A large-sheet battery-grade anhydrous iron phosphate and its preparation method
By controlling the concentration ratio and temperature of iron and phosphorus solutions, and combining dropwise addition and segmented calcination, anhydrous iron phosphate with high tap density and high purity was prepared, solving the problems of impurity residue and complex process in existing iron phosphate materials, and making it suitable for high energy density batteries.
Patent Information
- Application Number
- CN202610443871.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-07
- Publication Date
- 2026-05-26
AI Technical Summary
Existing technologies for preparing iron phosphate materials cannot simultaneously achieve high tap density, uniform particle size distribution, and high purity. They also suffer from problems such as impurity residues, complex processes, and high costs, which cannot meet the needs of high-energy-density batteries.
By using a specific concentration ratio of iron solution and phosphorus solution, controlling pH and temperature, and carrying out the reaction through dropwise addition, combined with segmented calcination, large-layer battery-grade anhydrous iron phosphate is prepared, avoiding the use of additives and precisely controlling crystal growth.
Anhydrous iron phosphate with a regular large-scale layered structure was prepared, with uniform particle size distribution, high tap density, and high purity, making it suitable for high-energy-density battery systems, simplifying process steps and reducing costs.
Smart Images

Figure CN122079099A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium battery materials technology, specifically to a large-sheet battery-grade anhydrous iron phosphate and its preparation method. Background Technology
[0002] In the field of lithium-ion battery materials technology, iron phosphate, as a key precursor for lithium iron phosphate cathode materials, directly affects the compaction density, lithium-ion diffusion rate, and electrochemical performance of the final cathode material due to its microstructure and structural characteristics. In recent years, iron phosphate with layered or stacked structures has become a research hotspot in order to improve the specific surface area of iron phosphate materials and optimize ion transport pathways.
[0003] In existing technologies, the preparation of lithium iron phosphate materials typically relies on the addition of precipitants or dispersants to regulate their morphology. For example, Chinese patent application CN115432687A discloses a method for preparing lithium iron phosphate materials, which uses polyethylene glycol as a dispersant and structure-directing agent to impart a layered framework to lithium iron phosphate. While this process improves the uniformity of the morphology of lithium iron phosphate to some extent, it is prone to introducing impurities and increasing the difficulty of subsequent purification due to its reliance on external organic reagents, thus complicating the process. Chinese patent application CN118877850A discloses a method for preparing lithium iron phosphate materials, which involves actively doping with titanium to introduce defects in the crystal lattice, thereby inhibiting crystal growth along a specific direction and ultimately forming an ordered lamellar structure on the particle surface. However, this method requires the introduction of a large amount of titanium salt to induce morphology, resulting in a high residual titanium content in the lithium iron phosphate (>3000 ppm). Excessive titanium not only reduces the theoretical specific capacity limit of lithium iron phosphate by occupying active sites but also becomes a key bottleneck hindering its application in high-energy-density battery systems. Furthermore, the obtained iron phosphate D50 has a particle size of 30-60 μm, significantly exceeding the 1-9 μm particle size range recommended by the industry standard HG / T4701-2021 for anhydrous iron phosphate used in batteries. Excessively large particle size means a longer bulk diffusion path for lithium ions within the particles, which may exacerbate electrode polarization during high-rate charge and discharge, thus limiting the full realization of power performance. Current methods for preparing layered iron phosphate structures relying on "additive regulation," whether using polymeric additives or metal ion doping, inevitably lead to increased costs, more complex processes, residual impurities, and potential loss of material properties.
[0004] Current research also explores methods to control the growth of ferric phosphate by regulating the temperature rise time to obtain a lamellar structure, thus avoiding the addition of precipitants, dispersants, and other substances. For example, Chinese patent application CN117430099A discloses a method for preparing battery-grade lamellar anhydrous ferric phosphate. This method involves preparing a FeSO4 solution using iron rods as raw material, adding phosphoric acid to obtain a ferric phosphate slurry, precipitating the slurry by adding hydrogen peroxide for oxidation and adding NaOH to adjust the pH, followed by heating and aging with controlled aging time to achieve the lamellar structure of ferric phosphate. However, the anhydrous ferric phosphate prepared by this method does not have ideal performance, with a tap density of 0.50-0.58 g / cm³. 3The D50 particle size ranged from 1.75 to 4.42 μm, failing to meet the performance specifications recommended by the industry standard HG / T4701-2021 for anhydrous iron phosphate used in batteries. This makes it difficult to achieve excellent electrochemical performance in the subsequent preparation of lithium iron phosphate cathode materials. Chinese patent application CN110436428A discloses a method for preparing flake iron phosphate. This method primarily involves oxidizing a ferrous salt solution to an ferric salt solution, then adding the ferric salt solution at a certain rate to a phosphate salt solution preheated to 90-100°C for reaction, followed by calcination to obtain flake iron phosphate. This method rapidly forms a white flake iron phosphate product by adding the material at high temperatures, reducing the probability of sulfate ions being encapsulated within the flake iron phosphate, thereby significantly reducing the sulfur content in the finished product. However, research has revealed that this method still uses a phosphate salt system composed of phosphoric acid and sodium hydroxide, inevitably introducing metallic impurities such as sodium ions. Furthermore, this method only avoids sulfate encapsulation through high-temperature rapid reaction, without a dedicated crystal nucleation and growth control process. The resulting flake-like iron phosphate has only a basic flake morphology and lacks regular large-layer structure characteristics. The particle tap density is low, making it difficult to meet the dual requirements of high density and excellent morphology for iron phosphate precursors in high-energy-density battery systems. At the same time, it still uses high-purity ferrous salt as the iron source, resulting in high raw