Toughened high-barrier phas composite and preparation method thereof
Patent Information
- Application Number
- CN202610967957.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-01
- Publication Date
- 2026-08-11
AI Technical Summary
然而,常规PHA材料本身存在一个突出的性能缺陷,即结晶度偏高、晶体球粒尺寸较大,导致其脆性显著,断裂伸长率极低,通常仅为2%~5%,抗撕裂强度和冲击强度严重不足
本申请通过在PHA基体中原位生成的接枝共聚物与交联弹性共聚物协同作用,使材料在获得优异断裂伸长率的同时,抗撕裂强度与抗冲击强度也大幅提高,从根源上解决了常规增韧PHA材料柔韧性和抗损伤能力不足的问题。进一步的,本申请采用具有磷酸盐与氨基双重基团的成核剂,使其通过化学附着于弹性微粒表面诱导界面结晶,进一步强化了两相结合与应力传递,改善材料的力学性能。最终,所得复合材料在长期使用中保持柔韧性和抗破裂能力,且降解能力良好,尤其适合用于对耐久性和阻隔性均有较高要求的可降解包装膜与农用地膜等领域。
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application relates to the field of biodegradable polyester plastics, and in particular to a toughened high-barrier PHA composite material and its preparation method. Background Technology
[0002] Polyhydroxyalkanoates (PHAs) are a class of biodegradable polyesters synthesized directly by microorganisms through carbon source fermentation. They have attracted widespread attention due to their complete degradation in various natural environments such as compost, soil, and seawater, as well as their excellent thermoplastic processing properties. Leveraging PHA's superior biodegradability, it is currently being used on a large scale in the industrial production of disposable products, such as shopping bags, food packaging films, straws, and disposable tableware. In scenarios with short lifecycles and high degradation requirements, these products can effectively replace traditional petroleum-based plastics, significantly reducing the risk of white pollution.
[0003] With increasingly stringent global environmental regulations and a deepening of the concept of sustainable development, not only disposable products, but also many durable consumer and industrial products with longer lifespans and higher mechanical performance requirements, such as durable packaging films, agricultural mulch films, and cushioning packaging for electronic products, are required to possess a certain degree of biodegradability at the end of their service life. Introducing PHA material systems into the production of such durable products not only aligns with the expanding application of biodegradable materials but also offers broad market prospects and significant environmental benefits. However, conventional PHA materials have a prominent performance defect: high crystallinity and large crystal spherule size, resulting in significant brittleness, extremely low elongation at break (typically only 2%–5%), and severely insufficient tear and impact strength. Under long-term use or repeated stress conditions, these products are prone to brittle fracture, failing to maintain good mechanical integrity and thus failing to meet the basic requirements of durable products for material toughness and reliability. Summary of the Invention
[0004] This application aims to provide a biodegradable PHA composite material that combines high elongation at break and high tear strength to meet the application requirements of durable products.
[0005] In a first aspect, this application provides a toughened high-barrier PHA composite material, comprising the following raw materials in parts by weight: The mixture comprises 100 parts of PHA copolymer, 1-3 parts of isocyanate chain extender, 10-20 parts of hydroxyl-containing acrylate copolymer, 5-10 parts of cross-linked acrylate copolymer, 3-10 parts of hydrophobic modified filler, 0.1-1 part of catalyst, 0.5-2 parts of nucleating agent, and 0.1-5 parts of other additives; the raw material monomers of the hydroxyl-containing acrylate copolymer include: 70-90 wt% soft monomer, 5-10 wt% hydroxyl acrylate, and 5-20 wt% hard monomer; the raw material monomers of the cross-linked acrylate copolymer include: 70-92 wt% soft monomer, 1-5 wt% divinylbenzene, 2-5 wt% epoxy acrylate, and 5-20 wt% hard monomer.
[0006] In one embodiment, the PHA copolymer is selected from one or more of poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), and poly(3-hydroxybutyrate-co-4-hydroxybutyrate).
[0007] Compared to PHA homopolymers, the above-mentioned PHA copolymers have a moderate crystallization rate and superior toughness compared to pure PHB.
[0008] In one embodiment, the soft monomer is selected from at least one of butyl acrylate, isooctyl acrylate, and ethyl acrylate; and / or, the hard monomer is selected from at least one of methyl methacrylate, styrene, and acrylonitrile.
[0009] In one embodiment, the hydroxy acrylate is selected from at least one of hydroxyethyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl acrylate; and / or, the epoxy acrylate is selected from at least one of glycidyl acrylate and allyl glycidyl ether.
[0010] In one embodiment, the isocyanate chain extender is selected from at least one of diphenylmethane diisocyanate, toluene diisocyanate, hexamethylene diisocyanate, and dicyclohexylmethane-4,4'-diisocyanate.
[0011] In one embodiment, the catalyst is an organotin catalyst, preferably dibutyltin dilaurate or stannous octoate.
[0012] In one embodiment, the acrylate copolymer with cross-linked structure and the acrylate copolymer with hydroxyl group are both obtained by free radical copolymerization reaction; wherein, the acrylate copolymer with cross-linked structure is an elastomer microsphere with cross-linked structure prepared by emulsion polymerization or suspension polymerization, with an average particle size of 0.1 to 5 μm; while the acrylate copolymer with hydroxyl group is a non-cross-linked linear copolymer.
