A method for preventing cracking of a martensitic heat-resistant steel cast blank by heat treatment

By employing a multi-stage temperature and speed controlled heat treatment process, the cracking problem of martensitic heat-resistant steel electrode billets and electroslag ingots during long-term storage or transportation at room temperature was solved, achieving a stable transformation of the billet structure and the release of internal stress, thus avoiding the occurrence of cracking.

CN123063587APending Publication Date: 2026-11-10CHINA FIRST HEAVY IND +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611473545.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

How to effectively prevent cracking of martensitic heat-resistant steel electrode billets and electroslag ingots during long-term storage or transportation at room temperature.

Method used

A multi-stage temperature and rate controlled heat treatment process is adopted, including holding at 450℃ to 550℃, then cooling to 150℃ to 250℃ at a slow first cooling rate and holding at that temperature, then heating to 600℃ to 750℃ at a rate not exceeding 30℃/h and holding at that temperature, and then cooling to no higher than 250℃ at a second cooling rate before being removed from the furnace and air-cooled. This ensures that the microstructure of the billet changes from unstable coarse martensite to stable tempered sorbite, releasing internal stress.

Benefits of technology

This method significantly reduces the risk of cracking in martensitic heat-resistant steel electrode billets and electroslag ingots during long-term storage or transportation at room temperature, ensuring the stability and integrity of the billet structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063587A_ABST
    Figure CN123063587A_ABST
Patent Text Reader

Abstract

The application provides a crack-proof heat treatment method for a martensitic heat-resistant steel casting blank, and relates to the technical field of metal material heat treatment.The heat treatment method comprises the following steps: keeping the casting blank after demoulding at 450-550 DEG C for a first time, then furnace cooling to 150-250 DEG C at a first cooling rate, and keeping at 150-250 DEG C for 10-20 hours; then heating to 600-750 DEG C at a preset heating rate, keeping for a second time; then furnace cooling to not higher than 250 DEG C at a second cooling rate, and air cooling to room temperature after discharging to obtain a heat-treated casting blank; wherein the temperature of the high-temperature side of the casting blank after demoulding is 500-650 DEG C; the casting blank is an electrode blank or an electroslag ingot, and the preset heating rate is not higher than 30 DEG C / h.The method can effectively avoid the cracking of the martensitic heat-resistant steel electrode blank and electroslag ingot during long-time storage at room temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of heat treatment technology for metallic materials, and more specifically, to a method for preventing cracking in martensitic heat-resistant steel billets. Background Technology

[0002] Martensitic heat-resistant steel rotor forgings for supercritical and higher-level generator sets have high alloy content, making them prone to segregation of alloying elements during solidification. To reduce macroscopic and microscopic segregation during solidification and to meet the extremely stringent performance requirements of standard forgings in rotor forging production, these steel ingots are typically smelted using electroslag remelting.

[0003] However, the electroslag remelting process has its unique characteristics. Before remelting the electroslag ingot, an electrode blank must first be vacuum-cast. To ensure the internal metallurgical quality of the electroslag ingot, reduce defects, and facilitate welding of the electrode blank, the electrode blank needs to be processed. This means that the electrode blank needs to be kept at room temperature for a relatively long time and must have good machinability. However, the directly cast electrode blank has a coarse martensitic as-cast structure, which is very prone to cracking if kept at room temperature for a long time.

[0004] Furthermore, to ensure efficient production, electroslag ingots need to be stockpiled in advance or sold directly and transported over long distances. After remelting and demolding, electroslag ingots also need to be stored or transported at room temperature for extended periods. The non-equilibrium as-cast martensite structure formed after remelting is highly prone to cracking when stored at room temperature for a long time.

[0005] In summary, how to effectively prevent cracking of martensitic heat-resistant steel electrode billets and electroslag ingots during long-term storage at room temperature has become a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0006] The problem solved by this invention is: how to effectively prevent cracking of martensitic heat-resistant steel electrode blanks and electroslag ingots during long-term storage at room temperature.