material costs and failure to realize the resource utilization of industrial by-products. Both cost and performance advantages are significantly lacking in industrial applications. Meanwhile, even existing technologies that attempt to control the growth of iron phosphate by regulating the temperature rise time to avoid additives suffer from problems such as low iron-phosphorus source concentration, easy introduction of alkali metal impurities into the reaction system, and limited crystal form control methods. As a result, the key indicators such as the tap density and particle size distribution of the prepared iron phosphate are difficult to meet the requirements of the industry standard "HG / T4701-2021". The lamellar regularity and uniformity are poor, and the subsequent prepared lithium iron phosphate performs poorly in terms of lithium ion diffusion rate and electrode tap density, which cannot meet the current industry demand for high energy density and high rate performance of power batteries. In summary, existing technologies for preparing layered iron phosphate either rely on additives or metal doping, leading to impurity residues and complex processes, or, while avoiding additives, suffer from low precision in morphology control, substandard product performance, and high raw material costs. There is an urgent need to develop a battery-grade anhydrous iron phosphate preparation method that requires no additives, can precisely control the regular morphology of large layers, and simultaneously achieves high tap density, high purity, and low raw material costs. This method would address the many drawbacks of existing technologies and meet the application requirements of high-energy-density battery systems. Summary of the Invention
[0005] To overcome the shortcomings of the existing technology, one of the objectives of this invention is to provide a method for preparing large-sheet battery-grade anhydrous iron phosphate, comprising the following steps:
[0006] S1. Prepare iron solution and phosphorus solution separately; the iron solution is ferric sulfate solution with an iron concentration of 55-65 g / L; the phosphorus solution is monoammonium phosphate solution with a phosphorus concentration of 80-100 g / L. S2. Adjust the pH of the iron solution to 1-2 using sulfuric acid. Preheat the phosphorus solution to 50-60℃ as the base solution and the iron solution to 50-60℃ as the dropping solution. Under stirring conditions, add the iron solution dropwise to the phosphorus solution. The amounts of iron and phosphorus solutions are controlled to maintain a phosphorus to iron molar ratio of 1.18-1.28. After the addition is complete, keep the temperature at 50-60℃ for 0.5-1 h, then raise the temperature to 85-95℃ and age for 2-3 h to obtain iron phosphate slurry. S3. Filter, wash and dry the ferric phosphate slurry to obtain ferric phosphate dihydrate. S4. Calcining ferric phosphate dihydrate yields anhydrous ferric phosphate for large-sheet battery applications.
[0007] By selecting a 55-65 g / L ferric sulfate solution for the iron solution and an 80-100 g / L monoammonium phosphate solution for the phosphorus solution, and matching this with a subsequent P / Fe molar ratio of 1.18-1.28, the goal of eliminating the need for additional dilution / concentration of the solution is achieved. This avoids excessively slow reaction rates and insufficient crystal growth, or excessively fast reaction rates and crystal agglomeration / distorted morphology, ensuring the uniformity of ferric phosphate crystal nucleation and growth, laying the foundation for the regularity of the lamellar structure. Simultaneously, the high-concentration phosphorus source as the base solution ensures an excess and uniform distribution of phosphorus during the addition of the iron solution, inhibiting localized hydrolysis of iron ions and reducing the probability of impurity formation. Using monoammonium phosphate as the sole phosphorus source, compared to the composite phosphorus source of phosphoric acid plus alkali solution in existing technologies, monoammonium phosphate is a single phosphorus source. The dissociated NH4+... 4+ It leaves no metal impurities and provides a mild buffer environment for the reaction system, avoiding crystal morphology loss due to sudden pH changes. It also solves the problem that composite phosphorus sources easily introduce alkali metal impurities and affect the electrochemical performance of lithium iron phosphate.
[0008] 50-60℃ is the optimal temperature for iron phosphate crystal nucleation. Simultaneous preheating of the phosphorus and iron solutions avoids sudden temperature drops in the reaction system caused by the addition of cold solutions, preventing abrupt changes in the crystal nucleation rate and resulting in uneven morphology, thus ensuring consistent nucleation of lamellar crystals. An excess phosphorus source is used as the base solution, while the iron source is added slowly, allowing iron ions to disperse evenly and react gradually within the phosphorus source. This avoids rapid crystal growth / agglomeration caused by excessively high local iron ion concentrations, achieving slow, orderly growth of lamellar crystals and improving the regularity and thickness uniformity of the lamellar layers.
[0009] Controlling the P / Fe molar ratio to 1.18-1.28 ensures sufficient coordination between phosphate and iron ions, enabling complete conversion of iron ions into iron phosphate and improving raw material utilization. Simultaneously, excess phosphate can adsorb onto the surface of iron phosphate crystals, inhibiting crystal growth along non-lamellar directions and inducing preferential growth along lamellar directions, thus enhancing the large lamellar structure. This ratio also reduces the amount of phosphate eluted during subsequent washing, lowering washing water consumption and process time, thus balancing reaction completeness and industrialization efficiency.
[0010] After the addition is complete, maintaining the temperature at 50-60℃ for 0.5-1 hour allows for slow and uniform nucleation of iron phosphate crystals, forming a large number of uniformly sized nuclei. This lays the foundation for subsequent high-temperature aging and avoids the problems of uneven nucleation rates and wide particle size distribution caused by a single high-temperature reaction. Then, raising the temperature to 85-95℃ for 2-3 hours increases the crystal growth rate, allowing nuclei to preferentially grow along the lamellar direction, forming large lamellar structures with uniform thickness and regular size. Simultaneously, the 2-3 hour aging time further refines the iron phosphate crystal form, increasing crystallinity and reducing lattice defects. The resulting anhydrous iron phosphate exhibits superior electrochemical performance after subsequent calcination. This two-stage temperature process allows for step-by-step control of nucleation and growth, overcoming the technical limitations of traditional processes that cannot precisely control product size, thickness, and uniformity. The resulting lamellar structure exhibits significantly better regularity than existing technologies.