[0013] This application employs both hydroxyl-containing acrylate copolymers and cross-linked acrylate copolymers to form a synergistic complementarity, thereby effectively improving the durability of PHA composite materials, especially enabling membrane products to simultaneously improve in terms of high elongation at break, high tear strength, and high impact strength.
[0014] Specifically, hydroxyl-containing acrylate copolymers are linear molecules with side hydroxyl groups derived from hydroxyl acrylates on their molecular chains. During melt extrusion processing, isocyanate chain extenders preferentially couple with the terminal carboxyl groups, terminal hydroxyl groups, and side hydroxyl groups of the PHA copolymer, generating PHA-acrylate graft copolymers in situ. This process not only achieves uniform dispersion of the elastomer phase in the PHA matrix but also firmly anchors the flexible segments to the matrix molecules through covalent bonds. When the material is subjected to tension, these grafted flexible segments can effectively transfer stress, thereby significantly improving the elongation at break of the material. However, studies have found that this grafting has a limited effect on preventing rapid crack propagation, as it does not significantly improve the material's tear strength and impact strength.
[0015] Cross-linked acrylate copolymers can overcome the above-mentioned shortcomings. These copolymers are pre-made elastomeric microspheres with a cross-linked network, their surfaces bearing active epoxy groups derived from epoxy acrylates. During melt blending, these epoxy groups can ring-open and react with the end groups of PHA, or be indirectly anchored by isocyanates and other active hydrogens in the system, thus uniformly embedding themselves into the continuous PHA phase. When the film is subjected to high-speed loads such as tearing or impact, these cross-linked elastic microparticles dissipate external energy through their own high-elastic deformation and the plastic deformation of the matrix surrounding the microparticles, and blunt and branch crack tips, fundamentally inhibiting the generation and propagation of microcracks, thereby significantly improving the tear strength and impact strength of the material.
[0016] Through the synergistic combination of two acrylate copolymers, PHA composite materials can withstand long-term repeated stress conditions without failing due to excessive deformation or sudden damage due to local cracks, exhibiting excellent durability and making them particularly suitable for preparing high-performance biodegradable membrane products.
[0017] It is worth noting that the amount of hydroxyl acrylate copolymers should be controlled to no more than 10 wt% to ensure sufficient grafting reaction sites without causing excessive local crosslinking.
[0018] In one embodiment, the nucleating agent is sodium 4-aminophenyl phosphate.
[0019] The nucleating agent 4-aminophenyl phosphate sodium salt selected in this application not only acts as heterogeneous crystal nuclei dispersed in the polymer melt, but more importantly, its terminal active amino groups can undergo ring-opening reactions or form strong interactions such as hydrogen bonds with the epoxy groups on the surface of the cross-linked acrylate copolymer at processing temperatures. This allows it to selectively accumulate and anchor on the surface of these cross-linked elastomer particles. This chemical attachment process prevents the nucleating agent from being randomly distributed, but rather directionally anchored on the surface of the cross-linked particles. When the PHA copolymer cools and crystallizes from the melt, these heterogeneous nucleation sites, uniformly dispersed on the particle surface, can induce PHA molecular chains to preferentially crystallize and grow lamellar crystals around the elastomer particles, thereby forming a strong interfacial bond between the PHA matrix and the elastomer particles.
[0020] This interfacial structure, which induces crystallization in situ on the surface of the elastomer, greatly enhances the bonding strength between the elastomer microparticles and the PHA continuous phase. This makes it less likely for the two phases to debond under stress, and stress can be more effectively transferred from the matrix to the cross-linked elastic microparticles. The elastic performance is fully utilized, and the tear resistance and impact resistance of the composite material are further improved. This plays an important role in ensuring the durability of the product.
[0021] In one embodiment, the hydrophobic modified filler is prepared as follows: Amminated fillers were prepared by surface modification of sheet-like fillers with aminosilane compounds; hydrophobically modified fillers were prepared by nucleophilic addition of the aminated fillers with long-chain alkyl acrylates. The mass ratio of the sheet filler to the aminosilane coupling agent is 100:1 to 5; the molar ratio of the aminosilane coupling agent to the long-chain alkyl acrylate is 1:2 to 3.
[0022] In one embodiment, the long-chain alkyl group has 10 to 18 carbon atoms.
[0023] For example, the long-chain alkyl acrylate is selected from one or more of decyl acrylate, undecyl acrylate, cetyl acrylate, and stearyl acrylate.
[0024] In one embodiment, the aminosilane coupling agent is preferably aminopropyltrimethoxysilane and / or aminopropyltriethoxysilane.
[0025] In one embodiment, the sheet filler is selected from at least one of talc, mica, montmorillonite, and kaolin.
