A method for microwave-assisted multi-stage gradient acid leaching of lithium from lepidolite

By employing a microwave-assisted multi-level gradient acid leaching method for lithium extraction from lepidolite, combining mechanochemical activation, multi-level gradient acid leaching, and microwave-assisted technology, highly efficient and selective lithium extraction has been achieved, solving the problems of high energy consumption, low leaching efficiency, and severe environmental pollution in traditional lepidolite lithium extraction technologies.

CN121674736BActive Publication Date: 2026-11-10YICHUN JIANGLI LITHIUM BATTERY NEW ENERGY IND RES INST +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202511835949.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-12-08
Publication Date
2026-11-10
Estimated Expiration
2045-12-08

AI Technical Summary

Technical Problem

Traditional lithium extraction technology from lepidolite suffers from problems such as high energy consumption, low leaching efficiency, difficulty in selectively separating impurities, and serious environmental pollution.

Method used

A lithium extraction method using lepidolite microwave-assisted multi-stage gradient acid leaching is employed, which includes mechanochemical activation in the pretreatment stage, multi-stage gradient acid leaching, and a microwave-assisted enhancement system. The selective stepwise dissolution of lithium is achieved through a three-stage gradient acidic environment and a directional microwave field, combined with impurity removal using a precipitant.

Benefits of technology

It achieves efficient and selective lithium extraction, reduces energy consumption and environmental pollution, simplifies subsequent purification processes, improves lithium leaching rate and impurity control, and solves several problems existing in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMAGE_0BC1D5D1-A3EE-4682-B3B0-523D63B60DB4
    Figure IMAGE_0BC1D5D1-A3EE-4682-B3B0-523D63B60DB4
  • Figure IMAGE_12A75615-8722-4D2B-A2CC-1261A4D3386A
    Figure IMAGE_12A75615-8722-4D2B-A2CC-1261A4D3386A
  • Figure IMAGE_549D4ABE-5332-4613-B425-51904E3C9CEF
    Figure IMAGE_549D4ABE-5332-4613-B425-51904E3C9CEF
Patent Text Reader

Abstract

This invention belongs to the field of lithium resource recovery and extraction technology, specifically relating to a method for microwave-assisted multi-stage gradient acid leaching of lithium from lepidolite. The technical solution of this invention is as follows: a structure-destroying agent is added to lepidolite concentrate, followed by grinding and pre-leaching to obtain activated lepidolite concentrate; a first-stage acid and a configuration modifier are added to the activated lepidolite concentrate, followed by primary leaching and filtration to obtain leachate one and leach residue one; a second-stage acid is added to leach residue one, and microwaves are introduced, followed by secondary leaching and filtration to obtain leachate two and leach residue two; a third-stage acid is added to leach residue two, and microwaves are introduced, followed by tertiary leaching and filtration to obtain leachate three and leach residue three; leachate one, leachate two, and leachate three are combined to obtain a lithium-containing leachate; a precipitant is added to the lithium-containing leachate and the pH is controlled, followed by concentration, addition of a lithium-precipitating agent, and filtration to obtain filtrate and lithium carbonate product. The main purpose of this invention is to improve the leaching and extraction efficiency of lithium.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium resource recovery and extraction technology, specifically relating to a method for microwave-assisted multi-stage gradient acid leaching extraction of lithium from lepidolite. Background Technology

[0002] Current lithium extraction technologies from lepidolite largely rely on traditional sulfate roasting, acid leaching, and alkaline boiling methods. However, these traditional processes generally suffer from the following prominent problems: (1) High energy consumption and equipment cost: The process needs to be carried out under high temperature or high pressure conditions of 900-1050℃, which not only results in significantly high energy consumption, but also imposes strict requirements on the high temperature and high pressure resistance of the equipment, leading to high equipment purchase and maintenance costs. (2) Insufficient leaching efficiency and selectivity: The subsequent leaching process lacks efficient energy input or auxiliary enhancement methods, and relies more on simple multi-stage countercurrent leaching process, which makes it difficult to effectively destroy the stable crystal structure of lepidolite. This results in slow lithium leaching rate and low efficiency, and also makes it impossible to achieve selective separation of lithium from impurity elements. (3) The subsequent purification is difficult: A large amount of impurity ions such as aluminum and iron are easily dissolved in the leachate. These impurities are easy to combine with lithium in the lithium recovery process to form substances that are difficult to separate, resulting in additional lithium loss and significantly increasing the complexity and cost of the subsequent purification process. (4) Poor environmental friendliness: High-temperature roasting and strong acid and alkali leaching processes are prone to generating harmful gases or waste liquids. If not handled properly, they will cause environmental pollution, which does not meet the current development needs of green chemical industry.

[0003] In summary, traditional lithium extraction technology from lepidolite suffers from problems such as poor element selectivity, difficulty in separating lithium from aluminum, high impurity content, difficulty in removing impurities, low leaching efficiency, high energy consumption, and heavy environmental burden. Summary of the Invention

[0004] To address the problems existing in the prior art, the present invention aims to provide a method for lithium extraction from mica using microwave-assisted multi-stage gradient acid leaching. This method solves the problems of low leaching efficiency, low selective separation of lithium from impurity elements, high impurity content, and difficulty in impurity removal in traditional lepidolite lithium extraction technologies. It also solves the problems of high energy consumption and severe environmental pollution associated with traditional lepidolite lithium extraction technologies.

[0005] The technical solution of the present invention is as follows: This invention provides a method for microwave-assisted multi-stage gradient acid leaching of lithium from lepidolite, comprising the following steps: S1. Add a structure disruptor to lepidolite concentrate, grind, and pre-leach to obtain activated lepidolite concentrate; S2. Add a first-stage acid and a configuration modifier to the activated lepidolite concentrate, perform first-stage leaching, filter, and obtain leachate one and leaching residue one. S3. Add a second-stage acid to leaching residue one, introduce microwave, perform secondary leaching, filter, and obtain leaching solution two and leaching residue two. S4. Add the third-stage acid to the leaching residue II and introduce microwaves for tertiary leaching. Filter to obtain leaching solution III and leaching residue III. S5. Combine leachate one, leachate two and leachate three to obtain lithium-containing leachate.

[0006] Furthermore, the above-mentioned microwave-assisted multi-stage gradient acid leaching method for lithium extraction from lepidolite also includes: S6. Add a precipitant to the lithium-containing leachate and control the pH, concentrate, add a lithium precipitation agent, filter, and obtain filtrate and lithium carbonate product.

[0007] Furthermore, the first-order acid is selected from weak acids.

[0008] Furthermore, the second-order acid is selected from moderately strong acids.

[0009] Furthermore, the third-order acid is selected from strong acids.

