] S32. Use an alkaline etching solution to etch the UTG glass sheet to smooth it out. Specifically, first weigh 45 kg of water using an electronic scale, then add 5 kg of NaG and 50 kg of NaOH in batches while stirring until the NaG and NaOH are completely dissolved, thus preparing a mixture of 50% NaOH and 5% NaG by mass, which is the alkaline etching solution. Then, place the glass sheet in the alkaline etching solution and chemically etch the glass sheet at a temperature of 115-125℃, removing 0.005 mm of thickness on one side of the UTG glass sheet.

[0083] S4. Remove the skirt portion 102 of the smoothed UTG glass sheet and perform a second thinning of the UTG glass sheet.

[0084] In this embodiment, by removing the skirt portion 102 of the smoothed UTG glass sheet, the edge of the UTG glass sheet is prevented from being directly blasted by white corundum abrasive, which could cause the glass sheet to crack. Simultaneously, the frame marks generated during the smoothing process are removed, resulting in the desired product dimensions (the length and width of the glass sheet after removing the skirt portion 102 are 4.028-4.032mm larger than the final product's dimensions; this dimension must match the dimensions reserved during sandblasting. Any excess dimensions will be removed in subsequent processes such as CNC machining, surface etching, chamfering etching, and re-polishing). Specifically, the skirt portion 102 of the UTG glass sheet is removed using laser cutting. The cutting equipment is a laser cutting machine with a laser wavelength of 1030nm, a maximum power of 100W, a cutting speed of 150mm / s, a cutting frequency of 30000Hz, a duty cycle of 80%, and a dot pitch of 5μm. The secondary thinning of the UTG glass sheet aims to remove microcracks on the sandblasted surface, enhance the strength and toughness of the sandblasted UTG glass sheet, and further thin the UTG glass sheet to give it good bending properties. During the secondary chemical thinning, 45 kg of water is first weighed using an electronic scale. Then, 5 kg of NaG and 50 kg of NaOH are added in batches while stirring until the NaG and NaOH are completely dissolved, thus preparing a mixture of 50% NaOH and 5% NaG by mass. This becomes the etching solution. The glass sheet is then placed in the etching solution, and chemical thinning is performed at 115-125℃, resulting in an etching removal of 14-16 μm on one side of the UTG glass sheet.

[0085] It should be noted that the thickness of the UTG glass sheet to be sandblasted in this solution is 70-80μm (75μm in this embodiment). This is because the sandblasting breakage rate increases significantly when the thickness of the sandblasted UTG sample is less than 70μm. The total removal of sandblasting surface smoothing and chemical thinning is 16.5-18.5μm. This is because when the sandblasting surface removal is less than 15μm, the removal of microcracks on the sandblasted surface is insufficient, and the strength and toughness of the UTG sandblasted sample cannot meet the customer's requirements; while when the sandblasting surface removal is greater than 20μm, the sandblasting surface depth is insufficient and cannot meet the optical and roughness requirements of the sandblasted surface. After smoothing and chemical thinning, the total thickness of the UTG glass sheet is 39-41μm, which can also meet the thickness requirements of the back cover of the foldable screen electronic device. During the chemical thinning process, the glass in contact with the chemical thinning fixture will produce frame marks due to the different etching speeds compared to other parts. These marks can be removed during the subsequent lamination and chamfering process.

[0086] S5. Stack the UTG glass sheets after secondary thinning to obtain a glass laminate (the structure of the glass laminate is as follows). Figure 8 (As shown).

[0087] Step S5 includes:

[0088] S51. Apply adhesive between the stacked substrate 30 and the UTG glass sheet or between two UTG glass sheets 10 to form an adhesive-plate composition.

[0089] Step S51 further includes:

[0090] S511, Ultrasonic Cleaning: Ultrasonic cleaning is used to remove stains and grease remaining on the surface of the UTG glass sheet during the chemical thinning process. Specifically, the substrate 30 to be bonded and the surface of the UTG glass sheet are cleaned and kept dry to ensure there is no grease on the surface. Then, the bonding surfaces on both sides of the glass sheet are subjected to plasma cleaning treatment.