[0026] The increased amorphous region after the aforementioned toughening and grafting modification of PHA leads to a decrease in water vapor barrier properties. This application compensates for and strengthens this by introducing hydrophobically modified fillers. The selected filler is a sheet-like filler with a superior aspect ratio, which, when dispersed in the matrix, can significantly extend the water vapor permeation path, effectively compensating for the loss of barrier performance. More importantly, this application chemically modifies the surface of the sheet-like filler. First, the filler surface is silanized with an aminosilane compound, resulting in a covalently bonded layer of organosiloxane containing active amino groups. Subsequently, the surface amino groups undergo nucleophilic addition with long-chain alkyl acrylates, chemically grafting long-chain alkyl and acrylate segments onto the filler surface. Through this chemical modification, the filler surface is grafted with long alkyl chains and organosilicon segments, significantly increasing hydrophobicity. This not only further reduces water vapor permeation and adsorption but also improves the interfacial compatibility between the filler and the hydrophobic PHA matrix.
[0027] In one embodiment, the other additives are selected from any one or more of lubricants, plasticizers, anti-hydrolysis agents, antioxidants, UV stabilizers, and pigments.
[0028] Secondly, this application provides a method for preparing a toughened high-barrier PHA composite material, comprising the following steps: A mixture is prepared by mixing PHA copolymer, isocyanate chain extender, hydroxyl-containing acrylate copolymer, cross-linked acrylate copolymer, hydrophobic modified filler, catalyst, nucleating agent and other additives; The mixture is fed into a screw extruder and blended and melt-extruded at 120℃~170℃. After cooling and granulation, PHA composite material is obtained.
[0029] In summary, this application has the following beneficial effects: This application achieves excellent elongation at break, while significantly improving tear strength and impact strength through the synergistic effect of graft copolymers and crosslinked elastic copolymers generated in situ within a PHA matrix. This fundamentally solves the problem of insufficient flexibility and damage resistance in conventional toughened PHA materials. Furthermore, this application employs a nucleating agent with both phosphate and amino groups, which chemically adheres to the surface of elastic microparticles and induces interfacial crystallization, further strengthening the bonding and stress transfer between the two groups and improving the material's mechanical properties. Ultimately, the resulting composite material maintains flexibility and fracture resistance during long-term use and exhibits good degradation ability, making it particularly suitable for applications requiring high durability and barrier properties, such as biodegradable packaging films and agricultural mulch films. Detailed Implementation
[0030] Preparation Example Preparation Example 1-1: An acrylate copolymer with hydroxyl groups was prepared according to the following steps: Add 180g of deionized water and 1.5g of sodium dodecyl sulfate to a reaction flask, stir to dissolve, then purge with nitrogen to remove air and maintain a nitrogen atmosphere. Pre-mix 80g of butyl acrylate, 7.5g of hydroxyethyl acrylate, and 12.5g of methyl methacrylate to obtain a monomer mixture. In another container, dissolve 0.6g of potassium persulfate in 10g of deionized water to prepare an initiator solution. Heat the flask in a water bath to 75°C, add 1 / 3 volume of the monomer mixture and 1 / 3 volume of the initiator solution, maintaining a stirring speed of 250 rpm to initiate the reaction. After the temperature rises back up, maintain the temperature at 75–78°C for 30 minutes. Then, add the remaining monomer mixture and initiator solution dropwise using a peristaltic pump over approximately 2.5 hours. After the addition is complete, raise the temperature to 80°C and maintain the temperature for another 1.5 hours. Cool to room temperature, adjust the pH to approximately 7 with ammonia, and filter through a 300-mesh filter to obtain an emulsion. The resulting emulsion was dried using a spray dryer with an inlet temperature of 150°C and an outlet temperature of 80°C. The dried white powder was collected, which is the non-crosslinked acrylate copolymer with hydroxyl groups.
[0031] Preparation Examples 1-2: hydroxyl-containing acrylate copolymers were prepared according to the following steps: Add 190g of deionized water and 1.2g of sodium dodecyl sulfate to a reaction flask, stir to dissolve, then purge with nitrogen to remove air and maintain a nitrogen atmosphere. Mix 70g of butyl acrylate, 10g of hydroxyethyl methacrylate, and 20g of styrene thoroughly beforehand. Dissolve 0.5g of ammonium persulfate in 10g of deionized water. Heat in a water bath to 72°C, then add 1 / 4 volume of the monomer mixture and 1 / 4 volume of the initiator solution, stirring at 230 rpm to initiate the reaction. After the temperature rises back up, maintain the temperature at 75–78°C for 20 minutes. Then, add the remaining monomer mixture and initiator solution dropwise, controlling the dropping rate to maintain the reaction temperature at 75–78°C, for 2 hours. After the addition is complete, raise the temperature to 82°C and maintain for 1 hour. Cool to room temperature, adjust the pH to approximately 7 with ammonia, and filter to obtain the emulsion. The resulting emulsion was dried using a spray dryer with an inlet temperature of 140°C and an outlet temperature of 70°C. The dried white powder was collected, which is the non-crosslinked acrylate copolymer with hydroxyl groups.