[0010] This invention begins with the mechanochemical activation in the pretreatment stage (S1), pulverizing lepidolite to a D90 < 45 μm and introducing ammonium fluoride as a structure disruptor. This pre-leaching process breaks the Si-O-Al bonds, facilitating lithium ion release and improving subsequent lithium leaching efficiency, thus solving the problem of low leaching efficiency in traditional lepidolite lithium extraction technology. A multi-stage gradient acid leaching system (S2-S3) is added, achieving selective stepwise dissolution of lithium through a three-stage gradient acid environment (organic weak acid – medium-strong inorganic acid – strong inorganic acid). Furthermore, a microwave-assisted enhancement system is innovatively introduced in the critical leaching stage, utilizing a directional microwave field to generate local hotspots and selective heating effects, significantly improving the lithium ion diffusion rate and enhancing mass and heat transfer efficiency. Through this multi-stage gradient acid leaching system, highly selective lithium extraction is achieved while controlling the leaching rate of aluminum impurities. In step S5, the leachates from the three acid leaching processes are combined to obtain the final lithium-containing leachate. Then, a precipitating agent is added to remove impurities such as aluminum, iron, fluorine, and silicon, resulting in a purified lithium-containing leachate. This purified leachate is then evaporated and concentrated, followed by the addition of a lithium precipitation agent for a room-temperature, ambient-pressure lithium precipitation reaction. Filtration yields a lithium precipitate product and the remaining filtrate. This invention achieves efficient and selective extraction of lithium while controlling the leaching rate of aluminum impurities. It solves the problem of low selective separation between lithium and impurity elements in traditional lepidolite lithium extraction technologies, as well as the problems of high impurity content and difficulty in impurity removal in traditional lepidolite lithium extraction technologies.

[0011] Furthermore, the degree of grinding is such that the lepidolite concentrate is pulverized to D90 < 45 μm.

[0012] Furthermore, the pre-impregnation is carried out in a PTFE-lined reactor.

[0013] Furthermore, in S6, the precipitant is sodium hydroxide or calcium hydroxide, and the pH is >12; the lithium precipitant is sodium carbonate.

[0014] Preferably, in step S6, the precipitant is sodium hydroxide and the pH is >12; the lithium precipitant is sodium carbonate.

[0015] Preferably, in step S6, the precipitant is calcium hydroxide and the pH is >12; the lithium precipitation agent is sodium carbonate.

[0016] Furthermore, in S6, the concentration factor is 4 times, and the concentration method is evaporation.

[0017] Furthermore, the mass ratio of the lithium mica concentrate, structure disruptor, primary acid, configuration modifier, secondary acid, tertiary acid, and lithium precipitation agent is 1000:50~80:200~400:10~20:300:200~300:127~135.

[0018] Preferably, the mass ratio of the lithium mica concentrate, structure disruptor, primary acid, configuration modifier, secondary acid, tertiary acid and lithium precipitation agent is 1000:50:200:10:300:200:127.

[0019] Preferably, the mass ratio of the lithium mica concentrate, structure disruptor, primary acid, configuration modifier, secondary acid, tertiary acid, and lithium precipitation agent is 1000:60:300:15:300:200:132.

[0020] Preferably, the mass ratio of the lithium mica concentrate, structure disruptor, primary acid, configuration modifier, secondary acid, tertiary acid, and lithium precipitation agent is 1000:80:400:20:300:300:135.

[0021] By precisely controlling the dosage of lepidolite concentrate, structure disruptor, primary acid, configuration modifier, secondary acid, tertiary acid, and lithium precipitation agent, efficient lithium extraction can be achieved synergistically, while controlling reaction intensity and cost. Furthermore, the leaching and impurity removal effects can be optimized, reducing resource waste caused by lithium-containing waste residue. Simultaneously, the consumption of impurity removal reagents and the corresponding waste residue generation are reduced, and excessive reagent discharge can be avoided, preventing pollution of surrounding soil and groundwater, thus reducing the environmental burden. This solves the problems of high energy consumption and severe environmental pollution in traditional lepidolite lithium extraction technologies.

[0022] Furthermore, in S1, the structure disruptor is ammonium fluoride.

[0023] Furthermore, in S2, the first-order acid is malic acid and tartaric acid, and the mass ratio of malic acid to tartaric acid is 0~1:0~1; the configuration modifier is polyethylene oxide.

[0024] Furthermore, in S3, the second-order acid is phosphoric acid.

[0025] Furthermore, in S4, the third acid is sulfuric acid.

[0026] In S2 (first-stage acid leaching), by selecting a weak organic acid (malic acid / tartaric acid) and adding a configuration modifier, most of the highly reactive lithium can be selectively leached out while avoiding a large amount of aluminum entering the solution. In S3 (second-stage acid leaching), a medium-strong acid (phosphoric acid) is used for leaching, and a directional microwave field is introduced to further dissolve the remaining lithium. In S4 (third-stage acid leaching), a strong acid (sulfuric acid) is used for leaching, and a directional microwave field is also introduced to dissolve the remaining small portion of lithium.

[0027] Preferably, in S1, the structure disruptor is ammonium fluoride; in S2, the first-order acid is malic acid; the configuration modifier is polyethylene oxide; in S3, the second-order acid is phosphoric acid; and in S4, the third-order acid is sulfuric acid.

[0028] Preferably, in S1, the structure disruptor is ammonium fluoride; in S2, the first-level acid is tartaric acid; the configuration modifier is polyethylene oxide; in S3, the second-level acid is phosphoric acid; and in S4, the third-level acid is sulfuric acid.

[0029] Preferably, in S1, the structure disruptor is ammonium fluoride; in S2, the first-order acid is malic acid and tartaric acid, the mass ratio of malic acid and tartaric acid is 1:1, and the configuration modifier is polyethylene oxide; in S3, the second-order acid is phosphoric acid; and in S4, the third-order acid is sulfuric acid.

[0030] Ammonium fluoride (NH4F) is introduced as a structure disruptor during the pre-soaking process. - It will prioritize attacking and fracturing lepidolite (mainly K(Li,Al)3(AlSi3O)). 10The relatively weak Si-O-Al chemical bonds in (F,OH)2 are broken, disrupting its layered silicate structure and exposing lithium ions encased within the crystal lattice, thus creating favorable conditions for subsequent low-acidity leaching. In the first stage of acid leaching, weak organic acids such as malic acid / tartaric acid are used. These acids are relatively weak but possess good complexing abilities. At lower temperatures, they selectively react with lithium ions, which are most easily released after the structure is broken, while having a weaker effect on relatively stable oxides such as aluminum and iron, thereby achieving "high lithium, low impurities" leaching in the first stage. The addition of polyethylene oxide (PEO) in this stage inhibits the aluminum-malic acid / tartaric acid complexation reaction. Due to the high charge density of lithium ions, a stable hydrated layer is more easily formed on their surface, and the adsorption of PEO is affected by this hydrated layer, resulting in weaker adsorption capacity. Therefore, the PEO molecular chains selectively adsorb onto the surface of the aluminum-containing solid phase, forming a dense, hydrophilic molecular "isolation network." Malic acid / tartaric acid molecules have a relatively large volume, and the diffusion resistance is significantly increased when they try to penetrate the network structure composed of polyethylene oxide (PEO) molecular chains and contact the aluminum active sites on the particle surface to undergo a complexation reaction. This physical obstacle kinetically slows down the aluminum dissolution rate. In the second-stage acid leaching, phosphoric acid is used, which is stronger than organic acids and can further act on the lithium that was not completely leached in the first stage. More importantly, unlike the large malic acid / tartaric acid molecules, the relatively small phosphate ions (PO4 ions)... 3- It is easier for aluminum ions to penetrate the polyethylene oxide (PEO) adsorption layer. When a small amount of aluminum ions dissolve from the solid surface and enter the PEO adsorption layer region, this network rich in water and polar groups can serve as an ideal micro-reaction domain. Within this region, aluminum ions meet phosphate ions and rapidly form the core of aluminum phosphate precipitate, achieving an "in-situ impurity removal" effect. The network structure of the PEO molecular chain can stabilize the newly formed precipitate particles, preventing them from redissolving or agglomerating and growing, thus promoting the "in-situ" formation of aluminum phosphate on the surface of the solid particles in the form of a capping layer, further strengthening the "lock-in" effect on the internal aluminum. In the third-stage acid leaching, the traditional strong acid—sulfuric acid—is used at higher temperatures and lower pH values ​​to "attack" and leach the lithium remaining in the most stable structure. At this point, most of the lithium has been extracted, requiring only a lower concentration of sulfuric acid, thereby significantly reducing the total acid consumption. Adding sodium hydroxide or calcium hydroxide to the lithium-containing leachate can adjust the pH value to above 12, while simultaneously removing aluminum / fluorine impurities with the precipitant, resulting in a purified lithium-containing leachate.