[0091] S512. Adhesive Path Design: The adhesive path design involves calculating the volume of cured adhesive based on the size of the adhesive application area and the adhesive thickness, and then calculating the adhesive solid content (non-volatile matter content) using the following formula:

[0092] X = (V1 / V)·100

[0093] Where X is the content of non-volatile matter (in %), V1 is the volume of the adhesive after curing, and V is the volume of the adhesive before curing.

[0094] Calculate the volume of glue using the following formula:

[0095] V = LxWxH

[0096] Where L is the length of the adhesive, determined by the area to be applied; W is the width of the adhesive, determined by the diameter of the dispensing needle; H is the height of the adhesive, determined by the dispensing speed; and V is the volume of the adhesive before curing. Based on the above calculations and the outline of the sample's dispensing area, the dispensing circuit diagram can be designed.

[0097] S513. Fix the substrate 30 onto the dispensing fixture. Apply adhesive to the edges of holes (if holes are present) on the bonding surface (upper surface) of the substrate 30 and around the glass to form a dam. The dam should be 0.6-0.8 mm away from the edge of the substrate 30. Then, pre-cure the dam to set its shape. The pre-cured light intensity is 750-850 mW / cm². 2 The pre-curing time is 11-13 seconds. In this solution, the purpose of applying adhesive to the substrate 30 and the glass sheet is to prevent the adhesive from overflowing from the substrate 30 or the glass, which would lead to insufficient adhesive.

[0098] S514. Apply a second layer of adhesive to the area enclosed by the dammed adhesive on the substrate 30 to form a filler adhesive. The amount of filler adhesive is greater than the amount required for bonding the UTG glass sheet. Excess filler adhesive will overflow from the periphery of the glass sheet and the edges of holes (if there are holes) during the bonding of the UTG glass sheet. Attach the bonding surface of the UTG glass sheet to the corresponding position on the substrate 30, and then apply a downward pressing force to complete the bonding of the single UTG glass sheet to the substrate 30.

[0099] S52. The adhesive-board composition is irradiated with UV light (ultraviolet light) to cure the adhesive and form an adhesive layer 40.

[0100] In this embodiment, stacking UTG glass sheets using UV light irradiation is to rapidly cure the adhesive, thereby shaping the adhesive-sheet composition and preventing lateral displacement of the glass sheets during subsequent stacking. During UV curing, 365nm wavelength UV light is used to pre-cur the stacked UTG glass sheets for 6 seconds, followed by a final curing of 40 seconds. The curing energy is 1500-2000 mJ / cm². 2 .

[0101] S53. The adhesive-board composition after the adhesive layer 40 is cured is baked to remove small molecules and water generated during UV adhesive curing. The baking temperature is 80℃ and the baking time is 60min.

[0102] S54. Repeat steps S51-S53 until a glass stack is formed, consisting of two opposing substrates 30 and a plurality of UTG glass sheets stacked between the two substrates 30. When bonding the bottom UTG glass sheet to the substrate 30, each UTG glass sheet is sequentially stacked and bonded onto the substrate. Each glass sheet has an adhesive layer 40 on both its upper and lower surfaces. When the stack height of the glass sheets reaches a preset value, another substrate 30 is bonded to the upper surface of the topmost glass sheet, and the adhesive layer 40 is cured and baked. In this embodiment, the thickness of the substrate 30 is 0.405 mm, the thickness of a single layer of adhesive is 0.02 mm, and 10 layers of UTG glass sheets are stacked between the two substrates 30 separated by an adhesive layer. It should be noted that due to a 0-1.5mm offset during the stacking process, the length and width of the stacked glass are designed to be 4.028-4.032mm larger than the dimensions of the chamfered edges of the CNC-machined glass stack. This offset will be removed during the chamfering process of the CNC-machined glass stack.