[0011] Preferably, in step S1, the preparation method of the ferrous sulfate solution includes the following steps: preparing a ferrous sulfate solution using titanium dioxide byproducts, adjusting the pH to 3.5-4.5 with 20-30% ammonia water, filtering, and obtaining a purified ferrous sulfate solution; after complete oxidation with an oxidant, adjusting the pH to 1.0-1.5 with dilute sulfuric acid to obtain a ferrous sulfate solution. Titanium dioxide byproducts are waste products from the sulfuric acid process for titanium dioxide production. They are inexpensive and widely available, replacing high-purity ferrous sulfate raw materials, significantly reducing industrial production costs, and solving the environmental problem of byproduct accumulation. Through a two-step purification process of adjusting the pH to 3.5-4.5 with ammonia water and filtering, and reducing ferric iron with iron powder, heavy metal impurities such as titanium, calcium, magnesium, and aluminum in titanium dioxide byproducts can be effectively removed. At the same time, residual ferric iron is reduced to ferrous iron, avoiding uneven iron valence state caused by insufficient oxidation. The final ferric phosphate with impurity content is far lower than the standard of "HG / T4701-2021", improving the cycle stability of subsequent lithium iron phosphate.
[0012] Preferably, the oxidant is hydrogen peroxide, with a mass fraction of 20-30%. The amount of hydrogen peroxide used is 1-2 times the theoretical amount required to oxidize ferrous ions in the ferrous sulfate solution. The oxidation products of hydrogen peroxide are water and oxygen. Compared with oxidants such as sodium chlorate and nitric acid, there are no residual impurities such as chloride and nitrogen, avoiding the adsorption of impurities on the surface of ferric phosphate and affecting the subsequent lithiation reaction, thus ensuring the chemical purity of ferric phosphate. The 1-2 times theoretical amount of hydrogen peroxide ensures that ferrous ions are completely oxidized to ferric iron, while avoiding excessive oxidizing power of the system due to excessive oxidant, preventing premature precipitation of ferric phosphate precursor. After oxidation, dilute sulfuric acid is used to adjust the pH to 1.0-1.5, which can stabilize the chemical properties of the ferric sulfate solution, prevent the hydrolysis of ferric iron to generate ferric hydroxide impurities, and ensure the singularity of the subsequent reaction with the phosphorus source.
[0013] Preferably, the specific steps for preparing a ferrous sulfate solution using titanium dioxide byproducts are as follows: dissolve the titanium dioxide byproduct ferrous sulfate in deionized water, controlling the ferrous ion concentration in the solution to be 55-75 g / L, then add iron powder to reduce the residual ferric iron, stir the reaction for 20-40 minutes, and filter to obtain the ferrous sulfate solution. A small amount of ferric iron exists in the titanium dioxide byproducts; iron powder can selectively reduce ferric iron to ferrous iron, and excess iron powder can be removed by filtration without residue. This avoids incomplete oxidation reaction due to the presence of ferric iron, which could lead to an imbalance in the iron-to-phosphorus ratio in ferric phosphate, ensuring that the iron-to-phosphorus ratio of the product strictly meets industry standards.
[0014] Preferably, in step S2, the sulfuric acid is concentrated sulfuric acid with a mass fraction greater than 70%. Using concentrated sulfuric acid to adjust the pH to 1-2 provides a strongly acidic environment for the reaction system, preventing the hydrolysis of ferric iron during the dropwise addition of the iron solution to form ferric hydroxide colloids. This prevents the colloids from adsorbing onto the surface of the ferric phosphate crystals, which would lead to incomplete lamellar structures and increased impurity content. Under a strongly acidic environment, the coordination reaction between ferric iron and phosphate is the only major reaction, with no side reactions, thus improving the purity of ferric phosphate. The amount of concentrated sulfuric acid used is small, and subsequent washing can quickly remove it, avoiding excessive sulfate residue.
[0015] Preferably, in step S2, the stirring speed is 180-250 rpm; the dropping rate of the iron solution is 30-50 mL / min, and the dropping volume of the iron solution is 2-3 L. 180-250 rpm is a low-to-medium stirring speed, which ensures the homogeneity of the reaction system, prevents local concentration differences, and avoids the shearing damage to the nascent lamellar crystals caused by high speeds (e.g., 800 rpm), thus ensuring the integrity of the lamellar structure. Simultaneously, gentle stirring reduces collisions and agglomeration between crystals, improving the dispersibility of the product. The 2-3 L of iron solution is added at a rate of 30-50 mL / min, ensuring sufficient contact and reaction between iron ions and phosphate ions, and providing enough time for crystal nucleation and initial growth. This avoids excessively fast dropping rates leading to small crystals with excessively large specific surface areas, or excessively slow dropping rates leading to reduced production efficiency. This parameter synergizes with subsequent low-temperature holding and high-temperature aging to precisely control the D50 particle size to 5.66-6.57 μm. The stirring speed is matched with the dropping acceleration rate and the reaction temperature to keep the reaction system in a uniform reaction state without violent disturbance, thus achieving precise control of crystal growth.
[0016] Preferably, in step S3, the washing is performed using hot water at 65-75℃ for 3-7 minutes. Hot water at 65-75℃ can increase the solubility of soluble impurities such as sulfate and ammonium ions, and accelerate the desorption of impurities from the filter cake. The washing time of 3-7 minutes ensures that the impurities are completely washed away (so that the sulfur content is ≤300ppm), while avoiding the loss of iron phosphate crystals due to excessive washing time.
[0017] Preferably, in step S3, the drying temperature is 80-90℃, and the drying time is 12-24 hours. Drying at 80-95℃ is a low-temperature drying method, which can slowly remove free water and water of crystallization from the ferric phosphate filter cake, avoiding crystal structure collapse and lamellar cracking caused by high-temperature rapid drying, thus ensuring the integrity of the crystalline form of dihydrate ferric phosphate and laying the foundation for subsequent calcination to obtain regular anhydrous ferric phosphate lamellars. A drying time of 12-24 hours ensures complete removal of moisture from the ferric phosphate, preventing residual moisture from causing bumping during subsequent calcination, preventing damage to the crystal morphology, and simultaneously preventing water from reacting with ferric phosphate to generate impurities, ensuring product purity.
