A chip array bonding process and device

By using photoresist layer temporary bonding and chemical plating or electroplating processes to achieve bonding of optoelectronic chip arrays at room temperature, the problems of thermal stress damage and high cost caused by high-temperature processes in existing technologies are solved, the integration density and reliability of chip arrays are improved, and the manufacturing requirements of high-density optoelectronic chip arrays are met.

CN123076299APending Publication Date: 2026-11-10SHENZHEN REWO MICRO SEMICON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611273090.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing optoelectronic chip array bonding processes suffer from problems such as thermal stress damage caused by high-temperature processes, complex and costly processes, poor reliability of heterogeneous metal bonding interfaces, and limited improvement in electrode integration density.

Method used

Two wafers are temporarily bonded using a photoresist layer. The growth substrate of the first wafer is removed and patterned etching is performed. Bonding metal is grown in the plating window through chemical plating or electroplating processes to achieve metal bonding between the corresponding electrodes of the first wafer and the second wafer. The entire process is completed at room temperature.

Benefits of technology

It avoids thermal stress damage caused by high-temperature processes, reduces equipment investment and manufacturing costs, improves the integration density and long-term operational reliability of chip arrays, adapts to smaller pitch electrode interconnects, and balances device performance and mass production feasibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076299A_ABST
    Figure CN123076299A_ABST
Patent Text Reader

Abstract

This application proposes a chip array bonding process and device. The method includes aligning and bonding a first wafer carrying a plurality of chip arrays with a second wafer having corresponding electrode arrays, temporarily bonding the first wafer and the second wafer with a photoresist layer; removing the growth substrate of the first wafer and performing pattern etching on the first wafer to obtain multiple independent chip arrays; performing photolithography on the patterned wafer structure to form metal plating windows at the corresponding positions of the pins; growing bonding metal in the plating windows using chemical plating or electroplating processes, and achieving metal bonding between the corresponding electrodes of the first wafer and the second wafer through the bonding metal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of chip bonding technology, and in particular to a chip array bonding process method and device. Background Technology

[0002] With the rapid development of CPO and NPO co-packaged optics, AR augmented reality glasses, and other fields, the application scale of high-density optoelectronic chip array devices continues to expand, placing higher demands on device integration, optoelectronic performance, and manufacturing yield. The bonding and interconnection of the optoelectronic chip array with the driving circuit wafer is one of the core processes in device manufacturing. Its process precision, process conditions, and connection quality directly determine the pixel density, operational stability, and lifespan of the chip array. Therefore, high-performance bonding technology has become a key technology restricting the industrialization of next-generation micro-pitch optoelectronic devices.

[0003] Currently, the mainstream optoelectronic wafer bonding processes in the industry are mainly thermocompression bonding and hybrid bonding. Thermocompression bonding achieves physical connection by plastically deforming metal bumps under high temperature and pressure. However, its process temperature is high, which can easily generate thermal stress inside the optoelectronic chip and driver wafer, causing problems such as chip performance drift and decreased alignment accuracy. Moreover, the physical bonding interface of dissimilar metals has a large thermal resistance, making it difficult to guarantee heat dissipation performance and long-term reliability. Although hybrid bonding can achieve higher interconnect density, its process flow is lengthy, and it has extremely stringent requirements for wafer surface flatness and cleanliness. The equipment investment and process cost are high, and mass production yield control is difficult.

[0004] In addition, existing bonding solutions generally require the pre-fabrication of independent metal bump structures on the wafer surface, which involves complicated process steps. Furthermore, there are technical bottlenecks in miniaturizing the size and spacing of the bumps, which limits the further improvement of the pixel density of optoelectronic chip arrays. At the same time, most processes are only compatible with wafer-to-wafer bonding modes and cannot flexibly accommodate the heterogeneous integration requirements of chips to wafers, resulting in significant limitations in application scenarios. Summary of the Invention

[0005] In view of the aforementioned problems, this application is proposed to provide a chip array bonding process method that overcomes or at least partially solves the aforementioned problems, comprising the steps of: A first wafer carrying several chip arrays is aligned and bonded to a second wafer with corresponding electrode arrays, and the first wafer and the second wafer are temporarily bonded together by a photoresist layer; The growth substrate of the first wafer is removed, and the first wafer is patterned and etched to form multiple independent chip arrays. The chip array is subjected to photolithography and development processes to form metal-plated windows at the corresponding positions of the chip pins; A bonding metal is grown within the plating window using a chemical plating or electroplating process, and the metal bonding between the corresponding electrodes of the first wafer and the second wafer is achieved through the bonding metal.