[0007] To address the above problems, this invention provides a crack-resistant heat treatment method for martensitic heat-resistant steel billets, comprising: After demolding, the billet is held at 450℃ to 550℃ for a first time, then furnace cooled to 150℃ to 250℃ at a first cooling rate, and held at 150℃ to 250℃ for 10h to 20h. Then, raise the temperature to 600℃ to 750℃ at the preset heating rate and hold it for a second time. Then, furnace cool to no more than 250°C at a second cooling rate, remove from the furnace and air cool to room temperature to obtain the heat-treated billet; The high-temperature side temperature of the cast billet after demolding is 500°C to 650°C; the cast billet is an electrode billet or an electroslag ingot; and the preset heating rate is no more than 30°C / h.

[0008] Optionally, the preset heating rate is 20℃ / h to 30℃ / h.

[0009] Optionally, the first cooling rate is no greater than 20°C / h.

[0010] Optionally, the second cooling rate is no greater than 20°C / h.

[0011] Optionally, the first time t1 is (1 to 2)d / 100, where d is the diameter of the billet.

[0012] Optionally, the second time t2 is (2 to 4)d / 100, where d is the diameter of the billet.

[0013] Optionally, the diameter of the cast billet is 800 mm to 1300 mm.

[0014] Optionally, the height of the cast billet is 3000 mm to 4500 mm.

[0015] Optionally, the chemical composition of the martensitic heat-resistant steel includes: C: 0.10% to 0.16%, Si: ≤0.12%, Mn: 0.37% to 0.53%, Cr: 10.05% to 11.65%, Mo: 0.98% to 1.15%, Ni: 0.60% to 0.85%, V: 0.14% to 0.26%, N: 0.050% to 0.085%, W: 0.10% to 1.10%, Nb: 0.035% to 0.065%, Cu: ≤0.17%, S: ≤0.007%, P: ≤0.012%, with the balance being Fe and unavoidable impurities.

[0016] Optionally, the chemical composition of the martensitic heat-resistant steel includes: C: 0.12% to 0.16%, Si: ≤0.12%, Mn: 0.30% to 0.50%, Cr: 9.05% to 9.65%, Mo: 1.4% to 1.6%, Co: 1.10% to 1.30%, Ni: 0.10% to 0.25%, V: 0.15% to 0.26%, N: 0.015% to 0.035%, B: 0.0080% to 0.0110%, Nb: 0.035% to 0.065%, Cu: ≤0.15%, S: ≤0.007%, P: ≤0.012%, with the balance being Fe and unavoidable impurities.

[0017] Compared with related technologies, the method of this invention can effectively avoid cracking of martensitic heat-resistant steel electrode billets and electroslag ingots stored at room temperature for extended periods. The specific principle is as follows: After demolding, the high-temperature side of the billet is 500°C to 650°C, while the low-temperature side is approximately 250°C to 350°C, resulting in a significant axial temperature difference. If directly cooled to room temperature, huge structural stress will be generated between the martensitic transformation already occurring on the low-temperature side and the untransformed structure on the high-temperature side, easily leading to cracking. This invention, by holding the billet at 450°C to 550°C for the first time, can homogenize the overall temperature of the billet, eliminate the initial temperature difference, and prevent the low-temperature side from bearing excessive stress in the coarse martensitic state. Subsequently, it is slowly furnace-cooled at a first cooling rate to 150°C to 250°C and held for 10 to 20 hours, allowing the billet to complete the martensitic transformation at a controllable rate, avoiding the internal and external temperature differences and structural stress concentration caused by rapid cooling, and reducing the risk of phase transformation cracking. The temperature is then increased to 600℃ to 750℃ at a preset heating rate of no more than 30℃ / h. Within the elastic deformation zone of the billet, the internal and external temperature differences and instantaneous internal stress are minimized. This allows the supersaturated martensite to decompose uniformly with increasing temperature, carbides to precipitate slowly, and the billet to gradually transform into a balanced tempered sorbite structure, significantly reducing structural stress. During the second holding period at 600℃ to 750℃, the overall martensite of the billet is fully tempered into a stable tempered sorbite structure, while the retained austenite is fully decomposed into a balanced ferrite and carbide structure, further eliminating structural instability and internal stress. Finally, the billet is slowly furnace-cooled at a second cooling rate to no higher than 250℃ before being air-cooled. This ensures that the billet maintains a small internal and external temperature difference and thermal stress throughout the cooling process, avoiding the risk of new cracking during the cooling stage. Through the above-mentioned multi-stage temperature and speed controlled heat treatment process, the billet structure is transformed from unstable coarse martensite to stable tempered sorbite, and the internal stress is fully released, thereby effectively avoiding the cracking problem of electrode billets and electroslag ingots during long-term storage or transportation at room temperature. Attached Figure Description