[0018] Preferably, in step S4, the calcination adopts a segmented heating method: heating to 500℃ at a heating rate of 3-5℃ / min and holding for 1-2 hours, then heating to 550-600℃ and calcining for 2-3 hours. Heating to 500℃ at a slow heating rate of 3-5℃ / min can slowly remove the water of crystallization of ferric phosphate dihydrate, avoiding excessively high crystal porosity and lamellar cracking caused by the instantaneous escape of water of crystallization due to rapid heating; holding at 500℃ for 1-2 hours can completely remove the water of crystallization, ensuring the consistency of crystal transformation in subsequent calcination. 550-600℃ is the optimal temperature for the crystal transformation of anhydrous ferric phosphate. Calcination at this temperature can completely convert ferric phosphate dihydrate into anhydrous ferric phosphate without causing sintering or agglomeration of lamellar crystals due to excessive temperature; the 2-3 hour calcination time can further improve the crystal form and increase the crystal density, with the final anhydrous ferric phosphate having a tap density of 2.72 g / cm³. 3 The above are far superior to existing technologies. The anhydrous iron phosphate obtained by segmented calcination has high crystallinity and fewer lattice defects. When used as a precursor for lithium iron phosphate, it reacts more fully with the lithium source, resulting in lithium iron phosphate with a faster lithium-ion diffusion rate, and superior rate performance and cycle stability.
[0019] Another objective of this application is to provide a large-sheet battery-grade anhydrous iron phosphate, prepared by any of the above-mentioned preparation methods.
[0020] The beneficial effects are as follows: The anhydrous iron phosphate preparation method provided in this application, through precise control of the pH, temperature, dropping rate, and reactant feeding method of the reaction system, successfully prepares high-performance battery-grade anhydrous iron phosphate with a regular large-layer structure and high chemical purity. Its D50 particle size is 5.66-6.57μm (the D50 particle size of the anhydrous iron phosphate prepared in this application is determined by the reaction process conditions, which can avoid the shearing and breakage of the layered crystals by high-energy pulverization, ensuring the integrity of the large-layer structure, thereby retaining the structural advantage of the layers shortening the lithium-ion migration path and improving the rate performance of subsequent lithium iron phosphate), and the tap density is 2.72-2.83g / cm³. 3 Within the specified range, it is far higher than the industry standard of ≥0.6g / cm³. 3 The requirement is a specific surface area of 3.13-5.23 m². 2The content of each component within the range of / g meets the requirements of HG / T4701-2021 standard, and the content of all impurities is lower than the standard limit. This structural characteristic allows it to shorten the lithium-ion migration path through the laminations, which is beneficial for rate performance, and to achieve higher electrode compaction density through its particle size distribution, thereby improving volumetric energy density. This technical solution does not add any additives such as precipitants, dispersants, or metal dopants throughout the process, completely avoiding impurity residues. The resulting iron phosphate has high purity, and the subsequently prepared lithium iron phosphate has no impurity sites, theoretical specific capacity is not lost, and it is suitable for high energy density battery systems. It also eliminates the need for additional additive dissolution, addition, and removal steps, making the process simple, with fewer operating parameters, easier to control during industrialization, saving the raw material cost of additives, and reducing the washing and purification costs caused by additive removal, thus significantly improving the industrial competitiveness of the process. Attached Figure Description
[0021] The accompanying drawings, which are included to provide a further understanding of this application and form part of this application, illustrate exemplary embodiments of this application and are used to explain this application, but do not constitute an undue limitation of this application. In the drawings: Figure 1 The scanning electron microscope (SEM) image of the iron phosphate dihydrate prepared in Example 1 shows that it exhibits a regular lamellar morphology with uniform lamellar thickness. Figure 2 The scanning electron microscope (SEM) image of the anhydrous iron phosphate prepared in Example 1 shows that it has a complete, uniformly thick lamellar structure. Figure 3 The X-ray diffraction (XRD) pattern of the anhydrous ferric phosphate prepared in Example 1 shows that the characteristic peaks are consistent with those of the standard card PDF#34-0134, and there are no impurity peaks, indicating that the product is pure phase anhydrous ferric phosphate. Detailed Implementation
[0022] The present invention will now be described in further detail with reference to specific embodiments, so that those skilled in the art can more clearly understand the present invention.
[0023] The following embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. All other embodiments obtained by those skilled in the art based on the specific embodiments of the invention without inventive effort are within the protection scope of the invention. The technical solutions of the various embodiments can be combined with each other, but only on the basis that those skilled in the art can implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope claimed by the invention.
[0024] In the embodiments of this invention, unless otherwise specified, all raw material components are commercially available products well-known to those skilled in the art; in the embodiments of this invention, unless specifically indicated, the technical means used are all conventional means well-known to those skilled in the art. Where specific experimental steps or conditions are not specified in the embodiments, they can be performed according to the conventional experimental steps or conditions described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all conventional reagent products that can be obtained commercially. The titanium dioxide by-product used in the embodiments and comparative examples of this invention is a by-product of the sulfuric acid process for producing titanium dioxide in titanium dioxide plants, and its main component is ferrous sulfate.