[0031] Furthermore, in S1, the grinding also includes adding water to make the material moisture content 7~9%, the grinding time is 60~120min, the grinding is carried out using a planetary ball mill, and the rotation speed of the planetary ball mill is controlled at 280~320rpm; the stirring speed during the pre-soaking process is 60~100rpm, the pre-soaking time is 4~6h, and the pre-soaking temperature is 25~30℃.

[0032] Furthermore, in S2, during the primary leaching process, the stirring speed is 150~200 rpm, the primary leaching temperature is 40~50℃, and the primary leaching time is 90~120 min.

[0033] Furthermore, in S3, the frequency of the microwave is 2.45 GHz, and the power density of the microwave is 0.8~1.2 KW / L; during the secondary leaching process, the stirring speed is 150~200 rpm, the temperature of the secondary leaching is 60~70℃, and the leaching time is 90~120 min.

[0034] Furthermore, in S4, the frequency of the microwave is 2.45 GHz, and the power density of the microwave is 0.8~1.2 KW / L; during the three-stage leaching process, the stirring speed is 150~200 rpm, the temperature of the three-stage leaching is 80~90℃, and the leaching time is 60~90 min.

[0035] Preferably, in S1, the grinding further includes adding water to make the material moisture content 7%, the grinding time is 60 minutes, the grinding is performed using a planetary ball mill, and the rotation speed of the planetary ball mill is controlled at 280 rpm; the stirring speed is 60 rpm, the pre-soaking time is 4 hours, and the pre-soaking temperature is 25°C; in S2, the stirring speed is 150 rpm, the leaching temperature is 40°C, and the leaching time is 90 minutes; in S3, the microwave frequency is 2.45 GHz, the microwave power density is 0.8 kW / L, the stirring speed is 150 rpm, the leaching temperature is 60°C, and the leaching time is 90 minutes; in S4, the microwave frequency is 2.45 GHz, the microwave power density is 0.8 kW / L, the stirring speed is 150 rpm, the leaching temperature is 80°C, and the leaching time is 60 minutes.

[0036] Preferably, in S1, the grinding further includes adding water to make the material moisture content 8%, the grinding time is 80 min, the grinding is performed using a planetary ball mill, and the rotation speed of the planetary ball mill is controlled at 300 rpm; the stirring speed is 80 rpm, the pre-soaking time is 5 h, and the pre-soaking temperature is 28°C; in S2, the stirring speed is 170 rpm, the leaching temperature is 45°C, and the leaching time is 100 min; in S3, the microwave frequency is 2.45 GHz, the microwave power density is 0.8 KW / L; the stirring speed is 170 rpm, the leaching temperature is 65°C, and the leaching time is 100 min; in S4, the microwave frequency is 2.45 GHz, the microwave power density is 0.9 KW / L; the stirring speed is 170 rpm, the leaching temperature is 85°C, and the leaching time is 80 min.

[0037] Preferably, in S1, the grinding further includes adding water to make the material moisture content 9%, the grinding time is 120 min, the grinding is performed using a planetary ball mill, and the rotation speed of the planetary ball mill is controlled at 320 rpm; the stirring speed is 100 rpm, the pre-soaking time is 6 h, and the pre-soaking temperature is 30°C; in S2, the stirring speed is 200 rpm, the leaching temperature is 50°C, and the leaching time is 120 min; in S3, the microwave frequency is 2.45 GHz, the microwave power density is 1.2 KW / L; the stirring speed is 200 rpm, the leaching temperature is 70°C, and the leaching time is 120 min; in S4, the microwave frequency is 2.45 GHz, the microwave power density is 1.2 KW / L; the stirring speed is 200 rpm, the leaching temperature is 90°C, and the leaching time is 90 min.

[0038] Furthermore, the chemical composition of the lepidolite concentrate, by mass percentage, includes: 2.5% Li₂O, 27.87% Al₂O₃, 53.22% SiO₂, 0.70% Fe₂O₃, 0.09% CaO, 0.10% MgO, 9.99% K₂O, 1.907% Na₂O, 0.04% TiO₂, <0.01% ZrO₂, 0.29% P₂O₅, <0.05% SO₃, 1.39% F, 0.04% ZnO, <0.01% SrO, 0.38% MnO, <0.01% CuO, 1.34% Rb₂O, 0.06% Cs₂O, and other impurities.

[0039] Furthermore, the lithium leaching solution contains a lithium leaching rate of greater than 95% and an aluminum leaching rate of less than 10%.

[0040] The present invention also provides lithium carbonate prepared by the above-mentioned microwave-assisted multi-level gradient acid leaching method for lithium extraction from lepidolite.

[0041] The beneficial effects of this invention are: This invention provides a method for lithium extraction from lepidolite using microwave-assisted multi-level gradient acid leaching. By integrating three core modules—mechanical and chemical activation in the pretreatment stage, multi-level gradient acid leaching regulation, and microwave-assisted enhancement—it achieves efficient leaching and selective separation of lithium from lepidolite through synergistic effects from three dimensions: structural destruction, reaction regulation, and energy enhancement.

[0042] This invention begins with the mechanochemical activation in the pretreatment stage (S1), pulverizing lepidolite to a D90 < 45 μm and introducing ammonium fluoride as a structure disruptor. This pre-leaching process breaks the Si-O-Al bonds, facilitating lithium ion release and improving subsequent leaching efficiency, thus solving the problem of low leaching efficiency in traditional lepidolite lithium extraction technology. A multi-stage gradient acid leaching system (S2-S3) is added, achieving selective stepwise dissolution of lithium through a three-stage gradient acid environment (organic weak acid – medium-strong inorganic acid – strong inorganic acid). Furthermore, a microwave-assisted enhancement system is innovatively introduced in the critical leaching stage, utilizing a directional microwave field to generate local hotspots and selective heating effects, significantly improving the lithium ion diffusion rate and enhancing mass and heat transfer efficiency. Through this multi-stage gradient acid leaching system, highly selective lithium extraction is achieved while controlling the leaching rate of aluminum impurities. In step S5, the leachates from the three acid leaching processes are combined to obtain the final lithium-containing leachate. Then, a precipitating agent is added to remove impurities such as aluminum, iron, fluorine, and silicon, resulting in a purified lithium-containing leachate. This purified leachate is then evaporated and concentrated, followed by the addition of a lithium precipitation agent for a room-temperature, ambient-pressure lithium precipitation reaction. Filtration yields a lithium precipitate product and the remaining filtrate. This invention achieves efficient and selective extraction of lithium while controlling the leaching rate of aluminum impurities. It solves the problem of low selective separation between lithium and impurity elements in traditional lepidolite lithium extraction technologies, as well as the problems of high impurity content and difficulty in impurity removal in traditional lepidolite lithium extraction technologies.