[0032] Preparation Examples 1-3: acrylate copolymers with hydroxyl groups were prepared according to the following steps: Add 200g of deionized water and 2.0g of sodium dodecyl sulfate to a reaction flask, stir to dissolve, then purge with nitrogen to remove air and maintain a nitrogen atmosphere. Pre-mix 90g of isooctyl acrylate, 5g of hydroxypropyl acrylate, and 5g of acrylonitrile to obtain a monomer mixture. In another container, dissolve 0.8g of potassium persulfate in 10g of deionized water to prepare an initiator solution. Heat the flask in a water bath to 75°C, add 1 / 3 volume of the monomer mixture and 1 / 3 volume of the initiator solution, maintaining a stirring speed of 250 rpm to initiate the reaction. After the temperature rises back up, maintain the temperature at 70–73°C for 30 minutes. Then, use a peristaltic pump to add the remaining monomer mixture and initiator solution dropwise over approximately 3 hours. After the addition is complete, raise the temperature to 75°C and maintain the temperature for 1 hour. Cool to room temperature, adjust the pH to approximately 7 with ammonia, and filter through a 300-mesh filter to obtain an emulsion. The resulting emulsion was dried using a spray dryer with an inlet temperature of 150°C and an outlet temperature of 80°C. The dried white powder was collected, which is the non-crosslinked acrylate copolymer with hydroxyl groups.
[0033] Preparation Examples 1-4 are acrylate copolymers with hydroxyl groups, which differ from Preparation Example 1-1 in that an equal amount of butyl acrylate is used instead of hydroxyethyl acrylate.
[0034] Preparation Example 2-1, an acrylate copolymer with a cross-linked structure, was prepared according to the following steps: Add 220g deionized water, 1.2g sodium dodecylbenzenesulfonate, and 0.3g sodium bicarbonate to a reaction flask, stir to dissolve, and purge with nitrogen for 30 minutes while maintaining positive pressure. Mix 81g butyl acrylate, 3g divinylbenzene, 4g glycidyl methacrylate, and 12g methyl methacrylate thoroughly. Dissolve 0.35g potassium persulfate in 15g deionized water to prepare an initiator solution. Heat the mixture in a water bath to 72℃, add 1 / 4 of the total volume of the monomer mixture and 1 / 4 of the initiator solution, stir at 200rpm, and maintain the temperature at 75℃ for 20 minutes. Then, simultaneously add the remaining monomer and initiator solution dropwise over 2 hours, controlling the reaction temperature at 75-78℃. After the dropwise addition is complete, raise the temperature to 82℃ and continue the reaction for 1.5 hours. Cool, adjust the pH to approximately 7, and filter through a 200-mesh filter to obtain a cross-linked elastomer microsphere emulsion with an average microsphere size of approximately 1.2μm. The resulting emulsion was spray-dried (inlet temperature 160℃, outlet temperature 75℃) and then collected to obtain an acrylate copolymer powder with a cross-linked structure.
[0035] Preparation Example 2-2, an acrylate copolymer with a cross-linked structure, was prepared according to the following steps: Add 200g deionized water, 1.0g sodium dodecylbenzenesulfonate, and 0.2g sodium bicarbonate to a reaction flask, stir to dissolve, and purge with nitrogen for 30 minutes while maintaining positive pressure. Mix 70g butyl acrylate, 5g divinylbenzene, 5g glycidyl acrylate, and 20g styrene thoroughly. Dissolve 0.4g potassium persulfate in 15g deionized water to prepare an initiator solution. Heat the mixture in a water bath to 70℃, add 1 / 4 of the total volume of the monomer mixture and 1 / 4 of the initiator solution, stir at 200rpm, and maintain the temperature at 73℃ for 30 minutes. Then, simultaneously add the remaining monomer and initiator solution dropwise over 2.5 hours, controlling the reaction temperature at 73–76℃. After the dropwise addition is complete, raise the temperature to 80℃ and continue the reaction for 1.5 hours. Cool, adjust the pH to approximately 7, and filter through a 200-mesh filter to obtain a cross-linked elastomer microsphere emulsion with an average microsphere size of approximately 0.8μm. The resulting emulsion was spray-dried (inlet temperature 160℃, outlet temperature 75℃) and then collected to obtain an acrylate copolymer powder with a cross-linked structure.
[0036] Preparation Examples 2-3: Crosslinked acrylate copolymers were prepared according to the following steps: Add 250g deionized water, 0.8g sodium dodecylbenzenesulfonate, and 0.3g sodium bicarbonate to a reaction flask, stir to dissolve, and purge with nitrogen for 30 minutes while maintaining positive pressure. Mix 92g isooctyl acrylate, 1g divinylbenzene, 2g glycidyl methacrylate, and 5g styrene thoroughly. Dissolve 0.3g potassium persulfate in 12g deionized water to prepare an initiator solution. Heat the mixture in a water bath to 70°C, add 1 / 5 of the total volume of the monomer mixture and 1 / 5 of the initiator solution, and stir at 200 rpm. After the temperature returns to 70°C, maintain the reaction temperature for 30 minutes. Then, simultaneously add the remaining monomer and initiator solution dropwise over 3 hours, controlling the reaction temperature at 70–73°C. After the dropwise addition is complete, raise the temperature to 78°C and continue the reaction for 2 hours. Cool, adjust the pH to approximately 7, and filter through a 200-mesh filter to obtain a cross-linked elastomer microsphere emulsion with an average microsphere size of approximately 2.5 μm. The resulting emulsion was spray-dried (inlet temperature 160℃, outlet temperature 75℃) and then collected to obtain an acrylate copolymer powder with a cross-linked structure.
[0037] Preparation Example 2-4 is an acrylate copolymer with a cross-linked structure, which differs from Preparation Example 2-1 in that an equal amount of butyl acrylate is used instead of divinylbenzene.