[0006] Further, the step of aligning and bonding the first wafer carrying the chip array with the second wafer having a corresponding electrode array, and temporarily bonding the first wafer and the second wafer together using a photoresist layer, includes: The photoresist layer is formed using negative photoresist as a temporary bonding medium, and the first wafer and the second wafer are aligned and bonded according to the electrode correspondence. The first wafer and the second wafer are bonded using a wafer-to-wafer bonding mode or a chip-to-wafer bonding mode.

[0007] Further, the removal of the growth substrate from the first wafer and the pattern etching process performed on the first wafer to form a plurality of independent chip arrays include: The growth substrate of the first wafer is removed by laser lift-off process; The chip is patterned by inductively coupled plasma etching to form a preset array of multiple independent chips; wherein, the electrode pins of the first wafer and / or the electrodes of the second wafer are provided with metal pillars, the lateral dimension of the metal pillars being smaller than the lateral dimension of the electrode pins.

[0008] Furthermore, the step of performing photolithography and development on the patterned wafer structure to form a metal-plated window at the corresponding position of each chip pin includes: The patterned wafer structure is subjected to exposure and development processes in sequence to remove the photoresist outside the area corresponding to the electrode pins, and to form exposed metal plating windows at the preset bonding positions of the electrode pins.

[0009] Furthermore, the step of growing bonding metal within the plating window using a chemical plating or electroplating process, and achieving metal bonding between the corresponding electrodes of the first wafer and the second wafer through the bonding metal, includes: A bonding metal is grown within the plating window using a chemical plating or electroplating process; wherein the bonding metal is any one or more combinations of gold, silver, nickel, aluminum, copper, tin, and titanium. The bonding metal forms a metal chemical bond with the metal layers of the electrodes on both sides, thereby achieving the bonding connection between the corresponding electrodes of the first wafer and the second wafer.

[0010] Furthermore, the plating agent used in the electroless plating or electroplating process is a liquid agent or a gaseous agent.

[0011] Furthermore, the metal column is made of copper.

[0012] Furthermore, the growth substrate of the first wafer is one of sapphire substrate, gallium arsenide substrate, indium phosphide substrate or silicon substrate.

[0013] Furthermore, the second wafer is a wafer integrating a complementary metal-oxide-semiconductor driving circuit.

[0014] A chip array device, wherein the chip array device is fabricated using the chip array bonding process described in any one of the above claims.

[0015] This application has the following advantages: In the embodiments of this application, addressing the shortcomings of existing bonding processes such as high-temperature processes that easily cause thermal stress damage to chips, complex and costly processes, poor reliability of heterogeneous metal bonding interfaces, and limited improvement in electrode integration density, this application proposes a chip array bonding process method. Specifically, it includes aligning and bonding a first wafer carrying a plurality of chip arrays with a second wafer having corresponding electrode arrays; temporarily bonding the first wafer and the second wafer with a photoresist layer; removing the growth substrate of the first wafer and performing pattern etching on the first wafer to form multiple independent chip arrays; performing photolithography and development on the chip arrays to form metal plating windows at the corresponding positions of the pins of each chip; growing bonding metal within the plating windows using chemical plating or electroplating processes; and achieving metal bonding between the corresponding electrodes of the first wafer and the second wafer through the bonding metal. By first achieving precise alignment and temporary fixation of two wafers with a photoresist layer, and then growing bonding metals in situ after substrate peeling, electrode patterning, and photolithographic windowing to complete the interconnection, chemical bonding between metals can be achieved at room temperature, effectively avoiding thermal stress damage caused by high-temperature processes, and ensuring chip performance and alignment accuracy. There is no need to prepare independent metal bumps in advance, which simplifies the process steps and reduces equipment investment and manufacturing costs. The homogeneous metal bonding interface has low thermal resistance and high connection strength, which can be adapted to smaller pitch electrode interconnects, significantly improving the integration density and long-term operational reliability of the chip array, while taking into account both device performance and mass production feasibility. Attached Figure Description