[0018] Figure 1 This is an image of the heat-treated electrode blank prepared in Example 1 of the present invention, which was stored at room temperature for 6 days and then welded to a dummy electrode. Figure 2 This is an image of the heat-treated electrode blank obtained in Example 2 of the present invention after being stored at room temperature for 6 days; Figure 3 This is a picture of the heat-treated electroslag ingot prepared in Example 3 of the present invention after being stored at room temperature for 10 days; Figure 4 This is a picture of the heat-treated electrode blank obtained in Comparative Example 1 of the present invention; Figure 5 This is a picture of the heat-treated electrode blank prepared in Comparative Example 2 of the present invention after being stored at room temperature for 5 days; Figure 6This is a picture of the electroslag ingot prepared in Comparative Example 3 of the present invention after heat treatment, stored at room temperature for 5 days. Detailed Implementation

[0019] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Although some embodiments of the present invention are shown in the drawings, it should be understood that the present invention can be implemented in various forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the accompanying drawings and embodiments of the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention.

[0020] Unless otherwise defined, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.

[0021] The term "comprising" and its variations as used herein are open-ended, meaning "including but not limited to"; the term "based on" means "at least partially based on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one additional embodiment"; the term "some embodiments" means "at least some embodiments"; and the term "optionally" means "optional embodiments". Definitions of other terms will be given in the following description. It should be noted that the concepts of "first," "second," etc., mentioned in this invention are used to distinguish different objects, not to describe a specific order or hierarchy. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined with "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, unless otherwise stated, "a plurality of" means two or more.

[0022] It should be noted that, in this invention, for the electrode billet, the low-temperature side of the cast billet after demolding is the sprue side of the electrode billet, and the high-temperature side of the cast billet after demolding is the riser side of the electrode billet; for the electroslag ingot, the low-temperature side of the cast billet after demolding is the arc-starting end of the electroslag ingot, and the high-temperature side of the cast billet after demolding is the feeding end of the electroslag ingot.

[0023] This invention provides a method for preventing cracking in martensitic heat-resistant steel billets, comprising: After demolding, the billet is held at 450℃ to 550℃ for a first time, then furnace cooled to 150℃ to 250℃ at a first cooling rate, and held at 150℃ to 250℃ for 10h to 20h. Then, raise the temperature to 600℃ to 750℃ at the preset heating rate and hold it for a second time. Then, furnace cool to no more than 250°C at a second cooling rate, remove from the furnace and air cool to room temperature to obtain the heat-treated billet; The high-temperature side temperature of the cast billet after demolding is 500°C to 650°C; the cast billet is an electrode billet or an electroslag ingot; and the preset heating rate is no more than 30°C / h.