[0043] The method for lithium extraction from lepidolite using microwave-assisted multi-stage gradient acid leaching of the present invention achieves a total lithium leaching rate of over 95%, while controlling the leaching rate of major impurities such as aluminum and iron to below 10%, and reducing acid consumption by more than 50%. Compared with the traditional high-temperature sulfuric acid roasting process, it has significant advantages in reducing acid consumption, reducing energy consumption, simplifying subsequent purification processes, and improving economic and environmental benefits. Detailed Implementation

[0044] The present invention will be further described in detail below through embodiments, but in no way is the invention limited.

[0045] The chemical composition of the lepidolite concentrate used in the following embodiments and comparative examples of the present invention, by mass percentage, includes: 2.5 wt% Li₂O, 27.87 wt% Al₂O₃, 53.22 wt% SiO₂, 0.70 wt% Fe₂O₃, 0.09 wt% CaO, 0.10 wt% MgO, 9.99 wt% K₂O, 1.907 wt% Na₂O, 0.04 wt% TiO₂, <0.01 wt% ZrO₂, 0.29 wt% P₂O₅, <0.05 wt% SO₃, 1.39 wt% F, 0.04 wt% ZnO, <0.01 wt% SrO, 0.38 wt% MnO, <0.01 wt% CuO, 1.34 wt% Rb₂O, 0.06 wt% Cs₂O, and other impurities.

[0046] The malic acid, tartaric acid, phosphoric acid, and sulfuric acid used in the embodiments and comparative examples of this invention are all analytical grade reagents.

[0047] The technical mechanism of the present invention is as follows: The gradient acid species synergistic microwave-assisted multi-stage selective leaching system comprises four core components: 1) Pretreatment stage: Mechanochemical activation technology and ammonium fluoride pre-leaching are used to break Si-O-Al bonds; 2) Multi-stage gradient acid leaching stage: A three-stage acid leaching system is designed, using malic acid / tartaric acid, phosphoric acid, and sulfuric acid sequentially for selective leaching; 3) Microwave-assisted enhancement system: A directional microwave field is introduced during the second and third leaching processes to improve the lithium ion diffusion rate; 4) Configuration modifier: 0.5~2.0% of the configuration modifier polyethylene oxide (PEO) is added.

[0048] The method of lithium extraction by microwave-assisted multi-level gradient acid leaching of lepidolite starts with mechanochemical activation and achieves selective stepwise dissolution of lithium through a three-level gradient acid environment (organic weak acid - medium strong inorganic acid - strong inorganic acid). The method also innovatively introduces microwave-assisted technology in the key leaching stage, which significantly enhances the mass and heat transfer efficiency.

[0049] The method for lithium extraction from lepidolite using microwave-assisted multi-stage gradient acid leaching includes the following stages: (1) Pretreatment stage: Mechanochemical activation technology and ammonium fluoride pre-immersion are used to break the Si-O-Al bond.

[0050] High-intensity mechanical grinding not only pulverizes lepidolite particles to the micron level (D90 < 45 μm) to increase specific surface area, but more importantly, it induces lattice distortion and generates microscopic defects through mechanical force. Simultaneously, ammonium fluoride (NH4F) is introduced as a structure disruptor; during the pre-soaking process, F… - It will prioritize attacking and fracturing lepidolite (mainly K(Li,Al)3(AlSi3O)). 10The relatively weak Si-O-Al chemical bonds in (F, OH)2 are broken, disrupting its layered silicate structure and exposing lithium ions encased within the lattice, thus creating favorable conditions for subsequent low-acidity leaching.

[0051] (2) Multi-stage gradient acid leaching stage: A three-stage acid leaching system was designed, using malic acid / tartaric acid, phosphoric acid and sulfuric acid sequentially for selective leaching. Selective stepwise dissolution of lithium was achieved through a three-stage gradient acid environment (weak organic acid - medium-strong inorganic acid - strong inorganic acid).

[0052] Gradient acid leaching principle: This strategy abandons the traditional single acid leaching mode and adopts a "step-by-step" leaching strategy: First stage (mild leaching): This stage uses weak organic acids such as malic acid and tartaric acid, which have good complexing ability despite their low acidity. At lower temperatures, they selectively react with lithium ions, which are most easily released after structural damage, while having a weaker effect on relatively stable oxides such as aluminum and iron, thus achieving "high lithium, low impurities" leaching in the first stage. The addition of polyethylene oxide (PEO) in this stage inhibits the aluminum-malic acid / tartaric acid complexation reaction. Due to the high charge density of lithium ions, a stable hydration layer is more easily formed on their surface, and the adsorption of PEO is affected by this hydration layer, resulting in weaker adsorption capacity. Therefore, PEO molecular chains selectively adsorb onto the surface of the aluminum-containing solid phase, forming a dense, hydrophilic molecular "isolation network." Malic acid / tartaric acid molecules have a relatively large volume, and the diffusion resistance to penetrate this network structure composed of PEO molecular chains and contact the aluminum active sites on the particle surface to undergo a complexation reaction is significantly increased. This physical barrier kinetically slows down the rate of aluminum dissolution.

[0053] Second stage (deeper leaching): Phosphoric acid is a stronger acid than organic acids, allowing it to further act on the lithium that was not completely leached in the first stage. More importantly, unlike the larger malic acid / tartaric acid molecules, the relatively smaller phosphate ions (PO4 ions)... 3- It is easier for aluminum ions to penetrate the polyethylene oxide (PEO) adsorption layer. When a small amount of aluminum ions dissolve from the solid surface and enter the PEO adsorption layer region, this network rich in water and polar groups can serve as an ideal micro-reaction domain. Within this region, aluminum ions meet phosphate ions and rapidly form the core of aluminum phosphate precipitate, achieving an "in-situ impurity removal" effect. The network structure of the PEO molecular chains can stabilize the newly formed precipitate particles, preventing them from redissolving or agglomerating and growing, thus promoting the "in-situ" formation of aluminum phosphate on the surface of the solid particles in the form of a capping layer, further strengthening the "lock-in" effect on the internal aluminum.

[0054] The third stage (final leaching): Using traditional strong acid—sulfuric acid—at higher temperatures and lower pH conditions, the remaining lithium in its most stable structure is leached. At this stage, most of the lithium has been extracted, requiring only a lower concentration of sulfuric acid, thus significantly reducing total acid consumption. Polyethylene oxide continues to play a role in inhibiting the precipitation of impurities at this stage.

[0055] (3) Microwave-assisted enhancement principle: Microwave heating is not simply macroscopic heating; its core advantages lie in "selectivity" and "non-thermal effects." In the second and third stage leaching slurries, lepidolite mineral particles, as polar substances, can efficiently absorb 2.45 GHz microwave energy, while the absorption efficiency of acidic aqueous solutions is relatively low. This leads to the formation of instantaneous local high-temperature "hot spots" (up to 120~150℃) inside and around the mineral particles, which is much higher than the macroscopic apparent temperature of the slurry (60~90℃). This local high temperature greatly accelerates the destruction of the mineral structure and the internal diffusion rate of lithium ions. In addition, the high-frequency oscillation of the microwave electric field can also cause high-speed reciprocating motion of ions, producing a "stirring" effect, destroying the ion diffusion boundary layer, and further enhancing the mass transfer process.

[0056] (4) Configuration modifier: Add 0.5~2.0% of the configuration modifier polyethylene oxide (PEO).

