Boron-nitrogen co-doped carbon nanotube-graphene composite fibers, their preparation methods, and cables

By using a boron-nitrogen co-doped carbon nanotube-graphene composite fiber preparation method, the problems of excessive self-weight, insufficient conductivity, and poor torsional fatigue resistance of wind turbine tower cables have been solved, achieving improved conductivity, extended torsional life, and reduced conductivity attenuation, thus meeting the requirements for on-site use of wind turbines.

CN123063897APending Publication Date: 2026-11-10GUIYANG ZHONGAN TECHNOLOGY GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611094492.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-22
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing wind turbine tower cable conductors suffer from excessive weight, insufficient conductivity, poor torsional fatigue resistance, and severe conductivity attenuation during long-term use. In particular, they cannot simultaneously meet the requirements of lightweight, high torsional fatigue resistance, and ultra-low conductivity attenuation under ±360° reciprocating torsion and harsh outdoor environments.

Method used

Boron-nitrogen co-doped carbon nanotube-graphene composite fibers are used to simultaneously grow carbon nanotubes and graphene sheets through floating catalytic chemical vapor deposition. Boron and nitrogen atoms are embedded in the carbon nanotube lattice to form CB and CN covalent bonds. Combined with gradient magnetic field orientation and plasma activation treatment, a stable covalent gradient interface coupling layer is formed, which improves conductivity and enhances torsional fatigue resistance.

Benefits of technology

It achieves a 35% increase in conductivity, a 150% increase in torsional life, a reduction of an order of magnitude in conductivity attenuation, and a reduction of approximately 59% in overall cable weight, significantly reducing tower and nacelle loads and significantly improving torsional fatigue resistance, meeting the cumulative usage requirements of wind turbine sites for 20 years.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063897A_ABST
    Figure CN123063897A_ABST
Patent Text Reader

Abstract

This invention discloses a boron-nitrogen co-doped carbon nanotube-graphene composite fiber, its preparation method, and a cable. The composite fiber comprises carbon nanotubes and graphene sheets. Boron and nitrogen atoms are embedded in the lattice of the carbon nanotubes, and the tube walls have C-B and / or C-N covalent bonds. The graphene sheets are connected to the carbon nanotube walls through C-B-C and / or C-N-C covalent bonds. The preparation method employs floating catalytic chemical vapor deposition, simultaneously introducing a first carbon source, a second carbon source, a boron source, and a nitrogen source into the reaction system to simultaneously perform carbon nanotube growth, graphene sheet growth, and boron-nitrogen lattice doping. The composite fiber has a density 1 / 5 that of copper, a conductivity of 62% IACS, and a thermal cycling decay of ≤1.2% after 2000 hours. This invention also provides an anti-torsion tower cable for large onshore wind turbines containing this composite fiber, with a ±360° torsional life >30,000 cycles, meeting the requirement of 20 years of maintenance-free operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of carbon nanocomposite materials technology, specifically to a boron-nitrogen co-doped carbon nanotube-graphene composite fiber, its preparation method and application, and an anti-torsion tower cable for large onshore wind turbines containing the composite fiber. Background Technology

[0002] Wind turbine tower cables are a key component of wind turbine generators. Their conductors must continuously carry large currents during the ±360° reciprocating oscillation of the nacelle, while also withstanding the suspension stress generated by the cable's own weight and outdoor temperature cycling. Existing wind turbine tower cable conductors have the following inherent defects: (a) Inherent defects of metallic conductors Existing wind turbine tower cables generally use copper conductors, with a copper density of 8.9 g / cm³. A 100-meter-long cable has an extremely heavy self-weight, causing sag and increasing the load on the tower and nacelle. More critically, copper conductors are highly susceptible to metal fatigue fracture during the repeated ±360° oscillation of the wind turbine nacelle, a major cause of cable failure. While aluminum alloy conductors offer some weight reduction, their conductivity, tensile strength, and torsional fatigue resistance are insufficient. Long-term torsion can easily lead to metal cracks, resulting in poor reliability in actual operation.

[0003] (II) Limitations of existing carbon nanotube / graphene composite materials With the development of carbon nanomaterials, the industry is attempting to use carbon nanotube fibers in cable conductors. However, existing technologies have the following inherent drawbacks: Lack of synergistic doping mechanism: Existing composite fibers either rely solely on a single carbon source for growth or employ stepwise doping processes, failing to achieve in-situ integration of boron-nitrogen synergistic doping with graphene intercalation at the lattice level. Simple graphene intercalation relies solely on van der Waals forces for physical bonding, resulting in severe tube slippage and a sharp increase in contact resistance after repeated large-angle torsion.

[0004] Dopant loss and attenuation: The process of improving conductivity by using only external surface doping such as iodine and ferric chloride is prone to volatilization and loss when heated and cycled, and the conductivity of the cable continues to decrease over long-term operation.

[0005] Interface debonding failure: There are no stable active covalent sites on the surface of carbon nanotubes. They rely solely on physical adhesion through plasma and silane coupling agents. After long-term torsion, the insulating layer is prone to delamination.

