Method for manufacturing oily dispersions and cosmetics containing oily dispersions

By using specific compound treatment agents and non-organosilicon oils to disperse inorganic oxide powders at high temperatures, the problem of dispersing inorganic oxide powders in oily dispersions has been solved, achieving uniform dispersion at high solids concentrations and stability in cosmetics.

CN123076368APending Publication Date: 2026-11-10NIKKO CHEM
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202480090702.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-11
Filing Date
2024-11-25
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the existing technology, inorganic oxide powders are difficult to disperse in oily dispersions and require cumbersome hydrophobication treatment, which leads to poor preservation stability and makeup-holding properties of cosmetics.

Method used

Organosilicon compounds, higher fatty acids, carboxylic acid-modified organosilicon, and pyrrolidone carboxylic acid-modified organosilicon were used as treatment agents. The inorganic oxide powders that had not undergone hydrophobic treatment were heated and mixed at 40℃~120℃, dispersed using non-organosilicon oil agents, and further dispersed using a wet mixing disperser.

Benefits of technology

This technology enables uniform dispersion of inorganic oxide powders at high solids concentrations, improving the dispersibility and storage stability of cosmetics, eliminating the need for dispersants, and maintaining the user experience and stability of cosmetics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention provides a method for manufacturing an oily dispersion and a cosmetic containing the oily dispersion. The manufacturing method is a method for manufacturing an oily dispersion containing inorganic oxide powder and non-organosilicon oil, wherein the non-organosilicon oil contains at least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid modified organosilicon and pyrrolidone carboxylic acid modified organosilicon as a treatment agent. The manufacturing method comprises: a step (1) of adding inorganic oxide powder while heating the non-organosilicon oil containing the above-mentioned treatment agent at a temperature of 40°C to 120°C; and a step (2) of further mixing the dispersion after adding all the above-mentioned non-organosilicon oil and inorganic oxide powder at a temperature of 40°C to 120°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing an oily dispersion and cosmetics containing the oily dispersion. More specifically, this invention relates to a method for manufacturing an oily dispersion capable of effectively dispersing inorganic oxide powders in an oil even at high solids concentrations, and cosmetics containing the oily dispersion manufactured by this method. Background Technology

[0002] Generally, in oil-based dispersions used in cosmetics, the pigments used in foundations, eyeshadows, blushes, sunscreens, hair products, lotions, creams, and other basic cosmetics are already highly dispersed in an oily medium. Such oil-based dispersions for cosmetics are widely used due to their ease of use, resulting in less pigment dispersion and contamination during cosmetic preparation, and eliminating the need for specialized mixing equipment because the pigments are already highly dispersed.

[0003] On the other hand, inorganic oxide powders are difficult to disperse directly in oils due to their strong cohesive forces. Therefore, for pigments used in oil-based dispersions, hydrophobic treatments have been widely performed to facilitate the dispersion of inorganic oxide powders in oils. For example, methods are known to use higher fatty acids, higher alcohols, hydrocarbons, or organosilicones such as silicone oils and silicone resins to coat the pigment surface and thus impart hydrophobicity. Among these methods, numerous hydrophobic treatments of pigments using organosilicones as surface treatment agents have been established to date (see, for example, Japanese Patent Application Publication Nos. 60-163973 and 62-177070), and oil-based dispersions using these methods are widely known (see, for example, Japanese Patent Application Publication Nos. 2002-80748, 2005-171145, and 2011 / 007668).

[0004] Furthermore, because inorganic oxide powders have strong cohesive forces, in order to suppress re-agglomeration after dispersion and maintain dispersion stability, they are generally dispersed by adding organosilicon dispersants such as polyether-modified organosilicon or surfactants (for example, see Japanese Patent Application Publication No. 2007-291379 and Japanese Patent Application Publication No. 2012-184178). Summary of the Invention

[0005] However, the method of hydrophobizing inorganic oxide powders requires a pre-treatment process of surface treatment with a surface treatment agent before an oily dispersion can be produced, which is cumbersome and problematic.