[0024] The method described in this invention effectively prevents cracking of martensitic heat-resistant steel electrode billets and electroslag ingots during prolonged storage at room temperature. The specific principle is as follows: After demolding, the high-temperature side of the billet reaches 500°C to 650°C, while the low-temperature side reaches approximately 250°C to 350°C, resulting in a significant axial temperature difference. Direct cooling to room temperature would create significant structural stress between the martensitic transformation already occurring on the low-temperature side and the untransformed structure on the high-temperature side, easily leading to cracking. This invention, by holding the billet at 450°C to 550°C for the first time, homogenizes the overall temperature of the billet, eliminates the initial temperature difference, and prevents the low-temperature side from bearing excessive stress in the coarse martensitic state. Subsequently, a slow furnace cooling to 150°C to 250°C at a first cooling rate and holding for 10 to 20 hours allows the billet to complete the martensitic transformation at a controllable rate, avoiding internal and external temperature differences and structural stress concentration caused by rapid cooling, thus reducing the risk of phase transformation cracking. The temperature is then increased to 600℃ to 750℃ at a preset heating rate of no more than 30℃ / h. Within the elastic deformation zone of the billet, the internal and external temperature differences and instantaneous internal stress are minimized. This allows the supersaturated martensite to decompose uniformly with increasing temperature, carbides to precipitate slowly, and the billet to gradually transform into a balanced tempered sorbite structure, significantly reducing structural stress. During the second holding period at 600℃ to 750℃, the overall martensite of the billet is fully tempered into a stable tempered sorbite structure, while the retained austenite is fully decomposed into a balanced ferrite and carbide structure, further eliminating structural instability and internal stress. Finally, the billet is slowly furnace-cooled at a second cooling rate to no higher than 250℃ before being air-cooled. This ensures that the billet maintains a small internal and external temperature difference and thermal stress throughout the cooling process, avoiding the risk of new cracking during the cooling stage. Through the above-mentioned multi-stage temperature and speed controlled heat treatment process, the billet structure is transformed from unstable coarse martensite to stable tempered sorbite, and the internal stress is fully released, thereby effectively avoiding the cracking problem of electrode billets and electroslag ingots during long-term storage or transportation at room temperature.

[0025] In some embodiments of the present invention, the preset heating rate is 20℃ / h to 30℃ / h. Compared to heating rates greater than 30℃ / h, this embodiment further limits the upper limit of the heating rate, resulting in a smaller internal and external temperature difference and lower thermal stress in the cast billet during the heating process. This effectively avoids local overheating and crack initiation caused by excessively rapid heating, while also taking into account production efficiency and ensuring that the martensite structure decomposes smoothly into tempered sorbite within the elastic deformation zone.

[0026] In some embodiments of the present invention, the first cooling rate is no greater than 20°C / h. In this embodiment, controlling the first cooling rate to no greater than 20°C / h ensures that during the process of cooling from 450°C to 550°C to 150°C to 250°C, the entire billet completes the martensitic phase transformation at a sufficiently slow rate, avoiding a sharp increase in the internal and external temperature difference and stress concentration in the structure caused by excessively rapid cooling, thereby significantly reducing the risk of phase transformation cracking.

[0027] In some embodiments of the present invention, the second cooling rate is no greater than 20°C / h. In this embodiment, during the cooling stage after tempering and holding, the cooling rate is controlled to be no greater than 20°C / h, so that the billet is slowly furnace cooled from 600°C to 750°C to no higher than 250°C. This avoids the generation of new thermal stress and structural stress due to excessively rapid cooling, ensures that the already formed stable tempered sorbite structure is not damaged, and prevents delayed cracking during the cooling process.

[0028] In some embodiments of the present invention, the first time t1 is (1 to 2)d / 100, where t1 is in hours (h) and d is the diameter of the billet in mm. In this embodiment, the first-step holding time is dynamically adjusted according to the billet diameter to ensure that billets of different sizes have sufficient time to achieve temperature homogenization, eliminate the initial axial temperature difference, avoid excessive stress on the low-temperature side in the coarse martensite state, and avoid efficiency reduction due to excessively long holding time.

[0029] In some embodiments of the present invention, the second time t2 is (2 to 4)d / 100, where t2 is in hours (h) and d is the diameter of the billet in mm. In this embodiment, the tempering holding time is dynamically adjusted according to the billet diameter to ensure that the core of the large-section billet can also fully complete the transformation of martensite to tempered sorbite and the decomposition of residual austenite, thus completely eliminating structural instability and internal stress, while avoiding uneven performance due to insufficient holding or energy waste due to excessive holding.