[0038] Preparation Example 3-1, hydrophobic modified filler, was prepared according to the following operation: In a reaction flask, 100 g of mica powder (average particle size 5 μm) was mixed with 280 mL of anhydrous ethanol and 20 mL of deionized water, and sonicated for 20 minutes. Then, 3 g of aminopropyltrimethoxysilane was added, and the pH was adjusted to 4–5 with acetic acid. The mixture was stirred in a 60 °C water bath for 4 hours. After cooling to room temperature, the mixture was filtered, washed three times with ethanol to remove unreacted silane, and dried under vacuum at 80 °C to obtain the aminated filler. This aminated filler was transferred to another dry three-necked flask, 200 mL of anhydrous toluene was added, and the mixture was sonicated and dispersed. Then, 13.6 g of stearyl acrylate and 0.05 g of hydroquinone were added as polymerization inhibitors. The mixture was protected under nitrogen and stirred at 75 °C for 8 hours. After the reaction was complete, the mixture was cooled, filtered, and washed with toluene and ethanol, respectively. The product was dried under vacuum at 60 °C to constant weight to obtain the hydrophobic modified filler.
[0039] Preparation Example 3-2, hydrophobic modified filler, was prepared according to the following operation: In a reaction flask, 100 g of mica powder (average particle size 10 μm) was mixed with 290 mL of anhydrous ethanol and 10 mL of deionized water, and sonicated for 20 minutes. Then, 2 g of aminopropyltriethoxysilane was added, and the pH was adjusted to 4–5 with acetic acid. The mixture was stirred in a 50 °C water bath for 5 hours. After cooling to room temperature, the mixture was filtered, washed three times with ethanol to remove unreacted silane, and dried under vacuum at 80 °C to obtain the aminated filler. This aminated filler was transferred to another dry three-necked flask, 150 mL of anhydrous toluene was added, and the mixture was sonicated and dispersed. Then, 5.9 g of cetyl acrylate and 0.03 g of hydroquinone were added as polymerization inhibitors. The mixture was protected under nitrogen and stirred at 70 °C for 10 hours. After the reaction was complete, the mixture was cooled, filtered, and washed with toluene and ethanol, respectively. The product was dried under vacuum at 60 °C to constant weight to obtain the hydrophobic modified filler.
[0040] Preparation Example 3-3, hydrophobic modified filler, was prepared according to the following operation: In a reaction flask, 100 g of mica powder (average particle size 5 μm) was mixed with 280 mL of anhydrous ethanol and 20 mL of deionized water, and sonicated for 20 minutes. Then, 5 g of aminopropyltrimethoxysilane was added, and the pH was adjusted to 4–5 with acetic acid. The mixture was stirred in a 65°C water bath for 5 hours. After cooling to room temperature, the mixture was filtered, washed three times with ethanol to remove unreacted silane, and dried under vacuum at 80°C to obtain the aminated filler. This aminated filler was transferred to another dry three-necked flask, and 250 mL of anhydrous toluene was added. After ultrasonic dispersion, 27.1 g of stearyl acrylate and 0.08 g of hydroquinone were added as polymerization inhibitors. The mixture was protected under nitrogen and stirred at 80°C for 12 hours. After the reaction was complete, the mixture was cooled, filtered, and washed with toluene and ethanol, respectively. The product was dried under vacuum at 60°C to constant weight to obtain the hydrophobic modified filler.
[0041] Preparation Example 3-4, a hydrophobic modified filler, differs from Preparation Example 3-1 in that no long-chain alkyl acrylate was added for nucleophilic addition. The specific operation is as follows: In a reaction flask, 100 g of mica powder (average particle size 5 μm) was mixed with 280 mL of anhydrous ethanol and 20 mL of deionized water, and sonicated for 20 minutes. Then, 3 g of aminopropyltrimethoxysilane was added, and the pH was adjusted to 4–5 with acetic acid. The mixture was stirred in a 60 °C water bath for 4 hours. After cooling to room temperature, the mixture was filtered, washed three times with ethanol to remove unreacted silane, and dried under vacuum at 80 °C to obtain the hydrophobic modified filler.
[0042] Example Example 1: A toughened high-barrier PHA composite material was prepared according to the following steps: 1000g of poly(3-hydroxybutyrate-co-3-hydroxyvalerate) copolymer (Beijing Microstructure Workshop Biotechnology Co., Ltd., brand name PV3000G) was weighed and dried in a vacuum oven at 60℃ for 4 hours. The dried copolymer, along with 150g of hydroxyl-containing acrylate copolymer powder prepared according to Preparation Example 1-1, 80g of cross-linked acrylate copolymer powder prepared according to Preparation Example 2-1, 60g of hydrophobic modified filler prepared according to Preparation Example 3-1, 10g of nucleating agent sodium 4-aminophenyl phosphate (CAS 108084-47-5), and other auxiliaries consisting of 10g calcium stearate and 10g antioxidant 1010, were added to a high-speed mixer and mixed at 500rpm for 5 minutes at room temperature. Subsequently, 20g of diphenylmethane diisocyanate and 5g of catalyst dibutyltin dilaurate were pre-mixed evenly and poured into the mixer, and mixing was continued for 3 minutes to obtain the mixture. The mixture is added to a twin-screw extruder. The temperatures of each zone of the extruder are set as follows: feeding zone 120℃, conveying zone 140℃, melting zone 150℃, homogenizing zone 155℃, and die head 155℃. The screw speed is 200 rpm. The molten extruded strip is cooled in a water tank, air-dried, and pelletized.