[0006] In addition, when oily dispersions obtained by using dispersants, surfactants, etc. are incorporated into cosmetics, there is a risk that they may cause adverse effects such as reduced preservation stability and makeup hold-up of the cosmetics.

[0007] The present invention was made in view of the above-mentioned problems. The objective is to provide a method for manufacturing an oily dispersion and a cosmetic containing an oily dispersion manufactured by the method. The method does not require pre-treating the inorganic oxide powder to improve the dispersibility of the inorganic oxide powder in the oil. Furthermore, an oily dispersion with excellent dispersibility of the inorganic oxide powder can be obtained even without adding a dispersant.

[0008] To solve the aforementioned problems, the inventors conducted in-depth research and discovered that for non-organosilicon oils containing at least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid-modified organosilicon, and pyrrolidone carboxylic acid-modified organosilicon as a treatment agent, by heating at a temperature of 40°C to 120°C while adding unhydrophobically treated inorganic oxide powder, an oily dispersion with high powder dispersibility can be obtained, thus completing the present invention. Therefore, the oily dispersion of the present invention contains unhydrophobically treated inorganic oxide powder (component (A)), non-organosilicon oil (component (B)), and at least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid-modified organosilicon, and pyrrolidone carboxylic acid-modified organosilicon (component (C)).

[0009] One method for manufacturing an oily dispersion according to the present invention includes: a step (1) of adding inorganic oxide powder to a non-organosilicon oil agent while heating it at a temperature of 40°C to 120°C, wherein the oil agent contains at least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid modified organosilicon and pyrrolidone carboxylic acid modified organosilicon as a treatment agent; and a step (2) of further mixing the dispersion after adding all the amount of the inorganic oxide powder at a temperature of 40°C to 120°C.

[0010] In one embodiment of the method for manufacturing the oily dispersion of the present invention, it is preferable to use a mixing machine or a wet mixing and dispersing machine for dispersion in step (2) of the above-described manufacturing method.

[0011] One method for manufacturing the oily dispersion of the present invention includes: after all the steps including step (1) of adding inorganic oxide powder to a non-organosilicon oil containing at least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid modified organosilicon and pyrrolidone carboxylic acid modified organosilicon as a treatment agent at a temperature of 40°C to 120°C, and step (2) of further mixing the dispersion after adding all the amount of said inorganic oxide powder at a temperature of 40°C to 120°C, the oily dispersion is cooled and further dispersed using a wet mixing disperser.

[0012] In one embodiment of the method for manufacturing the oily dispersion of the present invention, it is preferred to manufacture it as follows: after step (2) of the above manufacturing method, the oily dispersion is preferably cooled to room temperature (20°C to 30°C) and further dispersed using a wet mixing disperser.

[0013] In the above-described manner of the present invention, it is preferable that the solid content concentration of the inorganic oxide powder during the manufacture of the oily dispersion is 25% by mass or more.

[0014] According to the present invention, the oily dispersion comprises an unhydrophobically treated inorganic oxide powder (component (A)), a non-organosilicone oil (component (B)), and at least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid-modified organosilicon, and pyrrolidone carboxylic acid-modified organosilicon (component (C)), and component (A) is uniformly or substantially uniformly dispersed at a solids concentration of 25% by mass or more. Here, uniform or substantially uniform dispersion includes the following cases: the dispersed particles in the oily dispersion are uniform and no aggregation is observed, and the dispersed particles in the oily dispersion are substantially uniform but slight aggregation is observed. The solids concentration of component (A) is preferably 40% by mass or more and 80% by mass or less. Alternatively, the solids concentration of component (A) may be 40% by mass or more and 70% by mass or less.