[0030] In some embodiments of the present invention, the diameter of the cast billet is 800 mm to 1300 mm, and the height of the cast billet is 3000 mm to 4500 mm.

[0031] In some embodiments of the present invention, the chemical composition of the martensitic heat-resistant steel, exemplarily, comprises: C: 0.10% to 0.16%, Si: ≤0.12%, Mn: 0.37% to 0.53%, Cr: 10.05% to 11.65%, Mo: 0.98% to 1.15%, Ni: 0.60% to 0.85%, V: 0.14% to 0.26%, N: 0.050% to 0.085%, W: 0.10% to 1.10%, Nb: 0.035% to 0.065%, Cu: ≤0.17%, S: ≤0.007%, P: ≤0.012%, with the balance being Fe and unavoidable impurities.

[0032] In some embodiments of the present invention, the chemical composition of the martensitic heat-resistant steel, exemplarily, comprises: C: 0.12% to 0.16%, Si: ≤0.12%, Mn: 0.30% to 0.50%, Cr: 9.05% to 9.65%, Mo: 1.4% to 1.6%, Co: 1.10% to 1.30%, Ni: 0.10% to 0.25%, V: 0.15% to 0.26%, N: 0.015% to 0.035%, B: 0.0080% to 0.0110%, Nb: 0.035% to 0.065%, Cu: ≤0.15%, S: ≤0.007%, P: ≤0.012%, with the balance being Fe and unavoidable impurities.

[0033] The present invention will be further described below with reference to specific embodiments.

[0034] Example 1 The demolded electrode blank is held at 500℃ for a first time, then furnace cooled to 200℃ at a first cooling rate, and held at 200℃ for 10 hours; wherein, the first cooling rate is 12℃ / h; the first time is 8 hours; the diameter of the electrode blank is 800mm and the height is 3000mm; the high-temperature side temperature of the demolded electrode blank is 600℃; the chemical composition of the electrode blank includes: C: 0.13%, Si: 0.006%, Mn: 0.42%, Cr: 10.65%, Mo: 1.05%, Ni: 0.75%, V: 0.16%, N: 0.058%, W: 0.40%, Nb: 0.040%, Cu: 0.05%, S: 0.003%, P: 0.003%, with the balance being Fe and unavoidable impurities.

[0035] Then, the temperature is increased to 650°C at a preset heating rate and held for a second time; wherein, the preset heating rate is 28°C / h; and the second time t2 is 20h.

[0036] The furnace is then cooled to 250°C at a second cooling rate, and then air-cooled to room temperature to obtain the heat-treated electrode blank; wherein, the second cooling rate is 15°C / h.

[0037] Images of the heat-treated electrode blank prepared in Example 1, after being stored at room temperature for 6 days, and then welded to a dummy electrode, are shown below. Figure 1 As shown, from Figure 1 It can be seen that the electrode blank did not show any cracking.

[0038] Example 2 The demolded electrode blank is held at 550℃ for a first time, then furnace cooled to 250℃ at a first cooling rate, and held at 250℃ for 15 hours; wherein, the first cooling rate is 10℃ / h; the first time is 15 hours; the diameter of the electrode blank is 1300mm and the height is 4500mm; the high-temperature side temperature of the demolded electrode blank is 650℃; the chemical composition of the electrode blank includes: C: 0.13%, Si: 0.006%, Mn: 0.42%, Cr: 10.65%, Mo: 1.05%, Ni: 0.75%, V: 0.16%, N: 0.058%, W: 0.40%, Nb: 0.040%, Cu: 0.05%, S: 0.003%, P: 0.003%, with the balance being Fe and unavoidable impurities.

[0039] Then, the temperature is increased to 680℃ at a preset heating rate and held for a second time; wherein, the preset heating rate is 20℃ / h; and the second time t2 is 35h.