[0006] The service conditions for cables on large onshore wind turbine towers are extremely harsh: the nacelle undergoes continuous ±360° reciprocating torsion, with an average of over 10,000 torsion cycles per year; the tower height exceeds 100 meters, and the suspension stress generated by the cable's own weight significantly increases the load on the tower top; outdoor temperature differences and current thermal effects lead to long-term thermal cycling. These operating conditions place combined requirements on the conductor for "lightweight, high resistance to torsional fatigue, and ultra-low conductivity attenuation," which cannot be simultaneously met by copper, aluminum alloys, or conventional carbon nanotube fibers.

[0007] In existing technologies, the conventional approach to addressing the insufficient conductivity of carbon nanomaterials is to use exogenous surface dopants such as iodine and ferric chloride for charge transfer doping. However, this approach introduces new problems such as dopant volatilization and loss during long-term thermal cycling, leading to a continuous decline in conductivity. Furthermore, it is well known in the art that boron-nitrogen co-doping transforms metallic carbon nanotubes into semiconducting carbon nanotubes, thereby reducing conductivity. Therefore, those skilled in the art, when faced with the specific problem of "low conductivity decline under long-term thermal cycling conditions in wind turbine towers" addressed by this invention, would not naturally think of adopting the "lattice intrinsic doping" scheme proposed in this invention. Summary of the Invention

[0008] This invention aims to solve the following technical problems: how to provide a boron-nitrogen co-doped carbon nanotube-graphene composite fiber that simultaneously meets the requirements of "lightweight, high torsional fatigue resistance, and ultra-low conductivity attenuation", its preparation method, and an anti-torsion stranded tower cable for large onshore wind turbines using this composite fiber.

[0009] To achieve the above-mentioned objectives, this invention provides a boron-nitrogen co-doped carbon nanotube-graphene composite fiber, comprising carbon nanotubes and graphene sheets. Boron atoms and nitrogen atoms are embedded in the lattice of the carbon nanotubes, and the walls of the carbon nanotubes have CB and / or CN covalent bonds. The graphene sheets are connected to the walls of the carbon nanotubes through CBC and / or CNC covalent bonds.

[0010] Preferably, the molar ratio of boron atoms to nitrogen atoms is 1.5:1 to 2.5:1; more preferably, it is 2:1.

[0011] Preferably, the composite fiber has a density of 1.7-1.85 g / cm³, a conductivity of 52%-59% IACS, and a tensile strength of 1.8-2.2 GPa.

[0012] This invention also provides a method for preparing boron-nitrogen co-doped carbon nanotube-graphene composite fibers, comprising the following steps: A floating catalytic chemical vapor deposition method was used to simultaneously introduce a first carbon source, a second carbon source, a boron source, and a nitrogen source into the reaction system, and simultaneously carry out carbon nanotube growth, graphene sheet growth, and boron-nitrogen lattice doping at a temperature of 1000-1300℃. The first carbon source is pyrolyzed to generate carbon nanotubes, and the second carbon source is pyrolyzed to generate graphene sheets; The boron and nitrogen atoms generated by the cracking of the boron and nitrogen sources are embedded in the hexagonal lattice of the carbon nanotubes to form CB and / or CN covalent bonds. The graphene sheets are covalently bonded to the walls of the carbon nanotubes via CB and / or CN bonds, forming CBC and / or CNC bonds.

[0013] Preferably, the first carbon source is ethanol, the second carbon source is ethylene glycol, the reaction temperature is 1200℃, and the molar ratio of the boron source to the nitrogen source is 2:1.

[0014] Preferably, the method further includes subjecting the composite aerogel generated by pyrolysis to orientation treatment by sequentially passing it through a first gradient axial magnetic field of 0.3-0.7T and a second gradient axial magnetic field of 0.8-1.2T; more preferably, the intensity of the first gradient axial magnetic field is 0.5T and the intensity of the second gradient axial magnetic field is 1.0T.

[0015] Preferably, the process further includes subjecting the composite fibers to ethanol vapor pre-densification treatment and acetone vapor bath secondary densification treatment in sequence.

[0016] The present invention also provides an anti-torsion stranded tower cable for large onshore wind turbines, comprising a conductor, wherein the conductor comprises the aforementioned boron-nitrogen co-doped carbon nanotube-graphene composite fiber; the conductor is formed by stranding multiple of the composite fibers, and the stranding structure is a three-layer gradient variable pitch structure: the inner layer pitch ratio is 8-10, the middle transition layer pitch ratio is 10-12, and the outer layer pitch ratio is 13-16.

[0017] Preferably, the conductor is sequentially provided with a lattice-plasma dual covalent gradient interface coupling layer, a cross-linked polyethylene insulation layer, a shielding layer, and an outer sheath; the dual covalent gradient interface coupling layer is formed by plasma activation and silane coupling agent grafting. More preferably, the plasma activation process conditions are: Ar / O2 volume ratio 4:1, power 100W, and processing time 30-60s; the silane coupling agent is γ-aminopropyltriethoxysilane (KH560), and the grafting conditions are: soaking in 2wt% ethanol solution for 10 minutes and drying at 80℃ for 30 minutes.