[0103] S6. CNC machining is used to chamfer the edges of the glass laminate to roughly shape it according to the customer's requirements, and then polishing the glass laminate body to form the desired 3D chamfer. During the chamfering process, rough cutting is performed first, followed by finish cutting. The spindle speed for both rough and finish cutting is 28,000-32,000 rpm. A 400# grit wheel is used for rough cutting, with a feed rate of 80 mm / min. An 800# grit wheel is used for finish cutting, with a feed rate of 130 mm / min. For polishing the glass laminate body, a bristle brush with bristles 15-30 mm long is used. The speed for polishing the long side of the glass laminate is 1750-1850 rpm, and the speed for polishing the short side is 400-500 rpm. After the glass body is polished, ultrasonic cleaning is used to remove stains and grease remaining on the glass surface.

[0104] S7. The polished glass stack is split into several UTG glass sheets, and the edges of the UTG glass sheets are protected on both sides and etched to obtain the finished product.

[0105] Step S7 includes:

[0106] S71. De-adhere the glass laminate to separate it into several UTG glass sheets for subsequent processing. In step S71, the glass laminate is placed in hot water to de-adhere. Specifically, the glass laminate is placed in deionized water at 75-85℃ and continuously immersed for 28-32 minutes to soften the adhesive and allow it to detach from the surface of the glass sheets.

[0107] S72. Apply a protective film to both sides of the UTG glass plate.

[0108] It should be noted that the protective film used in this embodiment is a commercially available UV anti-adhesion and alkali-resistant protective film. For example, the HSD-206F UV anti-adhesion protective film produced by Dongguan Hongshengda New Material Co., Ltd. can be used, or other brands or models of UV anti-adhesion and alkali-resistant protective films can be used. The thickness of the UV anti-adhesion and alkali-resistant protective film is 50μm. The application requirements are as follows: under normal temperature conditions for the film material and fixture, the UV anti-adhesion and alkali-resistant protective film is applied to the surface of the UTG glass sheet using compressed air at 55-65KPa. The pre-forming air pressure during application is 15-25KPa, the pre-forming delay is 1s, and the compressed air flow rate is 25-35%. By applying the protective film to both sides of the UTG glass sheet, the impact on other parts of the glass sheet can be avoided when the edges of the glass sheet are beveled by alkaline etching.

[0109] S73. Use alkaline etching solution to etch the chamfered edges of the UTG glass sheet.

[0110] Specifically, first, weigh 45 kg of water using an electronic scale. Then, add 5 kg of NaG and 50 kg of NaOH in batches while stirring until the NaG and NaOH are completely dissolved, thus preparing a mixture of 50% NaOH and 5% NaG by mass, which is the etching solution. Subsequently, place the coated glass slide in the etching solution and chemically etch the glass slide at a temperature of 115-125℃. The removal amount on one side of the glass slide is 0.01 mm, and the etching time is 60 min. This allows the exposed glass slide to be etched with NaOH by the alkaline etching solution under double-sided protection, forming an edge chamfer.

[0111] S74. Remove the protective film from the surface of the UTG glass sheet. After chemical etching, remove the protective film from the surface of the UTG glass sheet using UV light adhesion reduction. Specifically, the conditions for UV light adhesion reduction are as follows: irradiate the glass sheet with a 365nm LED light source, and the light energy is 600-1000mJ / m². 2 The irradiation time is 180 seconds.

[0112] Step S74 is followed by:

[0113] S75. Chemically strengthen the UTG glass sheet to harden it. Specifically, preheat the glass sheet at 380-400℃ for 59-61 minutes, then add 100% solid KNO3 to the hardening furnace, calculating the mass W1 of added KNO3. Raise the temperature to 409-411℃ until all KNO3 melts, then add 100% H2SiO3, with the mass W = W1 * (0.5 / 99.5). Continue strengthening at 409-411℃ for 29-31 minutes (with the glass sheet suspended for hardening for 1 minute) to increase the hardness of the glass sheet.

[0114] S76. The strengthened UTG glass sheet is placed in an alkaline etching solution for repolishing. After repolishing, the surface roughness Sa of the UTG glass sheet is less than 1 nm. In this scheme, by repolishing the strengthened glass sheet, the unevenness formed on the glass surface during the strengthening process can be removed, thereby reducing the surface roughness of the glass sheet. During repolishing, 45 kg of water is weighed using an electronic scale, and then 5 kg of NaG and 50 kg of NaOH are added in batches while stirring until NaG and NaOH are completely dissolved, thereby preparing a mixture of 50% NaOH and 5% NaG by mass, which is the etching solution. The coated glass sheet is then placed in the etching solution, and the glass sheet is chemically etched at a temperature of 115-125°C. A very small thickness will be removed during the repolishing of the UTG glass sheet. The thickness removal during repolishing should be controlled to be consistent with the thickness increase during the UTG glass strengthening process. Preferably, the removal amount on one side of the glass sheet is 0.004-0.006 mm.