[0057] The role of polyethylene oxide (PEO) can be understood as a selectively permeable membrane: it kinetically hinders the attack of large malic acid / tartaric acid molecules on aluminum, while providing a stable reaction and precipitation site for phosphate ions and the small amount of dissolved aluminum ions, thus achieving efficient inhibition of aluminum dissolution through thermodynamic selectivity.

[0058] Example 1 The planetary ball mill used in this embodiment has a revolution speed of 280 rpm and a rotation speed to revolution speed ratio of 1:1.3.

[0059] A method for microwave-assisted multi-stage gradient acid leaching of lithium from lepidolite includes the following steps: S1. Add 1000g of lepidolite concentrate to a planetary ball mill, add 50g of structure disruptor ammonium fluoride, control the speed of the planetary ball mill to 280 rpm, the moisture content of the material to 7% (the material refers to the lepidolite concentrate and the structure disruptor, water is added to the material to control the moisture content), and the grinding time to 60 min, so that the lepidolite concentrate is crushed to D90 < 45μm; then pre-soak it in a PTFE-lined reactor for 4 hours, with stirring during the pre-soaking process, the solid-liquid ratio (mass ratio of solid matter to water) is 1:1, the pre-soaking temperature is 25℃, and the stirring speed during the pre-soaking process is 60 rpm, to obtain activated lepidolite concentrate.

[0060] S2. For the activated lepidolite concentrate obtained in S1, a three-stage acid leaching process is designed: The first stage of leaching involves adding malic acid (first-stage acid): malic acid and 10g of configuration modifier polyethylene oxide (PEO) are added to activated lepidolite concentrate. The mass ratio of mineral to acid (mass ratio of lepidolite concentrate to malic acid) is 1:0.2, the solid-liquid ratio (mass ratio of solid matter to liquid) is 1:2, the leaching temperature is 40℃, the leaching time is 90min, and the stirring speed is 150rpm. In this first-stage leaching, most of the active lithium is selectively dissolved. After solid-liquid separation, leachate one and leaching residue one are obtained. The second stage involves transferring the leaching residue from the previous stage to a microwave-heatable reactor for leaching with phosphoric acid (secondary acid): Phosphoric acid is added to leaching residue one, with a mineral-to-acid mass ratio (lithium mica concentrate to phosphoric acid mass ratio) of 1:0.3, a solid-to-liquid ratio of 1:2, a leaching temperature of 60℃, a leaching time of 90 min, a stirring speed of 150 rpm, and a microwave-assisted enhanced reaction with a frequency of 2.45 GHZ and a microwave power density of 0.8 KW / L. This secondary leaching further dissolves the remaining lithium, and after solid-liquid separation, leaching solution two and leaching residue two are obtained. In the third stage, the leaching residue from the second stage is transferred to a microwave-heatable reactor for leaching with sulfuric acid (the third-stage acid): sulfuric acid is added to the second leaching residue, with a mineral-to-acid mass ratio (lithium mica concentrate to sulfuric acid mass ratio) of 1:0.2, a solid-to-liquid ratio of 1:2, a leaching temperature of 80℃, a leaching time of 60 min, and a stirring speed of 150 rpm. A directional microwave field with a frequency of 2.45 GHz and a microwave power density of 0.8 KW / L is also introduced. After the three-stage leaching, the remaining small portion of lithium is dissolved. After solid-liquid separation, the third leaching solution and the third leaching residue are obtained.

[0061] S3. Combine leachate 1, leachate 2 and leachate 3 to obtain lithium-containing leachate. Add NaOH precipitant to lithium-containing leachate to adjust the pH value to above 12, so as to remove aluminum / fluorine impurities by precipitant, and obtain lithium-containing leachate after impurity removal. Here, NaOH has the function of adjusting pH and achieving sedimentation and impurity removal.

[0062] S4. Evaporate and concentrate the lithium-containing leachate after impurity removal by 4 times, then add 127 g of sodium carbonate lithium precipitation agent to carry out the lithium precipitation reaction. After the lithium precipitation reaction is completed, filter to obtain lithium carbonate product and remaining filtrate.

[0063] Example 2 The planetary ball mill used in this embodiment has a revolution speed of 300 rpm and a rotation speed to revolution speed ratio of 1:1.3.

[0064] A method for microwave-assisted multi-stage gradient acid leaching of lithium from lepidolite includes the following steps: S1. Add 1000g of lepidolite concentrate to a planetary ball mill, add 60g of structure disruptor ammonium fluoride, control the speed of the planetary ball mill to 300rpm, the moisture content of the material to 8% (the material refers to the lepidolite concentrate and the structure disruptor, water is added to the material to control the moisture content), and the grinding time to 80min, so that the lepidolite concentrate is crushed to D90<45μm; then pre-soak it in a PTFE-lined reactor for 5 hours, with stirring during the pre-soaking process, a solid-liquid ratio of 1:1, a pre-soaking temperature of 28℃, and a stirring speed of 80rpm during the pre-soaking process, to obtain activated lepidolite concentrate.

[0065] S2. For the activated lepidolite concentrate obtained in S1, a three-stage acid leaching process is designed: The first stage of leaching involves adding tartaric acid (first-stage acid): Tartaric acid and 15g of polyethylene oxide (PEO) configuration modifier are added to activated lithium mica concentrate. The mass ratio of mineral to acid (mass ratio of lithium mica concentrate to tartaric acid) is 1:0.3, the solid-liquid ratio is 1:2, the leaching temperature is 45℃, the leaching time is 100min, and the stirring speed is 170rpm. In this first-stage leaching, most of the active lithium is selectively dissolved. After solid-liquid separation, leachate one and leach residue one are obtained. The second stage involves transferring the leaching residue from the previous stage to a microwave-heatable reactor for leaching with phosphoric acid (secondary acid): Phosphoric acid is added to leaching residue one, with a mineral-to-acid mass ratio (mass ratio of lepidolite concentrate to phosphoric acid) of 1:0.3, a solid-to-liquid ratio of 1:2, a leaching temperature of 65℃, a leaching time of 100 min, a stirring speed of 170 rpm, and a microwave-assisted enhanced reaction with a frequency of 2.45 GHZ and a microwave power density of 0.8 KW / L. This secondary leaching further dissolves the remaining lithium, and after solid-liquid separation, leaching solution two and leaching residue two are obtained. In the third stage, the leaching residue from the second stage is transferred to a microwave-heatable reactor for leaching with sulfuric acid (the third-stage acid): sulfuric acid is added to the second leaching residue, with a mineral-to-acid mass ratio (lithium mica concentrate to sulfuric acid mass ratio) of 1:0.2, a solid-to-liquid ratio of 1:2, a leaching temperature of 85℃, a leaching time of 80 min, and a stirring speed of 170 rpm. A directional microwave field with a frequency of 2.45 GHz and a microwave power density of 0.9 KW / L is also introduced. After the three-stage leaching, the remaining small portion of lithium is dissolved. After solid-liquid separation, the third leaching solution and the third leaching residue are obtained.

[0066] S3. Combine leachate 1, leachate 2 and leachate 3 to obtain lithium-containing leachate. Add precipitant Ca(OH)2 to the lithium-containing leachate to adjust the pH value to above 12, so as to remove aluminum / fluorine impurities by precipitant, and obtain lithium-containing leachate after impurity removal. Here, Ca(OH)2 has the function of adjusting pH and also the function of sedimentation and impurity removal.

[0067] S4. Evaporate and concentrate the lithium-containing leachate after impurity removal by 4 times, then add 132 g of sodium carbonate lithium precipitation agent to carry out the lithium precipitation reaction. After the lithium precipitation reaction is completed, filter to obtain lithium carbonate product and remaining filtrate.