[0016] To more clearly illustrate the technical solution of this application, the drawings used in the description of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 This is a flowchart of a chip array bonding process provided in an embodiment of this application; Figure 2This is a schematic diagram of the alignment temporary bonding structure of a chip array bonding process provided in an embodiment of this application; Figure 3 This is a schematic diagram of the structure after substrate removal in a chip array bonding process according to an embodiment of this application; Figure 4 This is a schematic diagram of the structure after ICP etching in a chip array bonding process according to an embodiment of this application; Figure 5 This is a schematic diagram of the structure after exposure and development of a chip array bonding process provided in an embodiment of this application; Figure 6 This is a schematic diagram of the bonded structure of a chip array bonding process provided in an embodiment of this application. Detailed Implementation

[0018] To make the objectives, features, and advantages of this application more apparent and understandable, the application will be further described in detail below with reference to the accompanying drawings and specific embodiments. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

[0019] The inventors, through analysis of existing technologies, discovered that the current mainstream multilayer wafer bonding processes in the industry are mainly thermocompression bonding and hybrid bonding. Thermocompression bonding achieves physical connection by plastically deforming metal bumps under high temperature and pressure. However, its process temperature is high, which easily generates thermal stress inside the chip and driver wafer, causing problems such as chip performance drift and decreased alignment accuracy. Moreover, the physical bonding interface of dissimilar metals has a large thermal resistance, making it difficult to guarantee heat dissipation performance and long-term reliability. Although hybrid bonding can achieve higher interconnect density, its process flow is lengthy, and it has extremely stringent requirements for wafer surface flatness and cleanliness. The equipment investment and process costs are high, and mass production yield control is difficult.

[0020] Reference Figure 1 This paper illustrates a chip array bonding process, including the following steps: S110. Align and bond a first wafer carrying a plurality of chip arrays with a second wafer having a corresponding electrode array, and temporarily bond the first wafer and the second wafer together with a photoresist layer. S120: Remove the growth substrate of the first wafer and perform pattern etching on the first wafer to obtain multiple independent chip arrays; S130. Perform photolithography and development on the chip array to form a metal plating window at the corresponding position of the pin of each chip; S140. A bonding metal is grown in the plating window using a chemical plating or electroplating process, and the metal bonding between the corresponding electrodes of the first wafer and the second wafer is achieved through the bonding metal.

[0021] It should be noted that step S110 achieves temporary bonding between the two wafers through a photoresist layer. On the one hand, this precisely locks the correspondence between the upper and lower electrodes, providing a unified alignment reference for all subsequent back-side processes and avoiding the cumulative errors caused by repeated alignment in multiple processes. On the other hand, this photoresist layer can be directly reused as a mask substrate for subsequent photolithography processes, eliminating the need to remove the temporary bonding layer and reapply the photoresist, effectively simplifying the process. Steps S120 and S130, while maintaining the temporary bonding state, sequentially complete substrate removal, wafer patterning etching, and window deposition, without disrupting the wafer alignment throughout the process. This achieves micron-level pattern control precision, providing a technological foundation for high-density interconnection of micro-pitch chip arrays. At the same time, the photolithographic window precisely defines the metal growth area, effectively avoiding electrode short-circuit problems caused by bonding metal overflow.

[0022] Step S140 employs in-situ chemical or electroplating processes to grow bonding metals. The entire bonding process can be completed under ambient temperature and pressure conditions, fundamentally avoiding the damage to the chip's optoelectronic performance and driving circuit characteristics caused by high-temperature thermal stress in traditional hot-press bonding and hybrid bonding processes. It also eliminates the risk of alignment misalignment caused by wafer warpage at high temperatures. The in-situ grown bonding metal forms a metallurgical-grade chemical bond with the electrodes on both sides, resulting in high interface bonding strength and low contact and thermal resistance. Compared to physical pressing bonding of dissimilar metals, the electrical performance, heat dissipation capacity, and long-term reliability of the device are significantly improved. The overall process is suitable for both wafer-level mass production and chip-level heterogeneous integration, meeting the manufacturing requirements of high-density chip arrays in fields such as optical interconnect co-package optics and AR augmented reality glasses. While ensuring bonding accuracy and reliability, it effectively reduces process difficulty and production costs.