[0043] Example 2: A toughened high-barrier PHA composite material was prepared according to the following steps: 1000g of poly(3-hydroxybutyrate-co-3-hydroxyvalerate) copolymer (Beijing Microstructure Workshop Biotechnology Co., Ltd., brand name PV3000G) was weighed and dried in a vacuum oven at 60℃ for 4 hours. The dried copolymer, along with 120g of hydroxyl-containing acrylate copolymer powder prepared according to Preparation Example 1-2, 60g of cross-linked acrylate copolymer powder prepared according to Preparation Example 2-2, 40g of hydrophobic modified filler prepared according to Preparation Example 3-2, 8g of nucleating agent sodium 4-aminophenyl phosphate (CAS 108084-47-5), and other additives consisting of 5g calcium stearate and 5g antioxidant 1010, were added to a high-speed mixer and mixed at 500rpm for 5 minutes at room temperature. Subsequently, 15g of hexamethylene diisocyanate and 3g of catalyst stannous octoate were pre-mixed evenly and poured into the mixer, and mixing was continued for 3 minutes to obtain the mixture. The mixture is added to a twin-screw extruder. The temperatures of each zone of the extruder are set as follows: feeding zone 120℃, conveying zone 135℃, melting zone 145℃, homogenizing zone 150℃, and die head 150℃. The screw speed is 200 rpm. The molten extruded strip is cooled in a water tank, air-dried, and pelletized.
[0044] Example 3: A toughened high-barrier PHA composite material was prepared according to the following steps: 1000g of poly(3-hydroxybutyrate-co-3-hydroxyvalerate) copolymer (Beijing Microstructure Workshop Biotechnology Co., Ltd., brand name PV3000G) was weighed and dried in a vacuum oven at 60℃ for 4 hours. The dried copolymer, along with 180g of hydroxyl-containing acrylate copolymer powder prepared according to Preparation Examples 1-3, 90g of cross-linked acrylate copolymer powder prepared according to Preparation Examples 2-3, 80g of hydrophobic modified filler prepared according to Preparation Examples 3-3, 18g of nucleating agent sodium 4-aminophenyl phosphate (CAS 108084-47-5), and other auxiliaries consisting of 15g of calcium stearate and 10g of antioxidant 1010, were added to a high-speed mixer and mixed at 500rpm for 5 minutes at room temperature. Subsequently, 28g of diphenylmethane diisocyanate and 8g of catalyst dibutyltin dilaurate were pre-mixed evenly and poured into the mixer, and mixing was continued for 3 minutes to obtain the mixture. The mixture is added to a twin-screw extruder. The temperatures of each zone of the extruder are set as follows: feeding zone 125℃, conveying zone 140℃, melting zone 150℃, homogenizing zone 155℃, and die head 155℃. The screw speed is 200 rpm. The molten extruded strip is cooled in a water tank, air-dried, and pelletized.
[0045] Example 4, a toughened high-barrier PHA composite material, differs from Example 1 in that the hydrophobic modified filler of Preparation Example 3-1 is replaced with an equal amount of the hydrophobic modified filler of Preparation Example 3-4.
[0046] Example 5, a toughened high-barrier PHA composite material, differs from Example 1 in that an equal amount of sodium 2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate is used to replace sodium 4-aminophenyl phosphate.
[0047] Example 6, a toughened high-barrier PHA composite material, differs from Example 1 in that an equal amount of bis(3,4-dimethylbenzyl)sorbitol is used to replace sodium 4-aminophenyl phosphate.
[0048] Comparative Example Comparative Example 1, a toughened high-barrier PHA composite material, differs from Example 1 in that an equal amount of hydroxyl-containing acrylate copolymer powder prepared in Preparation Examples 1-4 is used instead of the hydroxyl-containing acrylate copolymer powder prepared in Preparation Examples 1-1.
[0049] Comparative Example 2, a toughened high-barrier PHA composite material, differs from Example 1 in that an equal amount of cross-linked acrylate copolymer powder prepared in Preparation Examples 2-4 is used instead of the cross-linked acrylate copolymer powder prepared in Preparation Example 2-1.
[0050] Comparative Example 3, a toughened high-barrier PHA composite material, differs from Example 1 in that an equal amount of hydroxyl-containing acrylate copolymer powder prepared in Preparation Example 1-1 is used instead of the cross-linked acrylate copolymer powder prepared in Preparation Example 2-1.
[0051] Comparative Example 4, a toughened high-barrier PHA composite material, differs from Example 1 in that an equal amount of cross-linked acrylate copolymer powder prepared in Preparation Example 2-1 is used instead of the hydroxyl-containing acrylate copolymer powder prepared in Preparation Example 1-1.