[0025] Example 1 This embodiment provides a method for preparing large-sheet battery-grade anhydrous iron phosphate, including the following steps: S1. Prepare iron solution and phosphorus solution separately; the iron solution is ferric sulfate solution with an iron concentration of 55 g / L; the phosphorus solution is monoammonium phosphate solution with a phosphorus concentration of 80 g / L. The preparation method of S1a ferrous sulfate solution includes the following steps: Ferrous sulfate solution is prepared using titanium dioxide byproducts; pH is adjusted to 3.5 by adding 20% ammonia water; the solution is filtered to obtain purified ferrous sulfate solution; 20% hydrogen peroxide hydroxide is added, with the amount of hydrogen peroxide being 1 times the theoretical amount of hydrogen peroxide required to oxidize ferrous ions in the ferrous sulfate solution; after complete oxidation, pH is adjusted to 1.0 by dilute sulfuric acid to obtain ferrous sulfate solution. S1aa, The specific steps for preparing ferrous sulfate solution using titanium dioxide by-products are as follows: dissolve ferrous sulfate by-products of titanium dioxide in deionized water, control the ferrous ion concentration in the solution to be 55 g / L, then add iron powder to reduce the residual ferric iron, stir the reaction for 20 min and filter to obtain ferrous sulfate solution. S2. Adjust the pH of the iron solution to 1 using concentrated sulfuric acid with a mass fraction greater than 70%. Preheat the phosphorus solution to 50°C as the base solution and the iron solution to 50°C as the dropping solution. Under stirring conditions, add the iron solution dropwise to the phosphorus solution. The stirring speed is 180 rpm, the dropping rate of the iron solution is 30 mL / min, and the dropping volume of the iron solution is 2 L. The amounts of iron solution and phosphorus solution are used to control the molar ratio of phosphorus to iron to be 1.18. After the dropping is completed, keep the temperature at 50°C for 0.5 h, and then raise the temperature to 85°C for aging for 2 h to obtain the iron phosphate slurry. S3. Filter the ferric phosphate slurry, wash it with hot water at 65℃ for 3 min, and dry it at 80℃ for 12 h to obtain ferric phosphate dihydrate. S4. Calcine iron phosphate dihydrate using a segmented heating method: heat to 500℃ at a heating rate of 3℃ / min and hold for 1 hour, then heat to 550℃ and calcine for 2 hours to prepare anhydrous iron phosphate for large-sheet battery applications.
[0026] Example 2 This embodiment provides a method for preparing large-sheet battery-grade anhydrous iron phosphate, including the following steps: S1. Prepare iron solution and phosphorus solution separately; the iron solution is ferric sulfate solution with an iron concentration of 58 g / L; the phosphorus solution is monoammonium phosphate solution with a phosphorus concentration of 85 g / L. The preparation method of S1a ferrous sulfate solution includes the following steps: Ferrous sulfate solution is prepared using titanium dioxide byproducts; pH is adjusted to 3.8 by adding 22% ammonia water; the solution is filtered to obtain purified ferrous sulfate solution; 22% hydrogen peroxide hydroxide is added, with the amount of hydrogen peroxide being 1.2 times the theoretical amount of hydrogen peroxide required to oxidize ferrous ions in the ferrous sulfate solution; after complete oxidation, pH is adjusted to 1.1 by dilute sulfuric acid to obtain ferrous sulfate solution. S1aa, The specific steps for preparing ferrous sulfate solution using titanium dioxide by-products are as follows: dissolve ferrous sulfate by-products of titanium dioxide in deionized water, control the concentration of ferrous ions in the solution to 60 g / L, then add iron powder to reduce the residual ferric iron, stir the reaction for 25 min and filter to obtain ferrous sulfate solution. S2. Adjust the pH of the iron solution to 1.2 using concentrated sulfuric acid with a mass fraction greater than 70%. Preheat the phosphorus solution to 52°C as the base solution and the iron solution to 52°C as the dropping solution. Under stirring conditions, add the iron solution dropwise to the phosphorus solution. The stirring speed is 200 rpm, the dropping rate of the iron solution is 35 mL / min, and the dropping volume of the iron solution is 2.2 L. The amounts of iron solution and phosphorus solution are used to control the molar ratio of phosphorus to iron to be 1.21. After the dropping is completed, keep the temperature at 52°C for 0.6 h, and then raise the temperature to 88°C for aging for 2.2 h to obtain the iron phosphate slurry. S3. Filter the ferric phosphate slurry, wash it with hot water at 68℃ for 4 min, and dry it at 82℃ for 16 h to obtain ferric phosphate dihydrate. S4. Calcine iron phosphate dihydrate using a segmented heating method: heat to 500℃ at a heating rate of 3.5℃ / min and hold for 1.2h, then heat to 565℃ and calcine for 2.2h to prepare anhydrous iron phosphate for large-sheet battery applications.
[0027] Example 3 This embodiment provides a method for preparing large-sheet battery-grade anhydrous iron phosphate, including the following steps: S1. Prepare iron solution and phosphorus solution separately; the iron solution is ferric sulfate solution with an iron concentration of 60 g / L; the phosphorus solution is monoammonium phosphate solution with a phosphorus concentration of 90 g / L. The preparation method of S1a ferrous sulfate solution includes the following steps: Ferrous sulfate solution is prepared using titanium dioxide byproducts; pH is adjusted to 4.0 with 25% ammonia water; the solution is filtered to obtain purified ferrous sulfate solution; 25% hydrogen peroxide hydroxide is added, with the amount of hydrogen peroxide being 1.5 times the theoretical amount of hydrogen peroxide required to oxidize ferrous ions in the ferrous sulfate solution; after complete oxidation, pH is adjusted to 1.2 with dilute sulfuric acid to obtain ferrous sulfate solution. S1aa, The specific steps for preparing ferrous sulfate solution using titanium dioxide by-products are as follows: dissolve ferrous sulfate by-products of titanium dioxide in deionized water, control the ferrous ion concentration in the solution to be 65 g / L, then add iron powder to reduce the residual ferric iron, stir the reaction for 30 min and filter to obtain ferrous sulfate solution. S2. Adjust the pH of the iron solution to 1.5 using concentrated sulfuric acid with a mass fraction greater than 70%. Preheat the phosphorus solution to 55°C as the base solution and the iron solution to 55°C as the dropping solution. Under stirring conditions, add the iron solution dropwise to the phosphorus solution. The stirring speed is 220 rpm, the dropping rate of the iron solution is 40 mL / min, and the dropping volume of the iron solution is 2.5 L. The amounts of iron solution and phosphorus solution are controlled to maintain a phosphorus to iron molar ratio of 1.24. After the dropping is completed, keep the temperature at 55°C for 0.75 h, and then raise the temperature to 90°C for aging for 2.5 h to obtain the iron phosphate slurry. S3. Filter the ferric phosphate slurry, wash it with hot water at 70℃ for 5 min, and dry it at 84℃ for 18 h to obtain ferric phosphate dihydrate. S4. Calcine iron phosphate dihydrate using a segmented heating method: heat to 500℃ at a heating rate of 4℃ / min and hold for 1.5h, then heat to 575℃ and calcine for 2.5h to prepare anhydrous iron phosphate for large-sheet battery applications.