[0018] In this invention, boron and nitrogen atoms, during their embedding into the hexagonal lattice of carbon nanotubes, induce local charge reconstruction and lattice strain, achieving permanent p-type doping and effectively mitigating long-term conductivity degradation. Simultaneously, the embedded atoms generate polar active covalent sites (CB, CN) on the carbon nanotube walls. When graphene sheets grow synchronously in situ within the same reaction system, they do not simply physically fill the gaps between the nanotubes, but rather form CBC and CNC covalent bridges with the carbon nanotubes through these active sites. Thus, the graphene sheets become "covalent sutures" connecting the individual carbon nanotubes, fundamentally alleviating the problem of nanotube slippage.

[0019] The synergistic effect exhibits a nonlinear superposition characteristic: boron-nitrogen doping alone only slightly improves conductivity, and physical composite of graphene alone only slightly improves torsional resistance; after in-situ lattice coupling of the two, conductivity is increased by 35%, torsional lifetime is increased by 150%, and thermal cycling decay is reduced by an order of magnitude after 2000 hours.

[0020] Compared with the prior art, the present invention has the following beneficial effects: Lightweight: The composite fiber density of this invention is only 1.7-1.85 g / cm³, which is about 1 / 5 of the density of copper. The weight of the entire cable is reduced by about 59% compared with copper cable, significantly reducing the load on the tower and nacelle.

[0021] High conductivity: By introducing permanent hole / electron carriers through boron-nitrogen lattice doping, the measured conductivity of the composite fiber reaches 62% IACS. Compared with undoped composite fibers, the conductivity is improved by 35%.

[0022] Ultra-low conductivity degradation: The CBC / CNC covalent bonding between graphene sheets and carbon nanotubes fundamentally suppresses tube slippage. The conductivity degradation rate after 2000 hours of thermal cycling is only 0.9%, far superior to the 6.8% of undoped composite fibers and the 21% of exogenously doped systems.

[0023] Ultra-high torsional fatigue life: The cable's ±360° torsional life exceeds 30,000 cycles, which is 10 times higher than copper cables and 150% higher than unadulterated composite fibers. After conversion according to industry standard safety factors, it can meet the equivalent cycle requirements of approximately 2 million cycles over 20 years in wind turbine field applications.

[0024] Strong interfacial adhesion: Through the lattice-plasma dual covalent gradient interfacial coupling layer, the insulation adhesion reaches 0.98 N / mm after 10,000 torsion cycles.

[0025] Synergistic effect: The "boron-nitrogen doping" and "in-situ graphene co-existence" of this invention exhibit nonlinear superposition characteristics - boron-nitrogen doping alone only slightly improves conductivity, and graphene composite alone only slightly improves torsional resistance; after in-situ lattice coupling of the two, conductivity is increased by 35%, torsional lifetime is increased by 150%, and thermal cycling decay is reduced by an order of magnitude. Attached Figure Description

[0026] Figure 1 This is a schematic diagram of the cross-sectional structure of the anti-torsion tower cable for large onshore wind turbines according to the present invention. Detailed Implementation

[0027] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of the invention.

[0028] Limitations of existing carbon nanotube / graphene composite materials: With the development of nanomaterials, the industry is attempting to use carbon nanotube fibers in cable conductors. However, existing technologies have the following inherent drawbacks: Lack of synergistic doping mechanism: Existing composite fibers either rely solely on a single carbon source for growth or employ stepwise doping processes, failing to achieve in-situ integration of boron-nitrogen synergistic doping and graphene intercalation at the lattice level. Simple graphene intercalation relies solely on van der Waals forces for physical bonding; after repeated large-angle torsion, the bundle slips significantly, leading to a sharp increase in contact resistance. Dopant loss and attenuation: Processes that only use external surface doping such as iodine and ferric chloride to improve conductivity are prone to volatilization and loss during thermal cycling, resulting in continuous attenuation of cable conductivity over long-term operation.

[0029] Interface debonding failure: There are no stable active covalent sites on the surface of carbon nanotubes. They rely solely on physical adhesion through plasma and silane coupling agents. After long-term torsion, the insulating layer is prone to delamination.

[0030] The service conditions for cables on large onshore wind turbine towers are extremely harsh: the nacelle undergoes continuous ±360° reciprocating torsion, with an average of over 10,000 torsion cycles per year; the tower height exceeds 100 meters, and the suspension stress generated by the cable's own weight significantly increases the load on the tower top; outdoor temperature differences and current thermal effects lead to long-term thermal cycling. These operating conditions place combined requirements on the conductor for "lightweight, high resistance to torsional fatigue, and ultra-low conductivity attenuation," which cannot be simultaneously met by copper, aluminum alloys, or conventional carbon nanotube fibers.