[0052] Performance testing Experiment 1: Tensile property test The composite material granules obtained in each embodiment and comparative example were blown into flat films with a thickness of 0.1 mm ± 0.01 mm using a single-screw blown film mill (length-to-diameter ratio 25:1, die diameter 60 mm, processing temperature 145–165 °C). Testing was conducted according to GB / T1040.3-2006 "Determination of tensile properties of plastics—Part 3: Test conditions for films and sheets". Five type 2 dumbbell-shaped specimens (10 mm wide, gauge length 50 mm) were punched from the film longitudinally and transversely using a cutter. After conditioning the specimens in a standard environment for 4 hours, they were tested on a universal testing machine. The clamp spacing was set to 50 mm, and the test speed was set to 500 mm / min. The tensile strength at break (MPa) and elongation at break (%) were recorded, and the arithmetic mean of the five specimens in the longitudinal and transverse directions was used as the final result.
[0053] Experiment 2: Tear Resistance Test Films from the same batch as those used in Test 1 were used, and the tests were conducted according to GB / T 16578.2-2009 "Determination of tear resistance of plastic films and sheets – Part 2: Elmendorf method". Ten specimens of specified dimensions were cut in both the longitudinal and transverse directions. Using a testing machine equipped with an Elmendorf tear device, an appropriate pendulum capacity was selected so that the tear reading fell between 15% and 85% of full scale. The specimens were placed in the instrument fixture, clamped, and the pendulum was released pneumatically or manually to tear the specimens, recording the tear force (mN). The median value of the tear resistance in each of the 10 longitudinal and transverse specimens was used to represent the tear strength in that direction.
[0054] Experiment 3: Impact Strength Test Films from the same batch as those used in Test 1 were tested according to GB / T 9639.1-2008 "Test Methods for Impact Resistance of Plastic Films and Sheets - Free-Falling Dart Method - Part 1: Step Method". Film samples measuring 200mm × 200mm were cut and conditioned for 8 hours in a standard environment. A dart impact tester with a dart head diameter of 38mm was used to determine the breaking mass of the film under free-falling dart impact using the step method. The initial dart mass was selected near the estimated breaking mass, and the drop height was fixed at 660mm. If the sample did not break, the dart mass was increased by one increment; if it broke, the increment was decreased. Breakage was defined as the appearance of any penetrating crack or hole on the sample. Twenty valid data points were collected for each type of film, and the impact breaking mass (g) was calculated according to the standard method, which was used as the impact strength.
[0055] Experiment 4: Water Barrier Performance Test The blown film from Experiment 1 was selected and tested according to GB / T 1037-2021 "Determination of Water Vapor Transmission Performance of Plastic Films and Sheets - Cup Weight Gain Method". A circular sample with a diameter of 70 mm was cut, with uniform thickness and no pinholes. Approximately 10 g of anhydrous calcium chloride was placed in a permeation cup as a desiccant, with the desiccant about 3 mm from the lower surface of the sample. The sample was fixed to the mouth of the permeation cup with sealing wax or a sealing ring, ensuring a tight seal around the perimeter. The assembled permeation cup was placed in a constant temperature and humidity chamber at 38℃±0.6℃ and 90%±2% relative humidity, maintaining a specified humidity difference on both sides of the sample. The sample was weighed periodically until the mass gain reached a stable permeability state. The water vapor transmission rate (WVT) and water vapor transmission coefficient (g·mm / (m²·24h)) were calculated using the formula, and the average value of five samples was taken as the final result.
[0056] Table 1 Test Results
[0057] The experimental results in the table above show that: Compared to Example 1, Example 4 used a hydrophobically modified filler without nucleophilic addition of long-chain alkyl acrylates. Its water vapor permeability coefficient increased significantly, and its barrier performance deteriorated markedly. Simultaneously, its tear strength and dart impact fracture quality also decreased slightly. This may be because the filler surface treated only with aminosilane lacks the chemical grafting of long-chain alkyl groups, resulting in insufficient hydrophobicity and poor interfacial compatibility with the PHA matrix. This not only fails to effectively block water vapor penetration but also reduces the interfacial bonding effect, weakening the filler's reinforcing effect on the matrix.
[0058] Example 5 used sodium 2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate to replace sodium 4-aminophenyl phosphate in Example 1. Its tear strength and dart impact fracture quality were significantly reduced, and its elongation at break also decreased to some extent. This may be because, although conventional phosphate nucleating agents can play a role in heterogeneous nucleation and grain refinement, they lack active amino groups that can react with the epoxy groups on the surface of cross-linked acrylate copolymers, and therefore cannot be directionally anchored on the surface of elastomer particles. Consequently, a strong interfacial crystalline layer cannot be induced in situ at the elastomer-PHA two-phase interface, resulting in decreased interfacial bonding strength, reduced stress transfer efficiency, and weakened tear and impact resistance. Example 6 used a dibenzyl sorbitol-based nucleating agent to replace sodium 4-aminophenyl phosphate, further reducing its tear strength and dart impact fracture quality, and showing a more significant decrease in mechanical properties. The reason is similar to that in Example 5. Sorbitol nucleating agents also lack active amino groups, which prevents the nucleating agents from anchoring and accumulating on the surface of elastomer particles. As a result, they cannot strengthen the interfacial bonding between the two phases and improve mechanical properties through interfacial induced crystallization.