[0115] In this invention, in order to improve the sandblasting and chamfering quality of the UTG glass sheet, a number of hypotheses were proposed to address the current problems of the back cover of foldable screen electronic devices, and the results were verified through repeated adjustments, as shown in the table below:

[0116]

[0117]

[0118] The back cover processing technology of the foldable screen electronic device of the present invention uses a sandblasting fixture 20 to shield the skirt 102 of the UTG glass sheet and removes the skirt 102 in subsequent operations. This achieves sandblasting of the UTG glass sheet surface, improves the anti-slip performance of the glass sheet, reduces the risk of glass sheet wear and scratches, and extends the product's service life. At the same time, it avoids the problem of glass sheet breakage caused by sandblasting particles contacting the edge of the glass sheet. Removing the skirt 102 also reduces frame marks generated after the product is smoothed, which can reduce the defect rate of sandblasting. By chamfering and polishing the UTG glass sheets after stacking, the burrs remaining from the CNC machining of the UTG glass sheets can be removed without breaking the UTG glass sheets, ensuring the strength of the UTG glass sheets. By protecting the edges of the UTG glass sheets on both sides and etching the polished edges, the chamfering of UTG glass with a thickness of less than 40μm can be satisfied. This significantly improves the yield rate of chamfering while improving the strength and toughness of the UTG glass sheets.

[0119] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0120] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A processing technology for the back cover of a foldable screen electronic device, characterized in that, Includes the following steps: S1. Cut and thin the glass once to obtain a UTG glass sheet to be sandblasted, the UTG glass sheet including a sandblasted portion and a skirt portion surrounding the sandblasted portion; S2. Load the UTG glass sheet into the sandblasting fixture, so that the part to be sandblasted is exposed to the sandblasting operation area of ​​the sandblasting equipment, and make the sandblasting fixture cover the skirt part to sandblast the UTG glass sheet to improve the anti-slip performance of the glass sheet. S3. Smooth the UTG glass sheet; S4. Remove the skirt edge of the smoothed UTG glass sheet and perform a second thinning of the UTG glass sheet; S5. Stack the UTG glass sheets after secondary thinning to obtain a glass laminate; S6. The edges of the glass laminate are chamfered using CNC machining, and the body of the glass laminate is polished. S7. The polished glass stack is separated into several UTG glass sheets. The edges of the UTG glass sheets are protected on both sides and the chamfers are etched to obtain the finished product. The sandblasting fixture includes: A sandblasting base includes a concave base and a convex base that are oppositely arranged and interlocked. The upper surface of the concave base has a first groove, and a mounting notch is provided on one side of the concave base adjacent to the convex base. The first groove penetrates the side of the concave base where the mounting notch is located. The upper surface of the convex base has a second groove, and a mounting protrusion that interlocks with the mounting notch is provided on one side of the convex base adjacent to the concave base. The second groove penetrates the side of the convex base where the mounting protrusion is located. A positioning frame, comprising a first U-shaped frame embedded in a first groove and fixedly connected to a concave base, and a second U-shaped frame embedded in a second groove and fixedly connected to a convex base. The upper surface of the first U-shaped frame is higher than the upper surface of the concave base, and the upper surface of the second U-shaped frame is higher than the upper surface of the convex base. The first and second U-shaped frames together form a limiting area for accommodating a UTG glass sheet, the height of which is less than or equal to the thickness of the UTG glass sheet. An annular cover plate is pressed and fixed on the upper surfaces of the first U-shaped frame and the second U-shaped frame. The annular cover plate forms a sandblasting shielding area above the limiting area corresponding to the skirt edge of the UTG glass sheet. The inner ring area of ​​the annular cover plate forms a sandblasting area corresponding to the sandblasting part of the UTG glass sheet. The first groove is provided with a plurality of first positioning holes and a plurality of first sand leakage holes, and the second groove is provided with a plurality of second positioning holes and a plurality of second sand leakage holes; the first U-shaped frame is provided with a plurality of third positioning holes corresponding to each of the first positioning holes and a plurality of first sand leakage notches corresponding to each of the first sand leakage holes, and the second U-shaped frame is provided with a plurality of fourth positioning holes corresponding to each of the second positioning holes and a plurality of second sand leakage notches corresponding to each of the second sand leakage holes; the annular cover plate is provided with a plurality of fifth positioning holes corresponding to each of the third positioning holes and the fourth positioning holes; the sandblasting base also includes a plurality of first mounting screws that sequentially pass through the fifth positioning holes, the third positioning holes, and the first positioning holes to connect the annular cover plate, the first U-shaped frame, and the concave base, and a plurality of second mounting screws that sequentially pass through the fifth positioning holes, the fourth positioning holes, and the second positioning holes to connect the annular cover plate, the second U-shaped frame, and the convex base; The sandblasting fixture further includes at least one baffle for shielding the skirt portion of the UTG glass sheet located in the sandblasting area. The baffle includes a horizontal bar straddling a concave or convex base and two locking blocks oppositely arranged and fixed at both ends of the horizontal bar. The concave base has two oppositely arranged first slots on the outer side of the first groove, and the convex base has two oppositely arranged second slots on the outer side of the second groove. The two locking blocks of the baffle are embedded one-to-one into the two first slots and fixedly connected to the annular cover plate by a limiting screw passing through the annular cover plate, or the two locking blocks of the baffle are embedded one-to-one into the two second slots and fixedly connected to the annular cover plate by a limiting screw passing through the annular cover plate.

