Method for recycling return material to produce high purity high temperature alloy

CN122648748APending Publication Date: 2026-08-28JIANGSU SINAGRT MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610476406.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-04-13
Publication Date
2026-08-28

AI Technical Summary

Technical Problem

[0006]本发明的目的在于提供一种返回料再生制备高纯高温合金的方法,以解决上述背景技术中提出的现有的技术问题

Benefits of technology

1.高效脱氧脱氮:通过“碳脱氧+钙终脱氧”的双脱氧工艺,并结合两次真空冷冻处理,能够将返回料中的氧、氮含量稳定降至10ppm以下,显著提升合金的纯净度和力学性能。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122648748A_ABST
    Figure CN122648748A_ABST
Patent Text Reader

Abstract

The application discloses a method for preparing high-purity high-temperature alloy from return material, and relates to the technical field of high-temperature alloy preparation. The method comprises the following steps: return material pretreatment, spectrum sorting, vacuum smelting, efficient deoxygenation and denitrification treatment, dynamic material supplementing and electroslag remelting. The efficient deoxygenation and denitrification treatment adopts a double deoxygenation process of carbon deoxygenation and calcium final deoxygenation, and combines twice vacuum freezing treatment to reduce the oxygen and nitrogen content to below 10 ppm. The dynamic material supplementing predicts the volatile loss of key elements based on an element burning loss model, and dynamically calculates the material supplementing amount combined with a material supplementing formula to ensure that the deviation of alloy elements is controlled within ±0.06 wt%. The application effectively solves the technical problems of high gas content and large composition fluctuation in the return material regeneration process, makes the performance of the regenerated material equivalent to that of brand-new material, and can be widely applied to the return material regeneration and utilization of high-temperature alloys such as K452 and RENE80.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-temperature alloy preparation technology, specifically a method for preparing high-purity high-temperature alloys from recycled materials. Background Technology

[0002] High-temperature alloys are core materials for high-end equipment in aerospace, energy, and other fields, possessing excellent high-temperature strength, oxidation resistance, and hot corrosion resistance. However, high-temperature alloys contain large amounts of scarce strategic metals (such as Ni, Cr, Co, W, and Mo), making them expensive. During the manufacturing process of high-temperature alloy components, a large amount of recycled material (such as risers, scrap, and chips) is generated, often accounting for 30%-60% of the total input material.

[0003] Effective recycling of these recycled materials could significantly reduce production costs and alleviate the supply-demand imbalance of strategic metal resources. However, compared to virgin materials, recycled high-temperature alloys present the following technical challenges: 1. High impurity content: The surface and interior of the recycled material contain a large amount of oxides and nitrides. 2. High gas content: The oxygen and nitrogen content is significantly higher than that of virgin materials, affecting the purity and mechanical properties of the alloy; 3. Large compositional fluctuations: The composition of different batches of recycled materials varies, making it difficult to accurately control the final alloy composition; 4. Numerous metallurgical defects: Casting defects such as porosity and shrinkage cavities exist.

[0004] Currently, traditional recycling methods for recycled materials are mostly simple remelting and refilling, which are difficult to effectively remove gases and inclusions. As a result, the performance of recycled materials cannot meet the standards of virgin materials, limiting their application in key components such as aero engines.

[0005] Therefore, developing a high-temperature alloy regeneration method that can efficiently deoxidize and denitrify and precisely control composition has significant industrial value. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing high-purity high-temperature alloys from recycled materials, so as to solve the existing technical problems mentioned in the background art.

[0007] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing high-purity high-temperature alloys from recycled materials, comprising the following steps: (1) Pretreatment of returned materials: shot blasting and surface cleaning are performed on the high-temperature alloy returned materials to remove surface impurities and oxides; (2) Spectral sorting: Spectral detection technology is used to identify and sort the pre-treated return materials, and return materials of the same grade are processed together; (3) Vacuum melting: The sorted return material is placed in a vacuum induction furnace for melting; (4) High-efficiency deoxidation and denitrification treatment: adopting a dual deoxidation and dual filtration process, combining carbon deoxidation and calcium final deoxidation, to reduce the oxygen and nitrogen content in the melt to below 10 ppm; (5) Dynamic feeding: Based on the element burn-off model, the volatilization and loss rate of key elements in the smelting process are predicted, and the amount of alloy elements to be added is dynamically calculated in combination with the feeding formula to ensure that the content deviation of each alloy element in the final melt is controlled within ±0.06wt%. (6) Electroslag remelting: The treated alloy is electroslag remelted to further purify it and obtain a high-purity high-temperature alloy ingot.