[0031] To address the aforementioned technical problems, this invention provides a boron-nitrogen co-doped carbon nanotube-graphene composite fiber and an anti-torsion tower cable for large onshore wind turbines using this composite fiber. This invention effectively solves the following problems: How to achieve a permanent increase in the conductivity of carbon nanotubes without using volatile exogenous dopants, and simultaneously generate active sites suitable for chemical bonding? How to solve the problem of severe slippage after torsion caused by relying solely on van der Waals forces for physical bonding between graphene and carbon nanotubes? How to integrate the functions of "doping" and "anchoring" into the same reaction system to achieve the transformation of "doped byproducts into main functional groups"? How to simultaneously grow one-dimensional carbon nanotubes and two-dimensional graphene in the same chemical vapor deposition reaction system and achieve lattice-level chemical bonding? How to solve the problem of anisotropic changes in magnetic susceptibility and low orientation of traditional single-segment magnetic fields caused by lattice distortion due to doping? How to establish a stable insulating layer bonding interface on the surface of carbon nanotubes without active sites? To achieve the above-mentioned objectives, this invention provides a boron-nitrogen co-doped carbon nanotube-graphene composite fiber, comprising carbon nanotubes and graphene sheets. Boron and nitrogen atoms are embedded in the lattice of the carbon nanotubes, and the walls of the carbon nanotubes have CB and / or CN covalent bonds. The graphene sheets are connected to the walls of the carbon nanotubes via CBC and / or CNC covalent bonds. The specific details of this invention are as follows: I. Raw Materials and Equipment Carbon source: First carbon source (carbon nanotube growth): ethanol (analytical grade).

[0032] Second carbon source (graphene in situ co-generation): ethylene glycol (99.9% purity).

[0033] The initial decomposition temperature of ethanol is about 800℃ and that of ethylene glycol is about 900℃. In this invention, the reaction zone is kept at a constant temperature of 1200℃, which is much higher than the initial decomposition temperature of the two carbon sources. This allows for the simultaneous and complete decomposition of the two carbon sources, and the simultaneous completion of the three-step reaction of carbon nanotube growth, graphene sheet growth, and boron-nitrogen lattice doping.

[0034] If other carbon source combinations are used, such as methane plus ethanol or ethanol plus benzene, the cracking rates and decomposition products of these carbon sources differ, making it difficult to simultaneously generate a lattice covalently bridged structure and easily leading to a layered physical mixture. Ethanol and ethylene glycol are the preferred carbon source combination for achieving a covalently co-existing structure under the process conditions of this invention.

[0035] Co-doped precursor: Trimethyl borate and ammonia borane, in a molar ratio of 2:1.

[0036] Through multiple sets of gradient ratio control experiments (1:1, 2:1, 3:1), it was verified that only a B / N molar ratio of 2:1 can achieve uniform embedding of boron and nitrogen atoms into the hexagonal lattice of carbon nanotubes, and the density of active sites of CB and CN in the lattice reaches the optimal threshold. A 1:1 ratio results in insufficient boron atom supply, a scarcity of lattice active sites, low covalent anchoring coverage of graphene, severe tube slippage after twisting, and a large increase in resistance.

[0037] A 3:1 ratio results in nitrogen atom deficiency, lattice strain imbalance, abnormal fiber magnetic susceptibility, a significant decrease in gradient magnetic field orientation, and a reduction in tensile strength.

[0038] Deviations from the 2:1 ratio will directly destroy the covalent symbiotic microstructure of this invention, making it impossible to achieve all the beneficial effects.

[0039] Comparative experiment of different B / N molar ratios: Uniform experimental conditions were maintained: only the molar ratio of trimethyl borate and ammonia borane co-doped precursors was adjusted, with three groups of samples set up at 1:1, 2:1, and 3:1 ratios respectively; all other preparation parameters, including carbon source type, CVD reaction temperature, two-stage gradient magnetic field orientation process, graded densification treatment, and fiber sample size, remained completely consistent. Five parallel monofilament fibers were prepared for each ratio. After testing, outlier data were discarded, and the average value and standard deviation were calculated. The experimental environment was uniformly controlled at 20±2℃ and 65±5%RH relative humidity.

[0040] (1) Mechanical property testing Testing instruments and execution standards: Universal testing machine, tensile testing is carried out in accordance with the national standard GB / T1040; fiber monofilament specimens with a length of 80mm and a diameter of 70-80μm are uniformly selected, the clamping length is 10mm, and the tensile rate is set to 2mm / min.

[0041] Experimental data: The B:N=1:1 specimen exhibited a tensile strength of 1.32±0.06 GPa, an elongation at break of 4.1±0.3%, and an elastic modulus of 112±5 GPa. Microscopic observation of the tensile fracture surface revealed extensive delamination and slippage of carbon nanotube bundles, and large-area peeling and detachment of graphene sheets.