2. The processing technology for the back cover of a foldable screen electronic device according to claim 1, characterized in that, Step S1 includes: S11. Apply protective oil to both sides of the incoming glass material; S12. Cut and bevel the glass material to obtain a rectangular glass sheet; S13. Polish the glass sheet and remove the protective oil from the glass sheet surface; S14. Place the glass sheet in the etching solution and thin it to 0.07-0.08 mm to obtain a UTG glass sheet; S15. Apply protective oil to the system surface of the UTG glass plate.

3. The processing technology for the back cover of a foldable screen electronic device according to claim 2, characterized in that, Step S3 includes: S31. Remove the protective oil from the surface of the UTG glass system; S32. Use an alkaline etching solution to etch the UTG glass sheet to smooth it out.

4. The processing technology for the back cover of a foldable screen electronic device according to claim 1, characterized in that, Step S5 includes: S51. Apply adhesive between the stacked substrate and the UTG glass sheet or between two UTG glass sheets to form an adhesive-plate composition; S52. UV light is used to cure the adhesive-board composition to form an adhesive layer; S53. Bake the glue-board composition after the adhesive layer has cured; S54. Repeat steps S51-S53 until a glass stack consisting of two opposing substrates and a plurality of UTG glass sheets stacked between the two substrates is formed.

5. The processing technology for the back cover of a foldable screen electronic device according to claim 1, characterized in that, Step S7 includes: S71. De-adhere the glass stack so that the glass stack is separated into several UTG glass sheets; S72. Apply a protective film to both sides of the UTG glass slide; S73. Use alkaline etching solution to etch the edge chamfer of the UTG glass sheet; S74. Remove the protective film from the surface of the UTG glass sheet.

6. The processing technology for the back cover of a foldable screen electronic device according to claim 5, characterized in that, In step S71, the glass laminate is placed in hot water to de-adhere.

7. The processing technology for the back cover of a foldable screen electronic device according to claim 5, characterized in that, Step S74 is followed by: S75. Chemically strengthen the UTG glass sheet to harden it; S76. The strengthened UTG glass sheet is placed in an alkaline etching solution for repolishing. After repolishing, the surface roughness Sa of the UTG glass sheet is less than 1 nm.

Citation Information

Patent Citations

  • Preparation method of ultrathin glass

    CN110052898A

  • Glass manufacturing method for manufacturing thin cover glass

    CN111452225A