[0015] Furthermore, the present invention relates to cosmetics formulated with the above-mentioned oily dispersion, or cosmetics formulated with an oily dispersion manufactured by the manufacturing method of the present invention. Detailed Implementation

[0016] Next, specific embodiments of the method for manufacturing the oily dispersion of the present invention and cosmetics containing the oily dispersion manufactured by the method will be described. It should be noted that in this specification, the range "X~Y" means "X or more and Y or less". Furthermore, unless otherwise stated, operations are carried out at room temperature (20°C to 30°C) and relative humidity 45 to 55%RH.

[0017] The method for manufacturing the oily dispersion of the present invention is a method for manufacturing an oily dispersion containing the following components (A) to (C): (A) an inorganic oxide powder that has not undergone hydrophobic treatment, (B) a non-organosilicon oil, and (C) at least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid modified organosilicon, and pyrrolidone carboxylic acid modified organosilicon. The manufacturing method comprises: a step (1) of heating the oil obtained by dissolving or dispersing component (C) in component (B) at a temperature of 40°C to 120°C while adding component (A) to the oil; and a step (2) of further mixing the dispersion after adding all the amount of component (A) at a temperature of 40°C to 120°C.

[0018] According to the present invention, by heating a non-organosilicon oil agent containing at least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid modified organosilicon and pyrrolidone carboxylic acid modified organosilicon as a treatment agent at a temperature of 40°C to 120°C while adding unhydrophobically treated inorganic oxide powder, an oily dispersion with high powder dispersibility and high solids concentration can be obtained, thereby enabling the production of cosmetics containing the oily dispersion.

[0019] The inorganic oxide powder used as component (A) of this invention, without hydrophobic treatment, is not particularly limited, and examples include inorganic oxides commonly used in cosmetics such as silicic anhydride (silicon oxide), alumina, iron oxide (red iron oxide, yellow iron oxide, black iron oxide, etc.), titanium oxide, zinc oxide, cerium oxide, and bismuth oxide. Partial inorganic oxides such as titanium oxide, zinc oxide, iron oxide, cerium oxide, and bismuth oxide, particularly for applications requiring UV shielding, can be used. These inorganic oxide powders can also be used in combination of two or more. However, all are made from inorganic oxide powders without hydrophobic treatment. Here, hydrophobic treatment refers to a treatment that imparts hydrophobicity by coating the surface of the inorganic oxide powder with organic substances such as higher fatty acids, higher alcohols, hydrocarbons, or silicone oils, silicone resins, etc.

[0020] The particle size of inorganic oxides is not particularly limited, for example, in the range of 0.001 to 50 μm. The particle size is based on volume and can be determined using a laser diffractometer.

[0021] The concentration of the inorganic oxide powder, which is component (A) of the present invention, in the oily dispersion is not particularly limited, but is preferably 25% by mass or more, more preferably 40-80% by mass, or 40-70% by mass. When the concentration of the inorganic oxide powder is less than 25% by mass, it is sometimes impossible to obtain an oily dispersion with good dispersibility of the inorganic oxide powder over time; when it exceeds 80% by mass, the powder may agglomerate and the dispersion itself may not be obtained.