[0042] The B:N=2:1 sample exhibited a tensile strength of 1.91±0.04 GPa, an elongation at break of 8.3±0.4%, and an elastic modulus of 146±4 GPa. Among the three groups of samples, the sample showed the highest tensile strength and moderate elongation at break. The tensile fracture cross-section was dense and flat, with no obvious slippage or delamination between the carbon nanotube bundles and graphene sheets.

[0043] The B:N=3:1 sample exhibited a tensile strength of 1.45±0.07 GPa, an elongation at break of 5.2±0.3%, and an elastic modulus of 121±6 GPa. Insufficient nitrogen content and excessive boron atoms embedded in the carbon lattice led to lattice strain imbalance and numerous distortion defects within the fiber.

[0044] Experimental conclusion: Only a B:N molar ratio of 2:1 can achieve lattice strain equilibrium and maximize the covalent anchoring effect between graphene and carbon nanotubes.

[0045] (2) Electrical performance testing Test instruments and operating methods: Four-probe low resistance tester; Before testing, silver paste electrodes are uniformly coated on both ends of the fiber to eliminate interference from interfacial contact resistance. The effective conductive test length of the fiber is 50mm; The resistance of each group of samples is tested repeatedly 8 times, and the average value is used to calculate the volume resistivity.

[0046] Experimental data: B:N=1:1 sample: volume resistivity 1.86×10 -4 Ω·cm. The imbalance in the total amount of boron and nitrogen doping causes their charge compensation effects to cancel each other out, resulting in scarce carrier migration channels within the crystal lattice.

[0047] Sample with B:N=2:1: Volume resistivity 0.72×10⁻⁶ -4 The resistivity was Ω·cm, the lowest among the three groups of samples. Boron atoms provided hole carriers in the crystal lattice, while nitrogen atoms provided electron carriers, resulting in optimal lattice charge reconstruction.

[0048] Sample with B:N=3:1: Volume resistivity 1.31×10⁻⁶ -4Ω·cm. Nitrogen atom supply is lacking, lattice charge reconstruction is incomplete, and the effective carrier concentration is lower than that of a 2:1 ratio sample.

[0049] Experimental conclusion: B:N=2:1 is the only critical ratio that can simultaneously utilize boron holes and nitrogen electrons to achieve synergistic conductivity.

[0050] (3) Magnetic performance test Test instruments and test conditions: Vibrating sample magnetometer (VSM), test was carried out at room temperature of 25℃, external magnetic field scanning range from -1T to 1T, complete acquisition of MH hysteresis loop, and calculation of the sample's room temperature magnetic susceptibility χ.

[0051] Experimental data: B:N=1:1 sample: The total boron and nitrogen doping content is low, the number of lattice active sites is sparse, the magnetic response signal intensity is weak, and the hysteresis loop signal-to-noise ratio is poor.

[0052] B:N=2:1 sample: The magnetic susceptibility is stable without abrupt changes, the hysteresis loop is smooth and regular, and it exhibits standard paramagnetic and weak magnetic response characteristics; the overall strain of the crystal lattice reaches equilibrium, and the magnetic order of the fiber is uniform and stable.

[0053] B:N=3:1 sample: Excessive boron atoms embedded in the lattice caused severe lattice distortion, resulting in irregular abrupt changes in the magnetic susceptibility value, and irregular protrusions and inflection points in many places on the hysteresis loop.

[0054] Experimental conclusion: Only a 2:1 molar ratio can achieve lattice strain balance, ensure uniform and stable fiber magnetization performance, and meet the requirements of gradient magnetic field oriented processing technology.

[0055]

[0056] Catalyst: Ferrocene (purity ≥ 98%).

[0057] Additive: Thiophene.

[0058] Carrier gas: a mixture of hydrogen and argon in a volume ratio of 1:1.

[0059] Reactor: Horizontal tube CVD furnace, constant temperature zone length ≥30cm.

[0060] Magnetic field device: A two-section gradient axial magnetic field is set along the fiber traction direction, which can provide a segmented adjustable magnetic field of 0.2-1.5T.

[0061] First magnetic field equipment: 0.5T steady-state weak axial magnetic field generator (first-stage pre-conditioned axial gradient solenoid magnet).

[0062] Second magnetic field equipment: 1.0T steady-state strong axial magnetic field generator (second-stage directional axial gradient solenoid magnet).

[0063] Magnetic field orientation principle: In the first stage (pre-regulation), the fiber enters the first magnetic field unit at a constant speed (e.g., 5 mm / s), where a weak magnetic field of 0.5T is used to pre-relax and regulate the lattice distortion and internal stress caused by doping within the fiber. In the second stage (precise orientation), the fiber enters the second magnetic field unit, where a strong magnetic field of 1.0T efficiently and uniformly locks all carbon nanotubes along the fiber axis. Transition zone protection effectively prevents orientation springback or disorder of the fiber when switching magnetic fields.

[0064] A single constant magnetic field or a single-segment magnetic field cannot eliminate the orientation disorder caused by doped lattice distortion, and the fiber orientation degree can only reach below 80%.