[0008] Furthermore, in step (4), the efficient deoxygenation and denitrification treatment specifically includes the following sub-steps: a. Deoxidation in the early stage of melting: Place carbon at the bottom of the crucible, accounting for 0.01%~0.015% of the weight of the returned material, evacuate to below 3Pa, and heat with a small power of 10~30kW to allow the carbon and oxygen to react fully to generate CO gas for removal; b. Melting period: After the returned material turns completely red, switch to high-power power supply until it is completely melted; c. Refining period: Evacuate to below 1 Pa, control the melt temperature at 1550℃±10℃, and refine for 10~20 minutes; d. First freezing period: Power supply is stopped, but the vacuum pump continues to work, allowing the alloy to cool and solidify naturally under vacuum. e. Final deoxidation period: After the alloy has completely solidified, it is re-energized and melted, and pure metallic calcium is added for final deoxidation. f. Second freezing period: Power is cut off after final deoxidation, allowing the alloy to solidify naturally again under high vacuum. g. Casting: After the alloy has completely solidified, re-energize and melt it, measure the temperature to 1480℃±10℃, and then cast it while energized.

[0009] Furthermore, the high-temperature alloy is either K452 alloy or RENE80 alloy.

[0010] Furthermore, in step (2), the spectral sorting is performed using a handheld laser-induced breakdown spectrometer or a direct-reading spectrometer for rapid component detection.

[0011] Furthermore, in step (3), the temperature of vacuum melting is controlled at 1450℃~1580℃, and the melting time is 2-3 hours.

[0012] Furthermore, the refining time during the refining period is adjusted according to the capacity of the vacuum induction furnace, ranging from 10 to 20 minutes.

[0013] Furthermore, in step (6), the electroslag remelting is an atmosphere-protected electroslag remelting to prevent secondary oxidation.

[0014] Furthermore, in step (1), the shot blasting time in the pretreatment of the return material is 1-3 hours.

[0015] Compared with the prior art, the beneficial effects of the present invention are: 1. High-efficiency deoxidation and denitrogenation: Through the dual deoxidation process of "carbon deoxidation + calcium final deoxidation" and combined with two vacuum freezing treatments, the oxygen and nitrogen content in the returned material can be stably reduced to below 10 ppm, which significantly improves the purity and mechanical properties of the alloy.

[0016] 2. Precise composition control: By establishing an element burn-off model and combining it with a dynamic feeding formula, the volatilization loss of alloying elements during the smelting process can be compensated in real time, so that the composition deviation of the final alloy is controlled within ±0.06wt%, solving the problem of large fluctuations in the composition of recycled materials.

[0017] 3. Intelligent sorting: Spectral sorting technology is used to quickly identify and classify returned materials, ensuring that returned materials of the same grade are processed centrally, thus avoiding compositional loss due to mixing.

[0018] 4. Performance equivalent to virgin material: Through the above comprehensive process, the high-temperature alloy prepared by recycling reaches the same level as virgin material in terms of gas content, inclusion rating, and mechanical properties, and can replace virgin material for high-end fields such as aerospace.

[0019] 5. Resource recycling: It significantly improves the utilization rate of strategic metal resources, reduces production costs, and has significant economic and social benefits. Attached Figure Description

[0020] Figure 1 This is a process flow diagram of the method of the present invention. Detailed Implementation

[0021] In the description of this invention, unless otherwise stated, "a plurality of" means two or more; the terms "upper," "lower," "left," "right," "inner," "outer," "front end," "rear end," "head," "tail," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the invention. Furthermore, the terms "first," "second," "third," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0022] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "connected" and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances. Example 1

[0023] This embodiment uses K452 alloy as an example, and employs the method of this invention to regenerate recycled materials to prepare high-purity high-temperature alloys. The specific steps are as follows: 1. Pretreatment of returned material: The K452 alloy returned material is shot blasted for 2 hours, and then the surface dust and residual steel shot are blown away with compressed air.

[0024] 2. Spectral sorting: A handheld laser-induced breakdown spectrometer is used to quickly identify and sort the components of the returned materials, ensuring that returned materials of the same grade are processed centrally.