[0023] In the embodiments of this application, addressing the shortcomings of existing bonding processes such as high-temperature processes that easily cause thermal stress damage to chips, complex and costly processes, poor reliability of heterogeneous metal bonding interfaces, and limited improvement in electrode integration density, this application proposes a chip array bonding process method. Specifically, it includes aligning and bonding a first wafer carrying a chip array with a second wafer having a corresponding electrode array; temporarily bonding the first wafer and the second wafer with a photoresist layer; removing the growth substrate of the first wafer and patterning the first wafer to obtain multiple independent chip arrays; performing photolithography on the patterned wafer structure to form metal plating windows at the corresponding pin positions; growing bonding metal within the plating windows using chemical plating or electroplating processes; and achieving metal bonding between the corresponding electrodes of the first wafer and the second wafer through the bonding metal. By first achieving precise alignment and temporary fixation of two wafers with a photoresist layer, and then growing bonding metals in situ after substrate peeling, electrode patterning, and photolithographic windowing to complete the interconnection, chemical bonding between metals can be achieved at room temperature, effectively avoiding thermal stress damage caused by high-temperature processes, and ensuring chip performance and alignment accuracy. There is no need to prepare independent metal bumps in advance, which simplifies the process steps and reduces equipment investment and manufacturing costs. The homogeneous metal bonding interface has low thermal resistance and high connection strength, which can be adapted to smaller pitch electrode interconnects, significantly improving the integration density and long-term operational reliability of the chip array, while taking into account both device performance and mass production feasibility.

[0024] The following will further describe a chip array bonding process method in this exemplary embodiment.

[0025] Reference Figure 2 As described in step S110, a first wafer carrying a plurality of chip arrays is aligned and bonded to a second wafer having a corresponding electrode array, and the first wafer and the second wafer are temporarily bonded together by a photoresist layer.

[0026] It should be noted that the core function of using a photoresist layer to temporarily bond two wafers is to provide stable structural support and alignment reference for subsequent back-side processes such as substrate removal, electrode patterning, and metal deposition. This ensures that the electrode correspondence between the upper and lower wafers remains accurate throughout multiple processes, preventing relative shifts. Simultaneously, the photoresist layer fills the microscopic gaps between the two wafer mating surfaces, improving the overall stability of the temporary bonding structure and preventing wafer warping and displacement during the process. Unlike traditional bonding processes where the bonding medium only serves a connecting function, the photoresist layer in this solution functions as both a temporary bonding medium and a mask substrate for subsequent photolithography processes. Patterning and windowing can be directly performed on this layer in subsequent steps without the need to remove the temporary bonding layer and re-fabricate the photolithography mask, effectively simplifying the process steps.

[0027] In one embodiment of the present invention, the specific process of step S110, which involves "aligning and bonding a first wafer carrying a plurality of chip arrays with a second wafer having a corresponding electrode array, and temporarily bonding the first wafer and the second wafer together with a photoresist layer", can be further described in conjunction with the following description.

[0028] As described in the following steps, a photoresist layer is formed using negative photoresist as a temporary bonding medium, and the first wafer and the second wafer are aligned and bonded according to the electrode correspondence. The first wafer and the second wafer are bonded using a wafer-to-wafer bonding mode or a chip-to-wafer bonding mode; It should be noted that negative photoresist is chosen as a temporary bonding medium because it undergoes cross-linking and curing after exposure. Unexposed areas can be removed by development. Its photolithographic properties are highly compatible with the subsequent window patterning process. The photoresist layer can be directly reused to complete the photolithographic window opening without recoating the photoresist, which can reduce process steps and lower manufacturing costs. Meanwhile, negative photoresist possesses excellent etching resistance and high-temperature resistance, capable of withstanding the process conditions of laser lift-off and plasma etching, maintaining the integrity of the bonding structure and the photoresist layer itself in multiple processes. The use of switchable wafer-to-wafer or chip-to-wafer bonding modes allows this process to be adapted to both large-scale mass production scenarios at the whole wafer level, improving production efficiency through synchronous alignment bonding across the entire surface, and heterogeneous integration and customized production scenarios, flexibly bonding chips of different specifications and processes to driver wafers, significantly broadening the process's applicability and scenario adaptability.

[0029] As described in step S120, the growth substrate of the first wafer is removed, and the first wafer is patterned and etched to obtain multiple independent chip arrays.