[0065]

[0066] Linear fitting results for the gradient transition region: Fitting equation B(z) = 0.0099z - 0.8808 (Z-axis interval 150-190mm), linear correlation coefficient R² = 0.9987, gradient value 2.50T / m.

[0067] Both magnetic field segments exhibit good plateau uniformity: the deviation of the first segment is ≤ ±0.3%, and the deviation of the second segment is ≤ ±0.25%.

[0068] II. Preparation Method Step 1: Dual carbon source floating catalytic co-growth plus in-situ boron-nitrogen doping of the crystal lattice Ferrocene was dissolved in ethanol to prepare a 1.0% (w / w) solution; ethylene glycol was added simultaneously as a carbon source for graphene growth, and a mixed precursor of trimethyl borate and ammonia borane was added (8% of the total mass of the mixed solution), and thiophene was added at 8% of the mass of ferrocene.

[0069] The mixed solution was injected into the evaporation chamber at 200℃ using a micro-injection pump at a rate of 12 mL / h for complete vaporization, and then carried into the reaction isothermal zone by a carrier gas of H2 / Ar with a total flow rate of 3000 sccm; the reaction zone was kept at a constant temperature of 1200℃.

[0070] Under this high-temperature environment, ethanol and ethylene glycol, two carbon sources, undergo simultaneous pyrolysis: ethanol pyrolysis begins at approximately 800°C, generating active carbon groups for one-dimensional carbon nanotube growth; ethylene glycol pyrolysis begins at approximately 900°C, releasing two-dimensional sheet carbon precursors. The 1200°C isothermal reaction zone is far above the pyrolysis thresholds of both carbon sources, enabling simultaneous and complete pyrolysis of both types of carbon sources, which can then be directionally supplied with the carbon units required for the growth of carbon nanotube bundles and ultrathin graphene sheets.

[0071] Simultaneously, boron and nitrogen atoms in a fixed 2:1 ratio are embedded into the carbon nanotube lattice to form stable CB and CN covalent bonds. The formation of these lattice active sites enables the in-situ growing graphene sheets to achieve in-situ covalent bonding with the carbon nanotube wall through these active sites, forming an integrated covalent symbiotic network of "doping-induced anchoring".

[0072] Step 2: Coordinated Orientation of Two Gradient Axial Magnetic Fields A segmented axial steady magnetic field is set between the reaction tube outlet and the fiber collection device: a 0.5T weak magnetic field in the front section pre-regulates the carbon nanotube / graphene composite aerogel, and a 1.0T strong magnetic field in the back section precisely orients the fiber axis.

[0073] After being modulated by a gradient magnetic field, the overall orientation degree of the composite aerogel fibers stabilizes at 93%-96%.

[0074] Orientation degree was determined using the sound velocity anisotropy method, and the specific operation is as follows: Sample preparation: Take composite aerogel fiber samples after gradient magnetic field control, with a length ≥100mm, and ensure that both ends are flush.

[0075] Axial sound velocity measurement: The propagation speed C (m / s) of sound waves along the fiber axis was measured using a sound velocity orientation measuring instrument under standard temperature and humidity conditions (20±2℃, 65±2%RH).

[0076] Random orientation sound velocity measurement: Isotropic aerogel samples from the same batch that have not been treated with a magnetic field were taken and their sound velocity C was measured under the same conditions. u .

[0077] Orientation factor calculation: The sound speed orientation factor f is calculated according to the Moseley sound speed orientation formula. a : f a = 1 C u ² / C² In the formula, f a C is the orientation factor (0~1). u denoted as ν0, where ν0 is the sound velocity of the randomly oriented sample (m / s), and C is the measured sound velocity of the sample to be tested (m / s).

[0078]

[0079] After being modulated by a gradient magnetic field, the acoustic velocity orientation factor f of the composite aerogel fiber is... a The value reached 0.93-0.96, which is highly consistent with the 93%-96% orientation degree measured by X-ray diffraction.

[0080] Step 3: Self-activation of intrinsic active sites in the crystal lattice After boron and nitrogen atoms are embedded in the carbon lattice, the fiber tube wall naturally carries polar active sites, which can greatly increase the carrier concentration without the need for additional external dopants such as sprayed iodine and ferric chloride.

[0081] Even under prolonged high-temperature conditions exceeding 500°C, lattice-doped B / N exhibits trace dedoping behavior. Under 2000h thermal cycling test conditions, the attenuation of the doped material can be controlled within 1.2%.

[0082] Step 4: Graded densification and continuous winding The composite fiber is first pre-densified by room temperature ethanol vapor, and then densified a second time by a 3s acetone vapor bath; after densification, the fiber density is stable at 1.7-1.85g / cm³; the traction roller traction speed is 2m / min for continuous winding, and the continuous length of a single fiber can reach more than 1000 meters.

[0083] III. Composite Fiber Performance Parameters

[0084] IV. Overall Cable Structure and Functional Layer Design From inside to outside: (I) Boron-nitrogen co-doped carbon nanotube-graphene composite fiber conductor Multiple continuous composite fibers are bundled together using a three-layer gradient variable pitch twisting method: the inner core layer has a pitch ratio of 8-10; the middle transition layer has a pitch ratio of 10-12; and the outer flexible layer has a pitch ratio of 13-16.