[0028] Example 4 This embodiment provides a method for preparing large-sheet battery-grade anhydrous iron phosphate, including the following steps: S1. Prepare iron solution and phosphorus solution separately; the iron solution is ferric sulfate solution with an iron concentration of 62 g / L; the phosphorus solution is monoammonium phosphate solution with a phosphorus concentration of 95 g / L. The preparation method of S1a ferrous sulfate solution includes the following steps: Ferrous sulfate solution is prepared using titanium dioxide byproducts; pH is adjusted to 4.2 by adding 28% ammonia water; the solution is filtered to obtain purified ferrous sulfate solution; 28% hydrogen peroxide hydroxide is added, with the amount of hydrogen peroxide being 1.8 times the theoretical amount of hydrogen peroxide required to oxidize ferrous ions in the ferrous sulfate solution; after complete oxidation, pH is adjusted to 1.4 by dilute sulfuric acid to obtain ferrous sulfate solution. S1aa, The specific steps for preparing ferrous sulfate solution using titanium dioxide by-products are as follows: dissolve ferrous sulfate by-products of titanium dioxide in deionized water, control the ferrous ion concentration in the solution to be 70 g / L, then add iron powder to reduce the residual ferric iron, stir the reaction for 35 min and filter to obtain ferrous sulfate solution. S2. Adjust the pH of the iron solution to 1.8 using concentrated sulfuric acid with a mass fraction greater than 70%. Preheat the phosphorus solution to 58°C as the base solution and the iron solution to 58°C as the dropping solution. Under stirring conditions, add the iron solution dropwise to the phosphorus solution. The stirring speed is 230 rpm, the dropping rate of the iron solution is 45 mL / min, and the dropping volume of the iron solution is 2.8 L. The amounts of iron solution and phosphorus solution are controlled to maintain a phosphorus to iron molar ratio of 1.26. After the dropping is completed, keep the temperature at 58°C for 0.9 h, and then raise the temperature to 92°C for aging for 2.8 h to obtain the iron phosphate slurry. S3. Filter the ferric phosphate slurry, wash it with hot water at 72℃ for 6 min, and dry it at 86℃ for 22 h to obtain ferric phosphate dihydrate. S4. Calcine iron phosphate dihydrate using a segmented heating method: heat to 500℃ at a heating rate of 4.5℃ / min and hold for 1.8h, then heat to 590℃ and calcine for 2.8h to prepare anhydrous iron phosphate for large-sheet battery applications.
[0029] Example 5 This embodiment provides a method for preparing large-sheet battery-grade anhydrous iron phosphate, including the following steps: S1. Prepare iron solution and phosphorus solution separately; the iron solution is ferric sulfate solution with an iron concentration of 65 g / L; the phosphorus solution is monoammonium phosphate solution with a phosphorus concentration of 100 g / L. The preparation method of S1a ferrous sulfate solution includes the following steps: Ferrous sulfate solution is prepared using titanium dioxide byproducts; pH is adjusted to 4.5 by adding 30% ammonia water; the solution is filtered to obtain purified ferrous sulfate solution; 30% hydrogen peroxide hydroxide is added, with the amount of hydrogen peroxide being twice the theoretical amount of hydrogen peroxide required to oxidize ferrous ions in the ferrous sulfate solution; after complete oxidation, pH is adjusted to 1.5 by dilute sulfuric acid to obtain ferrous sulfate solution. S1aa, The specific steps for preparing ferrous sulfate solution using titanium dioxide by-products are as follows: dissolve ferrous sulfate by-products of titanium dioxide in deionized water, control the ferrous ion concentration in the solution to be 75 g / L, then add iron powder to reduce the residual ferric iron, stir the reaction for 40 min and filter to obtain ferrous sulfate solution. S2. Adjust the pH of the iron solution to 2 using concentrated sulfuric acid with a mass fraction greater than 70%. Preheat the phosphorus solution to 60°C as the base solution and the iron solution to 60°C as the dropping solution. Under stirring conditions, add the iron solution dropwise to the phosphorus solution. The stirring speed is 250 rpm, the dropping rate of the iron solution is 50 mL / min, and the dropping volume of the iron solution is 3 L. The amounts of iron solution and phosphorus solution are used to control the molar ratio of phosphorus to iron to be 1.28. After the dropping is completed, keep the temperature at 60°C for 1 h, and then raise the temperature to 95°C for aging for 3 h to obtain the iron phosphate slurry. S3. Filter the ferric phosphate slurry, wash it with hot water at 75℃ for 7 min, and dry it at 90℃ for 24 h to obtain ferric phosphate dihydrate. S4. Calcine iron phosphate dihydrate using a segmented heating method: heat to 500℃ at a heating rate of 5℃ / min and hold for 2 hours, then heat to 600℃ and calcine for 3 hours to prepare anhydrous iron phosphate for large-sheet battery applications.