[0040] The furnace is then cooled to 250°C at a second cooling rate, and then air-cooled to room temperature to obtain the heat-treated electrode blank; wherein, the second cooling rate is 12°C / h.

[0041] Images of the heat-treated electrode blank prepared in Example 2 after being stored at room temperature for 6 days, as shown. Figure 2 As shown, from Figure 2 It can be seen that the electrode blank did not show any cracking.

[0042] Example 3 The demolded electroslag ingot is held at 450℃ for a first time, then furnace cooled to 250℃ at a first cooling rate, and held at 250℃ for 15 hours; wherein, the first cooling rate is 10℃ / h; the first time is 15 hours; the diameter of the electroslag ingot is 1300mm and the height is 4500mm; the high-temperature side temperature of the demolded electroslag ingot is 600℃; the chemical composition of the electroslag ingot includes: C: 0.14%, Si: 0.06%, Mn: 0.39%, Cr: 9.55%, Mo: 1.45%, Co: 1.18%, Ni: 0.22%, V: 0.19%, N: 0.017%, B: 0.0085%, Nb: 0.04%, Cu: 0.05%, S: 0.002%, P: 0.008%, with the balance being Fe and unavoidable impurities.

[0043] Then, the temperature is increased to 680℃ at a preset heating rate and held for a second time; wherein, the preset heating rate is 20℃ / h; and the second time t2 is 35h.

[0044] The furnace is then cooled to 250°C at a second cooling rate, and then air-cooled to room temperature to obtain the heat-treated electroslag ingot; wherein, the second cooling rate is 15°C / h.

[0045] The image shows the heat-treated electroslag ingot prepared in Example 3 after being stored at room temperature for 10 days, as shown. Figure 3 As shown, from Figure 3 It can be seen that the electroslag ingot did not show any cracking.

[0046] Comparative Example 1 The difference from Example 1 is that the preset heating rate is 50°C / h.

[0047] The heat-treated electrode blank obtained in Comparative Example 1 is as follows: Figure 4 As shown, from Figure 4 It can be seen that the electrode blank cracked directly without being preserved.

[0048] Comparative Example 2 The demolded electrode blank is held at 500℃ for a first time, and then furnace cooled to 300℃ at a first cooling rate; wherein, the first cooling rate is 12℃ / h; the first time is 8h; the diameter of the electrode blank is 800mm and the height is 3000mm; the high-temperature side temperature of the demolded electrode blank is 600℃; the chemical composition of the electrode blank includes: C: 0.13%, Si: 0.006%, Mn: 0.42%, Cr: 10.65%, Mo: 1.05%, Ni: 0.75%, V: 0.16%, N: 0.058%, W: 0.40%, Nb: 0.040%, Cu: 0.05%, S: 0.003%, P: 0.003%, with the balance being Fe and unavoidable impurities.

[0049] Then, the temperature is increased to 650°C at a preset heating rate and held for a second time; wherein, the preset heating rate is 28°C / h; and the second time t2 is 20h.

[0050] The furnace is then cooled to 250°C at a second cooling rate, and then air-cooled to room temperature to obtain the heat-treated electrode blank; wherein, the second cooling rate is 15°C / h.

[0051] The image shows the heat-treated electrode blank prepared in Comparative Example 2 after being stored at room temperature for 5 days, as shown. Figure 5 As shown, from Figure 5 It can be seen that the electrode blank has cracked.

[0052] Comparative Example 3 The demolded electroslag ingot is held at 450℃ for a first time, then furnace cooled to 250℃ at a first cooling rate, and held at 250℃ for 15 hours. It is then air-cooled to room temperature to obtain the heat-treated electroslag ingot. The first cooling rate is 10℃ / h; the first time is 15 hours; the diameter of the electroslag ingot is 1300mm and the height is 4500mm; the high-temperature side temperature of the demolded electroslag ingot is 600℃; the chemical composition of the electroslag ingot includes: C: 0.14%, Si: 0.06%, Mn: 0.39%, Cr: 9.55%, Mo: 1.45%, Co: 1.18%, Ni: 0.22%, V: 0.19%, N: 0.017%, B: 0.0085%, Nb: 0.04%, Cu: 0.05%, S: 0.002%, P: 0.008%, with the balance being Fe and unavoidable impurities.