[0059] Comparative Example 1 used a hydroxyl-free acrylate copolymer to replace the hydroxyl-containing acrylate copolymer, resulting in a sharp decrease in elongation at break and a significant deterioration in the flexibility of the composite material. This is because the acrylate copolymer lacking side hydroxyl groups cannot chemically graft with PHA via isocyanate chain extenders during melt blending; it can only be dispersed in the matrix through physical blending. Due to the lack of covalent bonds, these linear elastomers are prone to debonding from the matrix under tension, failing to effectively transfer and dissipate stress, thus having a very limited effect on improving elongation at break. Comparative Example 2 used a crosslinked acrylate copolymer without crosslinking monomers to replace the crosslinked acrylate copolymer, resulting in a significant deterioration in tear strength and dart impact fracture quality, exhibiting extremely poor damage resistance. This is because, without the crosslinking network provided by divinylbenzene, the copolymer particles are merely linear or slightly branched elastomer aggregates, lacking sufficient cohesive strength. When the material is subjected to tearing or high-speed impact loads, these particles cannot effectively blunt crack tips and dissipate energy, leading to a sharp decrease in their contribution to tear and impact resistance.
[0060] Comparative Example 3 used only acrylate copolymers with hydroxyl groups, without adding acrylate copolymers with cross-linked structures. Although it had the highest elongation at break, its tear strength and dart impact fracture quality were significantly lower than those of Example 1. This reveals the synergistic complementary effect of the two copolymers. The hydroxyl-containing copolymer mainly contributes to improving the elongation at break and imparting ductility to the material; however, without the pinning, passivation, and energy dissipation effects of the cross-linked elastic microparticles on cracks, the material is extremely prone to failure under tearing and impact loads. Comparative Example 4 used only acrylate copolymers with cross-linked structures, without adding acrylate copolymers with hydroxyl groups. Although it had higher tear strength and dart impact fracture quality, its elongation at break was significantly lower than that of Example 1, and the material's flexibility was severely insufficient. This indicates that without a linear toughening phase that can form covalent grafts with the matrix, the cross-linked microparticles, while providing some tear resistance and impact strength, cannot effectively improve the overall ductility of the material.
[0061] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A toughened high-barrier PHA composite material, characterized in that, The raw materials include the following parts by weight: The mixture comprises 100 parts of PHA copolymer, 1-3 parts of isocyanate chain extender, 10-20 parts of hydroxyl-containing acrylate copolymer, 5-10 parts of cross-linked acrylate copolymer, 3-10 parts of hydrophobic modified filler, 0.1-1 part of catalyst, 0.5-2 parts of nucleating agent, and 0.1-5 parts of other additives; the raw material monomers of the hydroxyl-containing acrylate copolymer include: 70-90 wt% soft monomer, 5-10 wt% hydroxyl acrylate, and 5-20 wt% hard monomer; the raw material monomers of the cross-linked acrylate copolymer include: 70-92 wt% soft monomer, 1-5 wt% divinylbenzene, 2-5 wt% epoxy acrylate, and 5-20 wt% hard monomer.
2. The composite material according to claim 1, characterized in that, The PHA copolymer is selected from one or more of poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), and poly(3-hydroxybutyrate-co-4-hydroxybutyrate).
3. The toughened high-barrier PHA composite material according to claim 1, characterized in that, The soft monomer is selected from at least one of butyl acrylate, isooctyl acrylate, and ethyl acrylate; and / or, the hard monomer is selected from at least one of methyl methacrylate, styrene, and acrylonitrile.
4. The composite material according to claim 1, characterized in that, The hydroxy acrylate is selected from at least one of hydroxyethyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl acrylate; and / or, the epoxy acrylate is selected from at least one of glycidyl acrylate and allyl glycidyl ether.
5. The composite material according to claim 1, characterized in that, The isocyanate chain extender is selected from at least one of diphenylmethane diisocyanate, toluene diisocyanate, hexamethylene diisocyanate, and dicyclohexylmethane-4,4'-diisocyanate.
6. The composite material according to claim 1, characterized in that, The catalyst is dibutyltin dilaurate or stannous octoate.
7. The composite material according to claim 1, characterized in that, The nucleating agent is sodium 4-aminophenyl phosphate.
8. The composite material according to claim 1, characterized in that, The method for preparing the hydrophobic modified filler is as follows: Amminated fillers were prepared by surface modification of sheet-like fillers with aminosilane compounds; hydrophobically modified fillers were prepared by nucleophilic addition of the aminated fillers with long-chain alkyl acrylates. The mass ratio of the sheet filler to the aminosilane coupling agent is 100:1 to 5; the molar ratio of the aminosilane coupling agent to the long-chain alkyl acrylate is 1:2 to 3.
9. The composite material according to claim 8, characterized in that, The long-chain alkyl group has 10 to 18 carbon atoms.
10. The method for preparing the composite material according to any one of claims 1 to 9, characterized in that, Includes the following steps: A mixture is prepared by mixing PHA copolymer, isocyanate chain extender, hydroxyl-containing acrylate copolymer, cross-linked acrylate copolymer, hydrophobic modified filler, catalyst, nucleating agent and other additives; The mixture is fed into a screw extruder and blended and melt-extruded at 120℃~170℃. After cooling and granulation, PHA composite material is obtained.