[0030] Comparative Example 1 The preparation method of this comparative example differs from that of Example 1 only in that the molar ratio of phosphorus to iron in step S2 is 1.15. All other components and experimental steps are the same as those in Example 1.
[0031] Comparative Example 2 The preparation method of this comparative example differs from that of Example 1 only in that the dropping rate of the iron solution in step S2 is 55 mL / min. All other components and experimental steps are the same as those in Example 1.
[0032] Comparative Example 3 The preparation method of this comparative example differs from that of Example 1 only in that the phosphorus solution and iron solution were not preheated in step S2, and were directly added dropwise at room temperature (25°C). All other components and experimental steps are the same as those in Example 1.
[0033] Comparative Example 4 The only difference between the preparation method of this comparative example and that of Example 1 is that after the addition of the ingredients in step S2, a low-temperature holding reaction was not carried out, and the temperature was directly raised to 90°C for aging for 2.5 hours. All other components and experimental steps are the same as those in Example 1.
[0034] Comparative Example 5 The preparation method of this comparative example differs from that of Example 1 only in that the calcination in step S4 is performed by directly heating to 575°C and holding for 2.5 hours, without staged heating. All other components and experimental steps are the same as in Example 1.
[0035] The anhydrous ferric phosphates prepared in Examples 1-5 and Comparative Examples 1-5 were tested according to the standard "HG / T4701-2021". The test results are shown in Tables 1 and 2.
[0036] Table 1. Test results of various properties of anhydrous ferric phosphate in Examples 1-5
[0037] Note: ND means Not Detected.
[0038] Table 2. Test results of various properties of anhydrous ferric phosphate in Comparative Examples 1-5
[0039] Note: ND means Not Detected.
[0040] As shown in Table 1, the anhydrous ferric phosphate D50 prepared in Examples 1-5 had a particle size between 5.66 and 6.57 μm and a tap density between 2.72 and 2.83 g / cm³. 3 Within the specified range, it is far higher than the industry standard of ≥0.6g / cm³. 3 The requirement is a specific surface area of 3.13-5.23 m². 2 The concentrations of iron and phosphorus phosphates within the range of / g all meet the requirements of HG / T4701-2021 standard, and the content of all impurities is lower than the standard limit. This indicates that by precisely controlling the iron and phosphorus concentration, pH value, reaction temperature, dropping rate, and two-stage aging process, this invention can stably prepare anhydrous iron phosphate with a regular large-scale lamellar structure, high tap density, and uniform particle size distribution without adding any additives. Figures 1 to 3 As shown, Figure 1 The scanning electron microscope (SEM) image of the iron phosphate dihydrate prepared in Example 1 shows that it exhibits a regular lamellar morphology with uniform lamellar thickness. Figure 2 The scanning electron microscope (SEM) image of the anhydrous iron phosphate prepared in Example 1 shows that it has a complete, uniformly thick lamellar structure. Figure 3 The X-ray diffraction (XRD) pattern of the anhydrous ferric phosphate prepared in Example 1 shows that the characteristic peaks are consistent with those of the standard card PDF#34-0134, and there are no impurity peaks, indicating that the product is pure phase anhydrous ferric phosphate.
[0041] As shown in Table 2, in Comparative Example 1, the phosphorus-to-iron ratio was reduced to 1.15, resulting in an excess of phosphorus source and an insufficient amount of phosphorus, leading to a tap density of only 1.28 g / cm³. 3 The D50 particle size is only 2.89 μm, and the specific surface area is 6.15 m². 2 The phosphorus source in Comparative Example 2 was significantly inferior to that of the product in the previous example in terms of key indicators. This may be because insufficient phosphorus source prevented it from being fully adsorbed onto the surface of the iron phosphate crystals to induce preferential growth of the lamellar structure. As a result, the crystals tended to grow in random directions and agglomerate, disrupting the regularity of the lamellar structure. Simultaneously, the iron ions could not fully coordinate, leading to insufficient crystal growth, resulting in smaller particle size and a significant decrease in tap density. In Comparative Example 2, the excessively rapid dropping rate of the iron solution resulted in a tap density of 1.15 g / cm³. 3The D50 particle size is 3.22 μm, and the specific surface area is 6.56 m². 2 The performance of the sample with a density of 1.22 g / cm³ was poor. This may be because the rapid addition of iron ions caused a sudden increase in local concentration, which drastically accelerated the crystal nucleation and growth rate, making slow and orderly lamellar growth impossible. The resulting crystal particles were small and uneven in morphology, with increased porosity between particles, leading to a significant decrease in tap density and a larger specific surface area. Comparative Example 3, due to the lack of preheating treatment and direct addition at room temperature, had a tap density of 1.22 g / cm³. 3 The D50 particle size is 3.86 μm, and the specific surface area is 7.21 m². 2 The measured value of / g did not meet expectations. This may be because the addition of cold liquid droplets caused a sudden drop in the local temperature of the reaction system, resulting in abrupt changes in the crystal nucleation rate and disruption of nucleation uniformity. The resulting crystal nuclei were of uneven size, leading to significant differences in thickness and low regularity in the subsequently grown lamellar structures. Furthermore, the slow crystal growth rate at low temperatures made it difficult to form large, uniformly thick lamellar structures, ultimately resulting in a product with a smaller particle size and lower tap density. Comparative Example 4 did not undergo a low-temperature holding reaction and directly entered high-temperature aging, resulting in a tap density of 1.31 g / cm³. 3 The D50 particle size is 3.99 μm, and the specific surface area is 5.75 m². 2 The density of the sample was 1.36 g / cm³, which failed to form a high-quality large lamellar structure. This may be due to the lack of a low-temperature, uniform nucleation stage. Direct high-temperature aging causes nucleation and growth to occur simultaneously, resulting in uneven nucleation rates and a wide particle size distribution. Furthermore, rapid high-temperature growth easily leads to numerous crystal lattice defects and uneven lamellar thickness, making it impossible to form a dense, large lamellar structure, thus significantly reducing the tap density. Comparative Example 5, which used direct heating and calcination without segmentation, resulted in a tap density of 1.36 g / cm³. 3 The D50 particle size is 4.21 μm, and the specific surface area is 6.59 m². 2 The performance of the product ( / g) is far inferior to that of the example product. This is likely because the rapid heating causes the water of crystallization of ferric phosphate dihydrate to escape instantaneously, creating numerous pores within the crystal. This leads to cracking and damage in the lamellar structure, severely compromising its density. Even subsequent high-temperature calcination cannot repair the crystal structure, ultimately resulting in a low tap density and loss of lamellar structure integrity. These results demonstrate that the synergistic effect of the process parameters used in this invention is crucial for achieving a large lamellar structure and high tap density anhydrous ferric phosphate. Any deviation of any parameter from the set range will disrupt the control logic of crystal nucleation and growth, leading to a significant decrease in product performance.