[0030] It should be noted that the substrate removal and electrode patterning processes are completed sequentially from the back side of the first wafer. The entire process is based on a locked alignment reference, which ensures that the final electrode pins maintain a precise correspondence with the electrodes on the second wafer, avoiding accuracy deviations caused by secondary alignment. Through substrate removal and patterning, the internal electrode structure of the chip can be precisely exposed and shaped into a preset bonding pin configuration. This provides a clean and regular working surface for subsequent metal plating and bonding connections, serving as a fundamental preparatory step for achieving high-density, precise electrode interconnection.

[0031] In one embodiment of the present invention, the specific process of step S120, "removing the growth substrate of the first wafer and performing pattern etching on the first wafer to obtain a plurality of independent chip arrays," can be further described in conjunction with the following description.

[0032] Reference Figures 3-4As described in the following steps, the growth substrate of the first wafer is removed by laser lift-off process to reduce the chip thickness; It should be noted that the laser lift-off process for removing the growth substrate utilizes laser energy to decompose the interface material between the substrate and the chip epitaxial layer. This allows for non-destructive lift-off of the substrate at low temperatures, effectively avoiding the damage to the chip's optoelectronic performance caused by high-temperature lift-off methods. Furthermore, it does not compromise the bonding strength and alignment accuracy of the temporary bonding layer. This process is particularly suitable for gallium nitride-based chips on sapphire substrates. After lift-off, the electrode surfaces of the chip exhibit good integrity and few surface impurities, allowing it to directly proceed to subsequent etching processes without requiring additional complex surface treatments.

[0033] As described in the following steps, the first wafer is patterned by inductively coupled plasma etching to form multiple independent chip arrays; wherein, metal pillars are pre-set on the electrode pins of the first wafer and / or the electrodes of the second wafer, and the lateral dimension of the metal pillars is smaller than the lateral dimension of the electrode pins; It should be noted that the electrode patterning process using inductively coupled plasma etching (ICP-E) offers advantages such as high etching precision, good anisotropy, and excellent edge steepness. This enables the fabrication of fine electrode patterns at the micrometer and even sub-micrometer scales, meeting the high-density pin fabrication requirements of micro-pitch chip arrays. By pre-setting smaller metal pillars on single-sided or double-sided electrodes, the lateral dimension of the actual bonding area can be reduced, further increasing the integration density of the electrode array. Simultaneously, the metal pillars can compensate for the microscopic gaps between the two wafer electrodes, making it easier for the subsequently deposited bonding metal to form a continuous and reliable connection interface, reducing the risk of false connections and improving bonding yield and connection reliability. The flexible single-sided or double-sided configuration also adapts to wafer structures with different process foundations, broadening the applicability of the process.

[0034] Reference Figure 5 As described in step S130, the chip array is subjected to photolithography and development processes to form a metal-plated window at the corresponding position of the pin of each chip.

[0035] It should be noted that the precise delineation of the growth area of ​​the bonding metal through photolithography provides accurate mask boundaries for subsequent electroless or electroplating. The final positional accuracy, dimensional tolerance, and morphological quality of the plated window directly determine the forming effect of the bonding metal, as well as the bonding alignment accuracy and connection reliability of the upper and lower electrodes. This process can directly reuse the temporary bonding photoresist layer formed in step S110 as the photolithography substrate, eliminating the need to remove the temporary bonding layer and recoat the photoresist. This simplifies the process steps, reduces process costs, avoids the cumulative errors caused by secondary coating and alignment, and ensures the alignment consistency between the plated window and the lower electrode pins.

[0036] In one embodiment of the present invention, the specific process of step S130, "performing photolithography and development on the chip array to form a metal plating window at the corresponding position of the pin of each chip," can be further described in conjunction with the following description.

[0037] As described in the following steps, the patterned wafer structure is sequentially exposed and developed to remove the photoresist outside the area corresponding to the electrode pins, and to form exposed metal plating windows at the preset bonding positions of the electrode pins. It should be noted that the two-step process of exposure and development to complete the photolithography patterning is designed to adapt to the material characteristics of negative photoresist: the exposed area of ​​the negative photoresist will undergo a polymer cross-linking reaction and solidify, and will not be dissolved in the developer. The unexposed area can be fully removed by the developer, thereby forming a precise exposed plating window at the preset bonding position of the electrode pin. The area outside the pin is covered and protected by the solidified photoresist.