[0085] (ii) Lattice-plasma dual covalent gradient interface coupling layer a) Plasma activation: The stranded conductor is passed through an atmospheric pressure plasma gun with an Ar / O2 volume ratio of 4:1, a power of 100W, and a processing time of 30-60s.

[0086] b) Covalent grafting with silane coupling agent: Immediately after treatment, immerse in 2wt% γ-aminopropyltriethoxysilane (KH560) ethanol solution for 10 minutes, and dry in an oven at 80℃ for 30 minutes to form a double-layer coupling thin layer with a thickness of 50-200nm.

[0087] (iii) Insulation layer The material is cross-linked polyethylene (XLPE), with a thickness of 1.2-2.0 mm; the extrusion process temperature is 165-190℃.

[0088] (iv) Shielding layer The inner shield is wrapped with a semi-conductive buffer strip; the outer shield is a copper wire braided shield with a braiding density of ≥80%.

[0089] (v) Anti-torsion cable structure The three-core cable uses EPDM rubber filler strips for positioning, with a cable section diameter ratio of 13-17; the outer side is wrapped with ceramicized polyolefin tape.

[0090] (vi) Outer sheath layer The material is thermoplastic polyurethane (TPU) or neoprene rubber (CR), with a thickness of 1.8-2.5mm.

[0091] V. Example 1 (I) Preparation of composite fibers Prepared according to the parameters described above. A dual carbon source of ethanol and ethylene glycol was used, with a strict molar ratio of trimethyl borate to ammonia borane of 2:1, and two gradient magnetic fields of 0.5T + 1.0T were applied.

[0092] The resulting composite fiber monofilament has a diameter of approximately 75 μm, a density of 1.78 g / cm³, a tensile strength of 1.9 GPa, a conductivity of 62% that of a copper conductor of the same cross-section, and a conductivity decay of only 0.9% after 2000 hours of thermal cycling.

[0093] XPS analysis showed that the molar ratio of boron to carbon atoms was 1:420 and the molar ratio of nitrogen to carbon atoms was 1:380.

[0094] TEM electron microscopy revealed that the graphene sheets were anchored to the carbon nanotube walls via CBC and CNC covalent bonds.

[0095] (ii) Conductor stranding Each bundle contains 120 composite fiber monofilaments, and a conductor with an equivalent cross-sectional area of ​​16 mm² is prepared by three-layer gradient stranding: the inner layer has 7 bundles with a pitch ratio of 9; the middle transition layer has 10 bundles with a pitch ratio of 11; and the outer layer has 12 bundles with a pitch ratio of 14.

[0096] (III) Interface Coupling Processing Plasma activation for 45 seconds; silane grafting (2wt% KH560, 10 minutes, dried at 80℃). The total thickness of the double-layer coupling layer is approximately 130nm, and the insulation adhesion is 0.98N / mm after 10,000 twists.

[0097] (iv) Cable processing XLPE insulation thickness 1.5mm; copper wire braided shielding density 85%; three-core gap filler EPDM, cabling section diameter ratio 15; TPU sheath thickness 2.0mm.

[0098] (v) Overall performance of the cable Under uniform test conditions (same tension, ambient temperature, and current carrying capacity), the total cable weight is 110kg / 100m, the ±360° torsional life is >30,000 cycles (for the whole cable test, a 15% increase in resistance is considered a failure), and the temperature rise is 51K.

[0099] Compared to copper cables of the same structure (only the conductor is replaced, and the rest of the layers are completely identical), their torsional life is only about 5,000 cycles. The overall cable life of this invention is 6 times longer than that of copper cables.

[0100] The cable's 30,000 laboratory torsional life, combined with industry standard safety factors, can meet the equivalent 2 million cycles required for wind turbine applications over 20 years.

[0101] VI. Comparative Example All comparative examples have insulation, shielding, filling, and sheathing structures that are completely identical to those in Example 1, except for the conductor material or manufacturing process. All examples are tested under the same conditions.

[0102] Comparative Example 1 (Conventional Copper Conductor): The conductor is a Class 2 soft copper stranded wire conforming to national standards, with an equivalent cross-section of 16mm² (GB / T3956). Test results: The total cable weight is 267kg / 100m; the core breaks after approximately 3000 ±360° twists; the temperature rise is 48K.

[0103] Comparative Example 2 (Ordinary exogenously doped pure carbon nanotube fibers): The conventional floating catalytic method has no gradient magnetic field, no graphene intercalation, and no boron-nitrogen lattice doping, only iodine external doping, with an orientation degree of 82% and a conductivity of 32% IACS. After 5000 twists, the resistance increases by 28%, and the insulation adhesion is only 0.05 N / mm.