[0068] Example 3 The planetary ball mill used in this embodiment has a revolution speed of 320 rpm and a rotation speed to revolution speed ratio of 1:1.3.

[0069] A method for microwave-assisted multi-stage gradient acid leaching of lithium from lepidolite includes the following steps: S1. Add 1000g of lepidolite concentrate to a planetary ball mill, add 80g of structure disruptor ammonium fluoride, control the speed of the planetary ball mill to 320rpm, the moisture content of the material to 9% (the material refers to the lepidolite concentrate and the structure disruptor, water is added to the material to control the moisture content), and the grinding time to 120min, so that the lepidolite concentrate is crushed to D90<45μm; then pre-soak it in a PTFE-lined reactor for 6 hours, with stirring during the pre-soaking process, a solid-liquid ratio of 1:1, a pre-soaking temperature of 30℃, and a stirring speed of 100rpm during the pre-soaking process, to obtain activated lepidolite concentrate.

[0070] S2. For the activated lepidolite concentrate obtained in S1, a three-stage acid leaching process is designed: The first stage of leaching involves adding a mixture of malic acid and tartaric acid in a 1:1 mass ratio (the mixed malic acid and tartaric acid serve as the primary acid): Malic acid and tartaric acid in a 1:1 mass ratio are added to activated lepidolite concentrate, along with 20g of polyethylene oxide (PEO) as a configuration modifier. The mineral-to-acid mass ratio (lepidolite concentrate to primary acid) is 1:0.4, the solid-to-liquid ratio is 1:2, the leaching temperature is 50℃, the leaching time is 120min, and the stirring speed is 200rpm. This first-stage leaching selectively dissolves most of the active lithium. After solid-liquid separation, leachate one and leaching residue one are obtained. The second stage involves transferring the leaching residue from the previous stage to a microwave-heatable reactor for leaching with phosphoric acid (secondary acid): Phosphoric acid is added to leaching residue one, with a mineral-to-acid mass ratio (lithium mica concentrate to phosphoric acid mass ratio) of 1:0.3, a solid-to-liquid ratio of 1:2, a leaching temperature of 70℃, a leaching time of 120 min, a stirring speed of 200 rpm, and a microwave-assisted enhanced reaction with a frequency of 2.45 GHZ and a microwave power density of 1.2 KW / L. This secondary leaching further dissolves the remaining lithium, and after solid-liquid separation, leaching solution two and leaching residue two are obtained. In the third stage, the leaching residue from the second stage is transferred to a microwave-heatable reactor for leaching with sulfuric acid (the third-stage acid): sulfuric acid is added to the second leaching residue, with a mineral-to-acid mass ratio (lithium mica concentrate to sulfuric acid) of 1:0.3, a solid-to-liquid ratio of 1:2, a leaching temperature of 90℃, a leaching time of 90 min, and a stirring speed of 200 rpm. A directional microwave field with a frequency of 2.45 GHz and a microwave power density of 1.2 KW / L is also introduced. After the three-stage leaching, the remaining small portion of lithium is dissolved. After solid-liquid separation, the third leaching solution and the third leaching residue are obtained.

[0071] S3. Combine leachate 1, leachate 2 and leachate 3 to obtain lithium-containing leachate. Add precipitant Ca(OH)2 to the lithium-containing leachate to adjust the pH value to above 12, so as to remove aluminum / fluorine impurities by precipitant, and obtain lithium-containing leachate after impurity removal. Here, NaOH has the function of adjusting pH and achieving sedimentation and impurity removal.

[0072] S4. Evaporate and concentrate the lithium-containing leachate after impurity removal by 4 times, then add 135 g of sodium carbonate lithium precipitation agent to carry out the lithium precipitation reaction. After the lithium precipitation reaction is completed, filter to obtain lithium carbonate product and remaining filtrate.

[0073] Comparative Example 1 Traditional lithium extraction technology using gradient acid seed multi-stage selective leaching of lepidolite includes the following steps: S1. Add 1000g of lithium mica concentrate to a planetary ball mill, add 80g of ammonium fluoride as a structure disruptor, control the speed of the planetary ball mill to 320rpm, the moisture content of the material to 9%, and the grinding time to 120min.

[0074] S2. The lepidolite concentrate obtained in S1 is subjected to a three-stage acid leaching process. The first stage involves leaching with a 1:1 mass ratio of malic acid and tartaric acid, along with 20g of polyethylene oxide (PEO) as a configuration modifier. The mineral-to-acid mass ratio is 1:0.4, the solid-to-liquid ratio is 1:2, the leaching temperature is 50℃, the leaching time is 120min, and the stirring speed is 200rpm. This selectively dissolves most of the active lithium, and after solid-liquid separation, leachate one and leachate residue one are obtained. The second stage involves transferring the leachate residue from the previous stage to a microwave-safe reactor and leaching with phosphoric acid. The mass ratio of minerals to acid is 1:0.3, the solid-liquid ratio is 1:2, the leaching temperature is 70℃, the leaching time is 120 min, and the stirring speed is 200 rpm. The remaining lithium is further dissolved, and after solid-liquid separation, leaching solution two and leaching residue two are obtained. In the third stage, the leaching residue of the second stage is transferred to a microwave-heatable reactor and leached with sulfuric acid. The mass ratio of minerals to acid is 1:0.3, the solid-liquid ratio is 1:2, the leaching temperature is 90℃, the leaching time is 90 min, and the stirring speed is 200 rpm. The remaining small portion of lithium is dissolved, and after solid-liquid separation, leaching solution three and leaching residue three are obtained.

[0075] S3. Combine leachate 1, leachate 2 and leachate 3 to obtain lithium-containing leachate. Add Ca(OH)2 to the lithium-containing leachate to adjust the pH value to above 12, so as to remove aluminum / fluorine impurities with the precipitant and obtain the lithium-containing leachate after impurity removal. S4. Evaporate and concentrate the lithium-containing leachate after impurity removal by 4 times, then add 137g of sodium carbonate lithium precipitation agent to carry out lithium precipitation reaction, and filter to obtain lithium carbonate product and remaining filtrate.

[0076] Comparative Example 2 Traditional lithium extraction technology using lepidolite-assisted microwave-assisted selective leaching includes the following steps: S1. Add 1000g of lepidolite concentrate to a planetary ball mill, add 80g of ammonium fluoride as a structure disruptor, control the rotation speed of the planetary ball mill to 320rpm, the moisture content of the material to 9%, the grinding time to 120min, and then pre-impregnate in a PTFE-lined reactor for 6 hours with a liquid-to-solid ratio of 1:1, a pre-impregnation temperature of 30℃, and a stirring speed of 100rpm to obtain activated lepidolite concentrate.

[0077] S2. The lithium mica concentrate obtained in S1 is added to a microwave-heatable reactor and leached with sulfuric acid at a mass ratio of 1:1, a solid-liquid ratio of 1:2, a leaching temperature of 90℃, a leaching time of 90 min, a stirring speed of 200 rpm, and a 2.45 GHz directional microwave field with a microwave power density of 1.2 KW / L. The mixture is then filtered to obtain a lithium-containing leachate and leaching residue.