[0022] In this invention, the non-organosilicon oil used as the dispersion medium for component (B) is not particularly limited as long as it is the medium for dispersing component (A) and is an oil without a polysiloxane skeleton, regardless of its source such as animal oil, vegetable oil, mineral oil, or its properties such as solid oil, semi-solid oil, liquid oil, or volatile oil. However, from the viewpoint of the dispersibility of component (A), liquid oil that is liquid at room temperature is preferred. For example, hydrocarbons, oils, hydrogenated oils, ester oils, and lanolin derivatives can be used. More specifically, examples include: liquid paraffin, light liquid isoalkanes, dodecane, isododecane, tetradecane, isotetradecane, hexadecane, isohexadecane, squalane, vegetable squalane, petrolatum, polyisobutylene, polybutene, and other hydrocarbons; octyl cetyl ester, isononyl isononanoate, isodecanyl isononanoate, isotridecyl isononanoate, tricyclodecane methyl isononanoate, (octyl / decanoic acid) cocoyl ester, hexyl laurate, methyl heptyl laurate, and octyl laurate. Decyl lauryl acid, isopropyl myristate, methyl heptyl myristate, 2-hexyl decyl myristate, octyl dodecyl myristate, isopropyl palmitate, methyl heptyl palmitate, 2-ethylhexyl palmitate, 2-ethylhexyl stearate, ethyl isostearate, isopropyl isostearate, isobutyl isostearate, decyl isostearate, methyl heptyl isostearate, 2-hexyl decyl isostearate, 2-ethylhexyl hydroxystearate, octyl dodecyl oleate, oleyl alcohol oleate, octyl dodecyl castor oil oleate, alkyl benzoate, glyceryl isostearate Monoester oils such as lipases; di(octanoic / capric)propylene glycol ester, neopentyl glycol diisononanoate, neopentyl glycol didecanoate, propylene glycol didecanoate, glyceryl diisostearate, polyglyceryl diisostearate, propylene glycol diisostearate, lauroyl glutamate di(phytosterol / octyldodecyl) ester, lauroyl glutamate di(cholesterol / behenol / octyldodecyl) ester, lauroyl glutamate di(octyldodecyl / phytosterol / behenol) ester, neopentyl dioctanoate, etc.; trimethylolpropane triisostearate, diglyceryl triisostearate, etc. The following are permitted oil types: esters, triglycerides (caprylic / capric), tricaprylic acid glycerides, macadamia nut oil, olive oil, castor oil, jojoba oil, avocado oil, sunflower seed oil, etc.; ester oils such as pentaerythritol tetracaprylate, diglycerol tetraisostearate, dipentaerythritol tetraisostearate, pentaerythritol tetraisostearate, etc.; oil-soluble UV absorbers such as ethylhexyl dimethyl para-aminobenzoate, ethylhexyl salicylate, ethylhexyl methoxycinnamate, octocrylene, dineoprothiolane-4'-methoxybenzyl malonate, etc. One or more of these may be used. Hydrocarbons and various ester oils are preferred.

[0023] In one aspect of the invention, the content of component (B) in the oily dispersion is not particularly limited, but is 20 to 70% by mass from the viewpoint of dispersibility, more preferably 25 to 65% by mass.

[0024] As a component (C) of the present invention, at least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid-modified organosilicon, and pyrrolidone carboxylic acid-modified organosilicon can be used as a treatment agent. Two or more of these can also be used in combination.

[0025] Examples of organosilicon compounds used as component (C) of this invention include silanizing agents or silane coupling agents that incorporate organic groups, such as tetramethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, tetraethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, isobutyltrimethoxysilane, n-decyltrimethoxysilane, n-octyltrimethoxysilane, octyltriethoxysilane, octadecyltrimethoxysilane, octadecyltrimethoxysilane, dimethylpolysiloxysilazane, triethoxysilylethylpolydimethylsiloxyethylpolydimethylsiloxane, triethoxysilylethylpolydimethylsiloxane, etc.

[0026] The higher fatty acids used as component (C) of the present invention are not particularly limited, but are generally fatty acids with 12 or more carbon atoms. Examples include lauric acid, myristic acid, palmitic acid, stearic acid, isostearic acid, palmitoleic acid, oleic acid, and linoleic acid. Isostearic acid, palmitoleic acid, oleic acid, and linoleic acid, which are liquid at room temperature, are preferred because they can reduce the viscosity of the oily dispersion.