[0104] Comparative Example 3 (Aluminum Alloy Conductor): Made of 8A07 aluminum alloy, with a cross-section of 25mm². It weighs 185kg / 100m, has a conductivity of 55% IACS, and develops fatigue cracks after approximately 8000 torsional cycles.

[0105] Comparative Example 4 (Graphene-carbon nanotube composite fibers without boron and nitrogen doping): Preparation differences: Except for the absence of trimethyl borate and ammonia borane precursors, the preparation conditions were exactly the same as in Example 1.

[0106] Test results: The total cable weight is 108 kg / 100 m; the conductivity is only 46% IACS; the conductivity decay rate after 2000 h of thermal cycling is 6.8%; the torsional life is about 12,000 cycles; and the insulation adhesion is 0.3 N / mm.

[0107] Comparative Example 5 (Simulation of Step-by-Step Combination of Existing Technologies): Preparation differences: Boron-nitrogen-doped carbon nanotube fibers were first prepared using conventional methods (single carbon source only, no in-situ graphene growth), and then graphene sheets were attached to the fiber surface by physical coating. The remaining conditions were the same as in Example 1.

[0108] Test results: The total cable weight is 112 kg / 100 m; the conductivity is only 51% IACS; the thermal cycling decay rate is 3.5% after 2000 h; the torsional life is about 15,000 cycles; and the insulation adhesion is 0.4 N / mm.

[0109] Comprehensive comparison summary table:

[0110] All the above comparative examples were tested under a complete cable structure. Although the bare fiber performance of Comparative Examples 4 and 5 was better than that of copper, when placed in the same cabling structure, the torsional life of the entire cable was much lower than that of Example 1 due to the lack of chemical and mechanical synergy between fiber-interface-insulation.

Claims

1. A boron-nitrogen co-doped carbon nanotube-graphene composite fiber, characterized in that, The composite fiber comprises carbon nanotubes and graphene sheets. Boron and nitrogen atoms are embedded in the lattice of the carbon nanotubes, and the walls of the carbon nanotubes have CB and / or CN covalent bonds. The graphene sheets are connected to the walls of the carbon nanotubes through CBC and / or CNC covalent bonds.

2. The composite fiber according to claim 1, characterized in that, The molar ratio of boron atoms to nitrogen atoms is 1.5:1 to 2.5:1; the density of the composite fiber is 1.7-1.85 g / cm³, the conductivity is 52%-59% IACS, and the tensile strength is 1.8-2.2 GPa.

3. The composite fiber according to claim 2, characterized in that, The molar ratio of boron atoms to nitrogen atoms is 2:

1.

4. A method for preparing boron-nitrogen co-doped carbon nanotube-graphene composite fibers, characterized in that, Includes the following steps: A floating catalytic chemical vapor deposition method was used to simultaneously introduce a first carbon source, a second carbon source, a boron source, and a nitrogen source into the reaction system, and simultaneously carry out carbon nanotube growth, graphene sheet growth, and boron-nitrogen lattice doping at a temperature of 1000-1300℃. The first carbon source is pyrolyzed to generate carbon nanotubes, and the second carbon source is pyrolyzed to generate graphene sheets; The boron and nitrogen atoms generated by the cracking of the boron and nitrogen sources are embedded in the hexagonal lattice of the carbon nanotubes to form CB and / or CN covalent bonds. The graphene sheets are covalently bonded to the walls of the carbon nanotubes via CB and / or CN bonds, forming CBC and / or CNC bonds.

5. The preparation method according to claim 4, characterized in that, The first carbon source is ethanol, the second carbon source is ethylene glycol, and the reaction temperature is 1200℃; the molar ratio of the boron source to the nitrogen source is 2:

1.

6. The preparation method according to claim 4, characterized in that, It also includes oriented treatment of the composite aerogel generated by pyrolysis by sequentially passing it through a first gradient axial magnetic field of 0.3-0.7T and a second gradient axial magnetic field of 0.8-1.2T.

7. The preparation method according to claim 6, characterized in that, The intensity of the first gradient axial magnetic field is 0.5T, and the intensity of the second gradient axial magnetic field is 1.0T.

8. The preparation method according to claim 4, characterized in that, It also includes subjecting the composite fibers to ethanol steam pre-densification treatment and acetone steam bath secondary densification treatment in sequence.

9. A torsion-resistant tower cable for large onshore wind turbines, comprising a conductor, characterized in that, The conductor comprises the boron-nitrogen co-doped carbon nanotube-graphene composite fiber as described in any one of claims 1-3; the conductor is formed by stranding multiple of the composite fibers, and the stranding structure is a three-layer gradient variable pitch structure: the inner layer pitch ratio is 8-10, the middle transition layer pitch ratio is 10-12, and the outer layer pitch ratio is 13-16.

10. The cable according to claim 9, characterized in that, The conductor is provided with a lattice-plasma dual covalent gradient interface coupling layer, a cross-linked polyethylene insulation layer, a shielding layer and an outer sheath in sequence; the dual covalent gradient interface coupling layer is formed by plasma activation and silane coupling agent grafting.