[0042] In summary, by precisely controlling the pH, temperature, feeding method, and aging conditions of the reaction system, this invention successfully prepared high-performance battery-grade anhydrous iron phosphate with a regular large-scale lamellar structure, narrow particle size distribution, high tap density, and suitable specific surface area without adding any additives. This solves the problems of dependence on additives, difficulty in morphology control, and substandard performance in existing technologies, and has significant industrial application value.
[0043] The above are merely embodiments of the present invention and are not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principle of the present invention should be included within the scope of the claims of the present invention.
Claims
1. A method for preparing anhydrous iron phosphate for large-sheet battery applications, characterized in that, Includes the following steps: S1. Prepare iron solution and phosphorus solution separately; the iron solution is ferric sulfate solution with an iron concentration of 55-65 g / L; the phosphorus solution is monoammonium phosphate solution with a phosphorus concentration of 80-100 g / L; S2. Adjust the pH of the iron solution to 1-2 using sulfuric acid. Preheat the phosphorus solution to 50-60℃ as the base solution and the iron solution to 50-60℃ as the dropping solution. Under stirring conditions, add the iron solution dropwise to the phosphorus solution. The amounts of iron and phosphorus solutions are controlled to maintain a phosphorus to iron molar ratio of 1.18-1.
28. After the addition is complete, keep the temperature at 50-60℃ for 0.5-1 h, then raise the temperature to 85-95℃ and age for 2-3 h to obtain iron phosphate slurry. S3. Filter, wash and dry the ferric phosphate slurry to obtain ferric phosphate dihydrate. S4. Calcining ferric phosphate dihydrate yields anhydrous ferric phosphate for large-sheet battery applications.
2. The method for preparing large-sheet battery-grade anhydrous iron phosphate according to claim 1, characterized in that, In step S1, the method for preparing the ferrous sulfate solution includes the following steps: preparing a ferrous sulfate solution using titanium dioxide byproducts, adjusting the pH to 3.5-4.5 with 20-30% ammonia by mass, filtering to obtain a purified ferrous sulfate solution; adding an oxidant for complete oxidation, adjusting the pH to 1.0-1.5 with dilute sulfuric acid to obtain the ferrous sulfate solution.
3. The method for preparing large-sheet battery-grade anhydrous iron phosphate according to claim 2, characterized in that, The oxidant is hydrogen peroxide, with a mass fraction of 20-30%, and the amount of hydrogen peroxide used is 1-2 times the theoretical amount of hydrogen peroxide required to oxidize ferrous ions in ferrous sulfate solution.
4. The method for preparing large-sheet battery-grade anhydrous iron phosphate according to claim 2, characterized in that, The specific steps for preparing ferrous sulfate solution using titanium dioxide byproducts are as follows: dissolve ferrous sulfate, a byproduct of titanium dioxide, in deionized water, control the ferrous ion concentration in the solution to be 55-75 g / L, then add iron powder to reduce the residual ferric iron, stir the reaction for 20-40 min, and then filter to obtain ferrous sulfate solution.
5. The method for preparing large-sheet battery-grade anhydrous iron phosphate according to claim 1, characterized in that, In step S2, the sulfuric acid is concentrated sulfuric acid with a mass fraction greater than 70%.
6. The method for preparing large-sheet battery-grade anhydrous iron phosphate according to claim 1, characterized in that, In step S2, the stirring speed is 180-250 rpm; the dropping rate of the iron solution is 30-50 mL / min; and the dropping volume of the iron solution is 2-3 L.
7. The method for preparing large-sheet battery-grade anhydrous iron phosphate according to claim 1, characterized in that, In step S3, the washing process involves washing with hot water at 65-75℃ for 3-7 minutes.
8. The method for preparing large-sheet battery-grade anhydrous iron phosphate according to claim 1, characterized in that, In step S3, the drying temperature is 80-90℃ and the drying time is 12-24h.
9. The method for preparing large-sheet battery-grade anhydrous iron phosphate according to claim 1, characterized in that, In step S4, the calcination adopts a segmented heating method: heating to 500℃ at a heating rate of 3-5℃ / min and holding for 1-2 hours, then heating to 550-600℃ and calcining for 2-3 hours.
10. A large-sheet battery-grade anhydrous iron phosphate, characterized in that, It is prepared by the preparation method according to any one of claims 1-9.
Citation Information
Patent Citations
Preparation method of flaky iron phosphate, the prepared flaky iron phosphate and application of the flaky iron phosphate
CN110436428A
Preparation method of lithium iron phosphate material
CN115432687A
Preparation method of anhydrous iron phosphate with battery grade sheet structure
CN117430099A
Iron phosphate material, preparation method thereof, positive electrode material, positive electrode plate and secondary battery
CN118877850A