[0053] The image shows the heat-treated electroslag ingot prepared in Comparative Example 3 after being stored at room temperature for 5 days, as shown. Figure 6 As shown, from Figure 6 It can be seen that the electroslag ingot has cracked.

[0054] While the present invention has been disclosed above, its scope of protection is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention, and all such changes and modifications will fall within the scope of protection of the present invention.

Claims

1. A method for preventing cracking in martensitic heat-resistant steel billets, characterized in that, include: After demolding, the billet is held at 450℃ to 550℃ for a first time, then furnace cooled to 150℃ to 250℃ at a first cooling rate, and held at 150℃ to 250℃ for 10h to 20h. Then, raise the temperature to 600℃ to 750℃ at the preset heating rate and hold it for a second time. Then, furnace cool to no more than 250°C at a second cooling rate, remove from the furnace and air cool to room temperature to obtain the heat-treated billet; The high-temperature side temperature of the cast billet after demolding is 500°C to 650°C; the cast billet is an electrode billet or an electroslag ingot; and the preset heating rate is no more than 30°C / h.

2. The anti-cracking heat treatment method for martensitic heat-resistant steel billets according to claim 1, characterized in that, The preset heating rate is 20℃ / h to 30℃ / h.

3. The anti-cracking heat treatment method for martensitic heat-resistant steel billets according to claim 1, characterized in that, The first cooling rate is no greater than 20℃ / h.

4. The anti-cracking heat treatment method for martensitic heat-resistant steel billets according to claim 1, characterized in that, The second cooling rate is no greater than 20℃ / h.

5. The anti-cracking heat treatment method for martensitic heat-resistant steel billets according to claim 1, characterized in that, The first time t1 is (1 to 2)d / 100, where d is the diameter of the billet.

6. The anti-cracking heat treatment method for martensitic heat-resistant steel billets according to claim 1, characterized in that, The second time t2 is (2 to 4)d / 100, where d is the diameter of the billet.

7. The anti-cracking heat treatment method for martensitic heat-resistant steel billets according to claim 1, characterized in that, The diameter of the cast billet is 800 mm to 1300 mm.

8. The anti-cracking heat treatment method for martensitic heat-resistant steel billets according to claim 1, characterized in that, The height of the cast billet is 3000mm to 4500mm.

9. The anti-cracking heat treatment method for martensitic heat-resistant steel billets according to claim 1, characterized in that, The chemical composition of the martensitic heat-resistant steel includes: C: 0.10% to 0.16%, Si: ≤0.12%, Mn: 0.37% to 0.53%, Cr: 10.05% to 11.65%, Mo: 0.98% to 1.15%, Ni: 0.60% to 0.85%, V: 0.14% to 0.26%, N: 0.050% to 0.085%, W: 0.10% to 1.10%, Nb: 0.035% to 0.065%, Cu: ≤0.17%, S: ≤0.007%, P: ≤0.012%, with the balance being Fe and unavoidable impurities.

10. The anti-cracking heat treatment method for martensitic heat-resistant steel billets according to claim 1, characterized in that, The chemical composition of the martensitic heat-resistant steel includes: C: 0.12% to 0.16%, Si: ≤0.12%, Mn: 0.30% to 0.50%, Cr: 9.05% to 9.65%, Mo: 1.4% to 1.6%, Co: 1.10% to 1.30%, Ni: 0.10% to 0.25%, V: 0.15% to 0.26%, N: 0.015% to 0.035%, B: 0.0080% to 0.0110%, Nb: 0.035% to 0.065%, Cu: ≤0.15%, S: ≤0.007%, P: ≤0.012%, with the balance being Fe and unavoidable impurities.