[0038] This patterning method achieves micron-level window size control precision, with good edge steepness, enabling precise matching of the extremely small electrodes of micro-pitch chip arrays. This effectively avoids defects such as bonding misalignment and metal overflow short circuits caused by excessive window offset. At the same time, the cured and retained photoresist layer can also serve as a protective masking layer in subsequent plating processes, isolating the plating agent from contact with non-bonded areas of the wafer and preventing the agent from corroding other structures of the chip. After the bonding process is completed, the photoresist can be removed and cleaned uniformly, making the process flow smoother and more efficient.

[0039] Reference Figure 6 As described in step S140, a bonding metal is grown in the plating window using a chemical plating or electroplating process, and the metal bonding between the corresponding electrodes of the first wafer and the second wafer is achieved through the bonding metal.

[0040] It should be noted that, unlike traditional hot-press bonding and hybrid bonding which rely on high temperature and high pressure to cause plastic deformation of metal bumps, this solution forms the bonding structure in situ through metal deposition growth. The entire process can be completed at room temperature without the need for high pressure and high temperature environments. This avoids the adverse effects of high temperature thermal stress on the chip's optoelectronic performance and driving circuit characteristics, and also eliminates the risk of alignment misalignment caused by wafer warping at high temperatures.

[0041] Meanwhile, the in-situ grown bonding metal can fully fill the micro gaps between the upper and lower electrodes, adapting to high-density chip arrays with tiny pitches, achieving high-precision interconnection without pre-fabricating independent metal bumps, effectively simplifying process steps and lowering the threshold for process implementation.

[0042] In one embodiment of the present invention, the specific process of step S140, "growing bonding metal in the plating window using chemical plating or electroplating process, and realizing metal bonding between the corresponding electrodes of the first wafer and the second wafer through the bonding metal," can be further described in conjunction with the following description.

[0043] As described in the following steps, a bonding metal is grown within the plating window using a chemical plating or electroplating process; wherein the bonding metal is made of any one or more combinations of gold, silver, nickel, aluminum, copper, tin, and titanium; It should be noted that the two processes, electroless plating and electroplating, can be flexibly selected according to the production scenario and process requirements: electroless plating does not require external electrodes and is suitable for metal deposition on complex morphologies and non-conductive substrates, offering greater process compatibility; electroplating, on the other hand, has a faster deposition rate and higher metal density, meeting the high-efficiency process requirements of large-scale mass production. Bonding metals selected include commonly used metals in the semiconductor field such as gold, silver, nickel, aluminum, copper, tin, and titanium, which can be adapted to different electrode substrates and performance requirements: for example, copper has excellent electrical and thermal conductivity, which can reduce interconnect losses and improve device heat dissipation; gold has good oxidation resistance and chemical stability, which can improve the long-term reliability of devices; nickel and titanium can be used as barrier layer metals to suppress inter-metal diffusion, further enriching the process's adaptability scenarios; at the same time, the plating process can use liquid or gaseous agents, adapting to the process conditions of different process equipment.

[0044] As described in the following steps, the bonding metal forms a metal chemical bond with the metal layers of the electrodes on both sides, thereby achieving the bonding connection between the corresponding electrodes of the first wafer and the second wafer; It should be noted that the metal-chemical bonding formed through in-situ growth differs from the physical bonding interface of dissimilar metals in traditional hot-press bonding. The bonding interface is a metallurgical bond of homogeneous or compatible metals, resulting in higher interface strength, lower contact resistance, and lower thermal resistance. This ensures electrical stability under high current drive and effectively improves the heat dissipation capacity of the device, extending its overall service life. Furthermore, the chemically bonded interface avoids the brittle intermetallic compound problems that easily arise in dissimilar metal pressing, preventing the risk of interface degradation and connection failure under long-term operation, significantly improving the long-term reliability of chip array devices. Moreover, the metal growth process can effectively fill the tiny gaps and surface morphology deviations between electrodes, effectively reducing process defects such as poor connections and open circuits, and improving mass production yield.

[0045] In one embodiment of the present invention, the plating agent used in the chemical plating or electroplating process is a liquid agent or a gaseous agent.