[0078] S3. Add Ca(OH)2 to the lithium-containing leachate to adjust the pH value to above 12, so as to remove aluminum / fluorine impurities with the precipitant and obtain the lithium-containing leachate after impurity removal. S4. Evaporate and concentrate the lithium-containing leachate after impurity removal by 4 times, then add 137 g of sodium carbonate lithium precipitation agent to carry out the lithium precipitation reaction, and filter to obtain lithium carbonate product and remaining filtrate.

[0079] Comparative Example 3 Traditional lithium extraction technology using lepidolite acid roasting includes the following steps: S1. Mix 1000 g of lepidolite concentrate powder with 98% concentrated sulfuric acid, then place the mixture in a muffle furnace and calcine it at 900℃ for 120 min to obtain the calcined product; wherein the mass ratio of lepidolite concentrate powder to 98% concentrated sulfuric acid is 1:2. S2. Add the lithium mica concentrate obtained in S1 to a water bath and leach it with tap water. The leaching solid-liquid ratio is 1:6, the leaching temperature is 90℃, the leaching time is 90min, the stirring speed is 200rpm, and the mixture is filtered to obtain lithium-containing leachate and leaching residue.

[0080] S3. Add Ca(OH)2 to the lithium-containing leachate to adjust the pH value to above 12, so as to remove aluminum / fluorine impurities with the precipitant and obtain the lithium-containing leachate after impurity removal. S4. Evaporate and concentrate the lithium-containing leachate after impurity removal by 4 times, then add 137 g of sodium carbonate lithium precipitation agent to carry out the lithium precipitation reaction, and filter to obtain lithium carbonate product and remaining filtrate.

[0081] Detection and Analysis 1. Determination of Li2O content, Al2O3 content, pH value of lithium-containing leachate, leaching residue yield, and Li2O leaching rate and Al2O3 leaching rate in leaching residue of Examples 1-3 and Comparative Examples 1-3.

[0082] The formula for calculating the Li2O leaching rate in lepidolite concentrate is shown in equation (I): Lithium oxide leaching rate = [volume of lithium-containing leachate (L) × lithium oxide concentration in lithium-containing leachate (g / L)] / [lithium oxide content in lepidolite concentrate (%) × mass of lepidolite concentrate (g)] × 100% (I) The formula for calculating the Al2O3 leaching rate in lepidolite concentrate is shown in equation (II): Al2O3 leaching rate = [volume of lithium-containing leachate (L) × Al2O3 concentration in lithium-containing leachate (g / L)] / [Al2O3 content in lepidolite concentrate (%) × mass of lepidolite concentrate (g)] × 100% (II) The formula for calculating the yield of leaching residue is shown in equation (III): Leaching residue yield (%) = [100% × dry weight of leaching residue (g)] / dry weight of lepidolite concentrate (g) (III) The results of the determination of the content, yield, leaching rate and pH value of each substance are shown in Table 1.

[0083] Table 1. Results of determination of the content, yield, leaching rate and pH value of each substance. As can be seen from the analysis in Table 1, by pre-leaching and activating the lithium mica concentrate through planetary ball milling, and then using microwave-assisted multi-stage gradient acid leaching to extract lithium, the leaching rate of Li2O in the lithium mica concentrate can be above 95%, and the leaching rate of Al2O3 (aluminum dissolution rate) in the lithium mica concentrate can be <10%.

[0084] By comparing Example 3 and Comparative Example 1, it can be seen that the microwave-assisted multi-stage gradient acid leaching method for lithium extraction from lepidolite increases the leaching rate of Li2O in the leachate (Li2O leaching rate in lepidolite concentrate) by 10.05% and decreases the leaching rate of Al2O3 in lepidolite concentrate by 10.15% compared with the multi-stage leaching process without pre-leaching and microwave assistance.

[0085] Comparing Example 3 and Comparative Example 2, it can be seen that Comparative Example 2, using only the traditional sulfuric acid-assisted microwave-assisted single-stage leaching process, resulted in an Al2O3 leaching rate of up to 29.27% ​​in the lepidolite concentrate, which is highly detrimental to subsequent impurity removal and ensuring product purity. In contrast, Example 3, employing a gradient acid-species assisted microwave-assisted multi-stage selective leaching process, increased the Li2O leaching rate (Li2O leaching rate in the lepidolite concentrate) by 15.81% compared to the traditional single-stage leaching, while reducing the Al2O3 leaching rate in the lepidolite concentrate by 22.06%.

[0086] As can be seen from Comparative Example 3, the traditional sulfuric acid high-temperature roasting process at 900℃ resulted in a lithium leaching rate (Li2O leaching rate in lepidolite concentrate) of only 77.72%, while the aluminum leaching rate (Al2O3 leaching rate in lepidolite concentrate) reached as high as 46.2%, which led to higher costs for subsequent lithium-aluminum separation and impurity removal. Comparing Example 3 and Comparative Example 3, Example 3, which used planetary ball milling to pre-leach and activate the lepidolite concentrate, followed by gradient acid seed synergistic microwave-assisted multi-stage selective leaching of lithium, compared to the traditional sulfuric acid high-temperature roasting process in Comparative Example 3, increased the Li2O leaching rate in the lepidolite concentrate by 20.34% and reduced the Al2O3 leaching rate by 38.99%.

[0087] In summary, this invention employs planetary ball milling for pre-leaching and activation of lepidolite concentrate, followed by microwave-assisted multi-stage selective leaching of lithium using gradient acid species, significantly improving the leaching rate of Li₂O (Li₂O leaching rate in lepidolite concentrate) while effectively controlling the leaching rate of aluminum (Al₂O₃ leaching rate in lepidolite concentrate). This allows for lithium conversion in lepidolite at relatively low temperatures and under mild pH conditions, saving energy and reducing production costs for subsequent impurity removal.

[0088] 2. Determination of Leachate Composition The lithium-containing leachate obtained in S3 of Example 3 and the lithium-containing leachate obtained in S3 of Comparative Example 3 were subjected to compositional analysis using inductively coupled plasma atomic emission spectrometry (ICP), atomic absorption spectrophotometry (AAS), gas chromatography-mass spectrometry (GC-MS), and automated potentiometric titration, respectively. The results are shown in Tables 2 and 3.

[0089] Table 2 shows the main components of the lithium-containing leachate obtained in Example 3. Note: The organic acid radical is malate ion (C4H4O5). ⁻ tartrate ion C4H4O6 2- .

[0090] Table 3 shows the main components of the lithium-containing leachate obtained in Comparative Example 3. As shown in Table 2, the lithium-containing leachate obtained in S3 of Example 3 had a Li concentration of 1.91 g / L. The main impurities included Al, Fe, Ca, SiO2, and F, while other impurities included Mg and Mn. Compared to the traditional 900℃ high-temperature roasting process shown in Table 2, the lithium content increased by 20.9%, the content of the main impurity Al decreased by 84.42%, and the content of SiO2 decreased by 50.89%. This result indicates that using gradient acid species in conjunction with microwave-assisted selective lithium extraction can effectively reduce the dissolution of impurities, thereby significantly improving the purity of the subsequent product. Furthermore, this process also demonstrates significant advantages in lithium-aluminum separation, further ensuring the purity and quality of the product.

[0091] In summary, the method for lithium extraction from lepidolite using microwave-assisted multi-stage gradient acid leaching provided by this invention has the following advantages: (1) By integrating the three core modules of mechanochemical activation, multi-level gradient acid leaching regulation and microwave-assisted enhancement in the pretreatment stage, the efficient dissolution and selective separation of lithium elements in lepidolite are achieved through the synergistic effect of structural destruction, reaction regulation and energy enhancement.