[0025] 3. Vacuum melting: Place the sorted return material in a vacuum induction furnace, control the melting temperature at 1500℃~1550℃, and the melting time is 2.5 hours.

[0026] 4. High-efficiency deoxygenation and denitrification treatment: a. Deoxidation in the early stage of melting: Place carbon accounting for 0.012% of the weight of the returned material at the bottom of the crucible, evacuate to 2.5 Pa, and heat with a low power of 20 kW; b. Melting period: After the returned material turns completely red, switch to high-power power supply until it is completely melted; c. Refining period: Evacuate to 0.8 Pa, control the melt temperature at 1550℃, and refine for 15 minutes; d. First freezing period: Power supply is stopped, but the vacuum pump continues to work, allowing the alloy to cool and solidify naturally under vacuum. e. Final deoxidation period: After the alloy has completely solidified, it is re-energized and melted, and pure metallic calcium is added for final deoxidation; f. Second freezing period: Power is cut off after final deoxidation, allowing the alloy to solidify naturally again under high vacuum; g. Casting: After the alloy has completely solidified, re-energize and melt it, measure the temperature to 1480℃, and then cast it while energized.

[0027] 5. Dynamic Feeding: Based on the elemental burn-off model, the volatilization loss rates of Al, Ti, Cr, and Co are predicted. During the smelting process, samples are taken every 12 minutes for real-time composition analysis using direct-reading spectral analysis, and the feeding formula ΔM is applied. i =M0×(C1-C2)+L i Dynamically calculate the amount of material to be added.

[0028] 6. Electroslag remelting: A ternary slag system of CaF2-Al2O3-CaO is used, with a CaO mass fraction of 20% in the slag. The melting rate is controlled at 4 kg / min, argon gas protection is used, and the depth of the molten pool is controlled at 25 mm.

[0029] Testing revealed that the K452 high-temperature alloy prepared in this embodiment contained 7 ppm oxygen and 6 ppm nitrogen; the Al element composition deviation was +0.03 wt%, the Ti element deviation was -0.04 wt%, and the deviations of Cr and Co were all within ±0.05 wt%; the 750℃ / 300MPa creep rupture life reached 95% of that of virgin K452 material, and the inclusion rating was Class A, fine series 0.5, and Class B, fine series 1.0. Example 2

[0030] This embodiment uses RENE80 alloy as an example, and employs the method of the present invention to regenerate recycled materials to prepare high-purity high-temperature alloys. The specific steps are as follows: 1. Pretreatment of returned material: The RENE80 alloy returned material is shot blasted for 2 hours, and then the surface dust and residual steel shot are blown away with compressed air.

[0031] 2. Spectroscopic sorting: Direct-reading spectrometers are used to quickly identify and sort the components of returned materials, ensuring that returned materials of the same grade are processed centrally.

[0032] 3. Vacuum melting: Place the sorted return material in a vacuum induction furnace, control the melting temperature at 1520℃~1550℃, and the melting time is 2 hours.

[0033] 4. High-efficiency deoxygenation and denitrification treatment: The specific sub-steps are the same as in Example 1, wherein the vacuum degree during the refining period is controlled at 0.5 Pa and the refining time is 12 minutes.

[0034] 5. Dynamic feeding: Based on the element burn-off model, the volatilization loss rate of Al, Ti, Co and Mo is predicted. Samples are taken every 10 minutes during the smelting process, and the feeding amount is dynamically calculated according to the feeding formula.

[0035] 6. Electroslag remelting: A ternary slag system of CaF2-Al2O3-CaO is used, with a CaO mass fraction of 18% in the slag. The melting rate is controlled at 3.5 kg / min, and argon gas protection is used.

[0036] Testing revealed that the RENE80 high-temperature alloy prepared in this embodiment contained 8 ppm of oxygen and 7 ppm of nitrogen; the deviations in the composition of each major alloying element were all within ±0.06 wt%; and the mechanical property test results were comparable to those of a brand-new RENE80 alloy.

[0037] K452 recycled material was processed using conventional vacuum induction melting (only one refining and feeding was performed, without step-by-step deoxidation and dynamic feeding). The final alloy had an oxygen content of 25 ppm, a nitrogen content of 18 ppm, and severe loss of Al and Ti elements. The composition deviation exceeded ±0.15 wt%, some mechanical properties were unqualified, and the inclusion rating was too high.