[0046] It should be noted that liquid reagents are a conventional form of semiconductor plating process. The supporting equipment is highly mature, the plating rate is stable and controllable, and it is suitable for mass production of large-size wafers, which can ensure the uniformity and consistency of metal layer deposition. Gaseous reagents possess superior penetration and coverage capabilities, enabling uniform deposition deep within minute coating windows with high aspect ratios. They are particularly well-suited for micro-pitch, high-density chip array electrode structures, effectively preventing incomplete coating and poor sidewall coverage within these small windows. The compatible design of the two reagent forms allows this process to adapt to different precision levels and production scales, flexibly switching between process schemes without adjusting core process logic, significantly improving the process's adaptability and equipment compatibility.

[0047] In one embodiment of the present invention, the metal column is made of copper.

[0048] It should be noted that copper was chosen as the material for the metal pillars because copper has excellent electrical and thermal conductivity, which can effectively reduce the contact resistance and Joule heat loss of electrode interconnects, while improving the thermal conductivity of the bonding structure, improving the overall heat dissipation performance of the device, and ensuring the working stability of the chip array under high current drive. Copper exhibits excellent metallurgical compatibility with bonding metals grown through subsequent electroless or electroplating processes. Particularly in homogeneous copper plating schemes, it can form a dense metal interface, further reducing interfacial thermal resistance and electrical resistance, and improving bonding strength and long-term reliability. Furthermore, the copper pillar fabrication process is mature and manufacturing costs are controllable. Combined with a pillar design smaller than the lead size, high-density interconnects can be achieved in micro-pitch electrode arrays, while compensating for microscopic gaps between upper and lower wafer electrodes, reducing the risk of poor connections, and improving bonding yield.

[0049] In one embodiment of the present invention, the growth substrate of the first wafer is one of sapphire substrate, gallium arsenide substrate, indium phosphide substrate or silicon substrate.

[0050] It should be noted that sapphire substrates are currently the most mainstream epitaxial growth substrates for gallium nitride-based LED chips, possessing advantages such as stable crystal quality, high optical transmittance, and controllable manufacturing costs, ensuring the growth quality and optoelectronic performance of the chip's epitaxial layer. Furthermore, sapphire substrates are well-suited for laser lift-off processes: the laser can penetrate the sapphire substrate and act on the interface between the substrate and the epitaxial layer, achieving low-temperature, non-destructive lift-off of the substrate by decomposing the interface material. The lift-off process does not cause thermal damage to the active area and electrode structure of the chip, nor does it compromise the alignment accuracy and structural stability of the temporary bonding layer. This aligns perfectly with the process logic of the back-side fabrication after temporary bonding in this solution. The resulting electrode surface is flat and clean, allowing direct entry into subsequent etching and plating processes.

[0051] In one embodiment of the present invention, the second wafer is a wafer integrating a complementary metal-oxide-semiconductor driving circuit.

[0052] It should be noted that the wafer integrating complementary metal-oxide-semiconductor (CMOS) driver circuitry is the core of the chip array's drive control, enabling independent addressing, power supply regulation, and brightness adjustment of each pixel unit within the chip array, supporting the normal light emission and display functions of the chip array. This process achieves direct bonding between the first wafer and the second driver wafer through room-temperature in-situ metal growth, significantly shortening the electrode interconnection path, reducing parasitic inductance and resistance, and improving the transmission speed and stability of the drive signal. This meets the performance requirements of high-density, high-refresh-rate optoelectronic chip arrays in fields such as co-packaged optics and augmented reality glasses. Simultaneously, the room-temperature bonding process does not cause thermal stress damage to the semiconductor devices inside the driver wafer, effectively ensuring the performance stability and production yield of the driver circuitry, achieving high-performance and high-reliability integration of the light-emitting unit and the driver circuitry.

[0053] In one embodiment of this application, a chip array device is also proposed, which is fabricated using the chip array bonding process described in any of the above embodiments.

[0054] It should be noted that the chip array device in this embodiment is fabricated using the aforementioned bonding process, fully inheriting the structural and performance advantages brought by this process. The chip array and the driving wafer electrodes inside the device form a metallurgical-grade chemical bond through in-situ grown bonding metal. The bonding interface has high bonding strength and low contact resistance and contact thermal resistance, which can not only ensure the stability of electrical transmission under high current drive and reduce interconnection loss and heat generation, but also effectively improve the overall heat dissipation capacity of the device, avoid problems such as interface degradation and connection failure under long-term operation, and significantly extend the service life and operational reliability of the device.