[0092] (2) Starting with the mechanochemical activation in the pretreatment stage (S1), lepidolite is pulverized to D90 < 45 μm. Ammonium fluoride is introduced as a structure disruptor to break the Si-O-Al bonds through pre-leaching, making lithium ions easier to release and improving subsequent leaching efficiency. This solves the problem of low leaching efficiency in traditional lepidolite lithium extraction technology. A multi-level gradient acid leaching system (S2~S3) is added, achieving selective stepwise dissolution of lithium through a three-level gradient acid environment (organic weak acid - medium-strong inorganic acid - strong inorganic acid). A microwave-assisted enhancement system is innovatively introduced in the key leaching stage, utilizing a directional microwave field to generate local hotspots and selective heating effects, significantly improving the lithium ion diffusion rate and enhancing mass and heat transfer efficiency. Through the multi-level gradient acid leaching system, highly selective extraction of lithium is achieved while controlling the leaching rate of aluminum impurities. In step S5, the leachates from the three acid leaching processes are combined to obtain the final lithium-containing leachate. Then, a precipitating agent is added to remove impurities such as aluminum, iron, fluorine, and silicon, resulting in a purified lithium-containing leachate. This purified leachate is then evaporated and concentrated, followed by the addition of a lithium precipitation agent for a room-temperature, ambient-pressure lithium precipitation reaction. Filtration yields a lithium precipitate product and the remaining filtrate. This invention achieves efficient and selective extraction of lithium while controlling the leaching rate of aluminum impurities. It solves the problem of low selective separation between lithium and impurity elements in traditional lepidolite lithium extraction technologies, as well as the problems of high impurity content and difficulty in impurity removal in traditional lepidolite lithium extraction technologies.

[0093] (3) The lithium extraction method of lithium mica microwave-assisted multi-level gradient acid leaching of the present invention ultimately achieves a total lithium leaching rate of over 95%, while controlling the leaching rate of major impurities such as aluminum and iron to below 10%, and reducing acid consumption by more than 50% (in the implementation of the present invention, the total amount of acid used is 700g to 1000g, see Examples 1, 2 and 1; while the total amount of acid used in the traditional process is 2000g, see Comparative Example 3; this is without considering the acid concentration, and the acid consumption is reduced by about 50%). Compared with the traditional sulfuric acid high-temperature roasting process, it has significant advantages in reducing acid consumption, reducing energy consumption, simplifying the subsequent purification process and improving economic and environmental benefits.

Claims

1. A method for microwave-assisted multi-stage gradient acid leaching of lithium from lepidolite, characterized in that, Includes the following steps: S1. Add a structure disruptor to lepidolite concentrate, grind, and pre-leach to obtain activated lepidolite concentrate; S2. Add a first-stage acid and a configuration modifier to the activated lepidolite concentrate, perform first-stage leaching, filter, and obtain leachate one and leaching residue one. S3. Add a second-stage acid to leaching residue one, introduce microwave, perform secondary leaching, filter, and obtain leaching solution two and leaching residue two. S4. Add the third-stage acid to the leaching residue II and introduce microwaves for tertiary leaching. Filter to obtain leaching solution III and leaching residue III. S5. Combine leachate 1, leachate 2 and leachate 3 to obtain lithium-containing leachate; In S1, the structural disruptor is ammonium fluoride; In S2, the first-order acid is malic acid and / or tartaric acid; the configuration modifier is polyethylene oxide. In S3, the second-order acid is phosphoric acid; In S4, the third-order acid is sulfuric acid.

2. The method for lithium extraction from lepidolite using microwave-assisted multi-stage gradient acid leaching according to claim 1, characterized in that, Also includes: S6. Add a precipitant to the lithium-containing leachate and control the pH, concentrate, add a lithium precipitation agent, filter, and obtain filtrate and lithium carbonate product.

3. The method for lithium extraction from lepidolite using microwave-assisted multi-stage gradient acid leaching according to claim 2, characterized in that, The mass ratio of the lithium mica concentrate, structure disruptor, primary acid, configuration modifier, secondary acid, tertiary acid, and lithium precipitation agent is 1000:50~80:200~400:10~20:300:200~300:127~135.

4. The method for microwave-assisted multi-stage gradient acid leaching of lithium from lepidolite according to claim 2, characterized in that, The mass ratio of the lithium mica concentrate, structure disruptor, primary acid, configuration modifier, secondary acid, tertiary acid, and lithium precipitation agent is 1000:50:200:10:300:200:

127. Alternatively, the mass ratio of the lithium mica concentrate, structure disruptor, primary acid, configuration modifier, secondary acid, tertiary acid, and lithium precipitation agent is 1000:60:300:15:300:200:

132. Alternatively, the mass ratio of the lithium mica concentrate, structure disruptor, primary acid, configuration modifier, secondary acid, tertiary acid, and lithium precipitation agent is 1000:80:400:20:300:300:

135.

5. The method for microwave-assisted multi-stage gradient acid leaching of lithium from lepidolite according to any one of claims 1 to 4, characterized in that, In S2, the mass ratio of malic acid to tartaric acid is 0~1:0~1, and is not 0.

6. The method for lithium extraction from lepidolite using microwave-assisted multi-stage gradient acid leaching according to claim 1, characterized in that, In S1, the grinding also includes adding water to make the material moisture content 7-9%, the grinding time is 60-120 minutes, the grinding is carried out using a planetary ball mill, and the rotation speed of the planetary ball mill is controlled at 280-320 rpm; the stirring speed during the pre-soaking process is 60-100 rpm, the pre-soaking time is 4-6 hours, and the pre-soaking temperature is 25-30℃; And / or, in S2, during the primary leaching process, the stirring speed is 150~200 rpm, the primary leaching temperature is 40~50℃, and the primary leaching time is 90~120 min; And / or, in S3, the frequency of the microwave is 2.45 GHz, and the power density of the microwave is 0.8~1.2 kW / L; during the secondary leaching process, the stirring speed is 150~200 rpm, the temperature of the secondary leaching is 60~70℃, and the time of the secondary leaching is 90~120 min; And / or, in S4, the frequency of the microwave is 2.45 GHz, and the power density of the microwave is 0.8~1.2 kW / L; during the three-stage leaching process, the stirring speed is 150~200 rpm, the temperature of the three-stage leaching is 80~90℃, and the leaching time is 60~90 min.

7. The method for microwave-assisted multi-stage gradient acid leaching of lithium from lepidolite according to any one of claims 1 to 4, characterized in that, The chemical composition of the lepidolite concentrate, by mass percentage, includes: 2.5% Li₂O, 27.87% Al₂O₃, 53.22% SiO₂, 0.70% Fe₂O₃, 0.09% CaO, 0.10% MgO, 9.99% K₂O, 1.907% Na₂O, 0.04% TiO₂, <0.01% ZrO₂, 0.29% P₂O₅, <0.05% SO₃, 1.39% F, 0.04% ZnO, <0.01% SrO, 0.38% MnO, <0.01% CuO, 1.34% Rb₂O, 0.06% Cs₂O, and other impurities.

8. The method for microwave-assisted multi-stage gradient acid leaching of lithium from lepidolite according to claim 1 or 2, characterized in that, The lithium leaching rate in the lepidolite concentrate is greater than 95%, and the aluminum leaching rate is less than 10%.

Citation Information

Patent Citations

  • Method for efficiently extracting lithium from lepidolite lithium extraction waste residue at low temperature

    CN116240400A