[0038]

[0039] As shown in Table 1, the experimental data of this invention demonstrate that the process is stable and controllable, and the equipment used is all common equipment in the metallurgical industry (vacuum induction furnace, electroslag furnace, spectrometer, etc.), making it easy to achieve industrial production.

[0040] It is understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, and the present invention is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A method for preparing high-purity high-temperature alloys from recycled materials, characterized in that, Includes the following steps: (1) Pretreatment of returned materials: shot blasting and surface cleaning are performed on the high-temperature alloy returned materials to remove surface impurities and oxides; (2) Spectral sorting: Spectral detection technology is used to identify and sort the pre-treated return materials, and return materials of the same grade are processed together; (3) Vacuum melting: The sorted return material is placed in a vacuum induction furnace for melting; (4) High-efficiency deoxidation and denitrification treatment: adopting a dual deoxidation and dual filtration process, combining carbon deoxidation and calcium final deoxidation, to reduce the oxygen and nitrogen content in the melt to below 10 ppm; (5) Dynamic feeding: Based on the element burn-off model, the volatilization and loss rate of key elements in the smelting process are predicted, and the amount of alloy elements to be added is dynamically calculated in combination with the feeding formula to ensure that the content deviation of each alloy element in the final melt is controlled within ±0.06wt%. (6) Electroslag remelting: The treated alloy is electroslag remelted to further purify it and obtain a high-purity high-temperature alloy ingot.

2. The method for preparing high-purity high-temperature alloys from recycled materials according to claim 1, characterized in that: In step (4), the efficient deoxygenation and denitrification treatment specifically includes the following sub-steps: a. Deoxidation in the early stage of melting: Place carbon at the bottom of the crucible, accounting for 0.01%~0.015% of the weight of the returned material, evacuate to below 3Pa, and heat with a small power of 10~30kW to allow the carbon and oxygen to react fully to generate CO gas for removal; b. Melting period: After the returned material turns completely red, switch to high-power power supply until it is completely melted; c. Refining period: Evacuate to below 1 Pa, control the melt temperature at 1550℃±10℃, and refine for 10~20 minutes; d. First freezing period: Power supply is stopped, but the vacuum pump continues to work, allowing the alloy to cool and solidify naturally under vacuum. e. Final deoxidation period: After the alloy has completely solidified, it is re-energized and melted, and pure metallic calcium is added for final deoxidation. f. Second freezing period: Power is cut off after final deoxidation, allowing the alloy to solidify naturally again under high vacuum. g. Casting: After the alloy has completely solidified, it is re-energized and melted, and the temperature is measured to 1480℃±10℃ before casting.

3. The method for preparing high-purity high-temperature alloys from recycled materials according to claim 1, characterized in that: In step (5), the amount of material replenished in the dynamic replenishment is calculated according to the following formula: ΔM i =M0×(C1-C2)+L i Where, ΔM i M0 is the amount of element i added, C1 is the target composition, C2 is the measured composition during the smelting process, and L is the total mass of the melt. i Let represent the loss of element i as predicted by the burn-off model.

4. The method for preparing high-purity high-temperature alloys from recycled materials according to claim 1, characterized in that: The high-temperature alloy is either K452 alloy or RENE80 alloy.

5. The method for preparing high-purity high-temperature alloys from recycled materials according to claim 1, characterized in that: In step (2), the spectral sorting is performed using a handheld laser-induced breakdown spectrometer or a direct-reading spectrometer for rapid component detection.

6. The method for preparing high-purity high-temperature alloys from recycled materials according to claim 1, characterized in that: In step (3), the temperature of vacuum melting is controlled at 1450℃~1580℃, and the melting time is 2-3 hours.

7. The method for preparing high-purity high-temperature alloys from recycled materials according to claim 2, characterized in that: The refining time during the refining period is adjusted according to the capacity of the vacuum induction furnace, ranging from 10 to 20 minutes.

8. The method for preparing high-purity high-temperature alloys from recycled materials according to claim 1, characterized in that: In step (6), electroslag remelting is atmospheric protective electroslag remelting to prevent secondary oxidation.

9. The method for preparing high-purity high-temperature alloys from recycled materials according to claim 1, characterized in that: In step (1), the shot blasting process in the pretreatment of the returned material takes 1-3 hours.

10. The method according to any one of claims 1 to 9, characterized in that, The high-purity high-temperature alloy prepared by the method has an oxygen content and a nitrogen content of less than 10 ppm, and the deviation of the main alloying element composition is controlled within ±0.06 wt%.