[0055] Meanwhile, since the bonding process is completed at room temperature, it avoids the thermal stress damage caused by traditional high-temperature bonding processes. The optoelectronic properties of the chip and the electrical characteristics of the driving circuit are fully preserved, resulting in better consistency of optoelectronic parameters and higher mass production yield. This process can achieve micron-level high-precision electrode interconnection, support chip pixel array integration with smaller pitch, and can fabricate chip array devices with higher resolution and higher integration. It can fully adapt to the application requirements of high-density, high-performance chip arrays in fields such as co-packaged optical modules and augmented reality glasses. Moreover, the process steps are simplified and the equipment compatibility is strong, which can effectively control the manufacturing cost of the device and adapt to the needs of large-scale mass production.

[0056] Although preferred embodiments of the present application have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of the embodiments of the present application.

[0057] Finally, it should be noted that in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or terminal device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or terminal device. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or terminal device that includes said element.

[0058] The chip array bonding process method and device provided in this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A chip array bonding process method, characterized in that, Including the following steps: A first wafer carrying several chip arrays is aligned and bonded to a second wafer with corresponding electrode arrays, and the first wafer and the second wafer are temporarily bonded together by a photoresist layer; The growth substrate of the first wafer is removed, and the first wafer is patterned and etched to obtain multiple independent chip arrays. The chip array is subjected to photolithography and development processes to form a metal-plated window at the corresponding position of the pin of each chip; A bonding metal is grown within the plating window using a chemical plating or electroplating process, and the metal bonding between the corresponding electrodes of the first wafer and the second wafer is achieved through the bonding metal.

2. The method according to claim 1, characterized in that, The step of aligning and bonding a first wafer carrying a chip array with a second wafer having a corresponding electrode array, and temporarily bonding the first wafer and the second wafer together using a photoresist layer, includes: The photoresist layer is formed using negative photoresist as a temporary bonding medium, and the first wafer and the second wafer are aligned and bonded according to the electrode correspondence. The first wafer and the second wafer are bonded using a wafer-to-wafer bonding mode or a chip-to-wafer bonding mode.

3. The method according to claim 1, characterized in that, The step of removing the growth substrate of the first wafer and performing pattern etching on the first wafer to form a plurality of independent chip arrays includes: The growth substrate of the first wafer is removed by laser lift-off process to reduce chip thickness; The first wafer is patterned by inductively coupled plasma etching to form multiple independent chip arrays; wherein, metal pillars are pre-set on the electrode pins of the first wafer and / or the electrodes of the second wafer, and the lateral dimension of the metal pillars is smaller than the lateral dimension of the electrode pins.

4. The method according to claim 1, characterized in that, The step of performing photolithography and development on the chip array to form a metal-plated window at the corresponding position of each chip pin includes: The patterned wafer structure is subjected to exposure and development processes in sequence to remove the photoresist outside the area corresponding to the electrode pins, and to form exposed metal plating windows at the preset bonding positions of the electrode pins.

5. The method according to claim 1, characterized in that, The step of growing bonding metal in the plating window using chemical plating or electroplating, and achieving metal bonding between the corresponding electrodes of the first wafer and the second wafer through the bonding metal, includes: A bonding metal is grown within the plating window using a chemical plating or electroplating process; wherein the bonding metal is any one or more combinations of gold, silver, nickel, aluminum, copper, tin, and titanium. The bonding metal forms a metal chemical bond with the metal layers of the electrodes on both sides, thereby achieving the bonding connection between the corresponding electrodes of the first wafer and the second wafer.

6. The method according to claim 1, characterized in that, The plating agents used in the electroless plating or electroplating process are liquid or gaseous agents.

7. The method according to claim 3, characterized in that, The metal column is made of copper.

8. The method according to claim 1, characterized in that, The growth substrate of the first wafer is one of sapphire substrate, gallium arsenide substrate, indium phosphide substrate or silicon substrate.

9. The method according to claim 1, characterized in that, The second wafer is a wafer with integrated complementary metal-oxide-semiconductor driving circuitry.

10. A chip array device, characterized in that, The chip array device is fabricated using the chip array bonding process described in any one of claims 1 to 9.