[0027] The carboxylic acid-modified organosilicon, which is component (C) of the present invention, can be manufactured by known methods, such as the following: a method in which a dimethyl polysiloxane having Si-H groups and an unsaturated carboxylic acid ester compound undergo an addition reaction under a platinum catalyst, followed by saponification to obtain a carboxylic acid; a method in which a dimethyl polysiloxane having Si-H groups and an unsaturated carboxylic acid silyl ester or an allyloxy carboxylic acid silyl ester undergo an addition reaction under a platinum catalyst, followed by hydrolysis to obtain the target compound; and a method in which a biterminated carboxylic acid-modified organosilicon is obtained by equilibration reaction using bis(hydroxycarbonylethyl)tetramethyldisiloxane and a cyclic siloxane and an acidic catalyst (Organosilicon Handbook, edited by Kunio Ito, Nikkan Kogyo Shimbun, pp. 166-167), etc. Furthermore, ES-5800 Formulation Aid (manufactured by Dow Toray Corporation) is a suitable carboxylic acid-modified organosilicon for the present invention.

[0028] The pyrrolidone carboxylic acid modified organosilicon, which is component (C) of the present invention, refers to a compound in which a portion of the polymethylsiloxane is a methyl (N-alkyl-pyrrolidone carboxylic acid)siloxane or a di (N-alkyl-pyrrolidone carboxylic acid)siloxane, and is described as "PCA DIMETHICONE" in the International Nomenclature of Cosmetic Ingredients (INCI). Furthermore, a suitable pyrrolidone carboxylic acid modified organosilicon for the present invention is, for example, SENSASIL PCA-LQ-(AP) (Croda Japan).

[0029] In one embodiment of the present invention, the amount of component (C) in the oily dispersion is not particularly limited, but is preferably in the range of 1 to 10 parts by mass when the concentration of the inorganic oxide powder is set to 100 parts by mass. When the amount is less than 1 part by mass, the inorganic oxide powder may not be uniformly dispersed in the non-organosilicon oil; when it exceeds 10 parts by mass, the use of the oily dispersion in cosmetics may sometimes lead to a decrease in the user experience and stability of the cosmetics. It should be noted that when two or more components (C) are used, the viscosity of the oily dispersion of the present invention can be reduced.

[0030] The method for manufacturing the oily dispersion of the present invention is a manufacturing method performed in the following order of steps (1) and (2).

[0031] Process (1): In step (1), while heating the non-silicone oil containing at least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid-modified organosilicon, and pyrrolidone carboxylic acid-modified organosilicon as component (C) at a temperature of 40°C to 120°C, the entire target amount of inorganic oxide powder of component (A) is added to the non-silicone oil containing component (B). Here, it is preferable to add the inorganic oxide powder to the non-silicone oil slowly. That is, it is preferable not to add the entire amount of inorganic oxide powder at once, but to add it in multiple portions, for example, over a given addition time.

[0032] During the addition of inorganic oxide powder, the temperature of the non-organosilicon oil is preferably maintained within the aforementioned temperature range. It is preferable to use a suitable heating device for heating to maintain the temperature within the aforementioned range.

[0033] The addition time of inorganic oxide powder to non-organosilicon oil is, for example, 1 minute to 100 minutes.

[0034] As a method for dispersing the oil dispersion obtained in step (1), an example is the method of adding inorganic oxide powder while stirring the non-organosilicon oil agent using a mixer such as a homogenizer or disperser. As for the stirring speed, there is no particular limitation as long as the dispersion is good, for example, 1000 rpm to 5000 rpm.

[0035] Process (2): The oil dispersion obtained in step (1) above is further mixed at a temperature of 40°C to 120°C to obtain an oily dispersion. From the viewpoint of the dispersibility of inorganic oxide powder in non-organosilicon oils, the mixing time in step (2) is preferably 2 hours or more, and from the viewpoint of effect saturation, it is more preferably 2 to 10 hours, and even more preferably 2 to 5 hours. In step (2), a homogenizer, disperser, etc. may also be used for dispersion, but it is preferable to use a mixer that can apply higher shear force, such as a kneading mixer, Henschel mixer, roller mixer, extrusion mixer, propeller mixer, high-speed mixer, dissolver, Ultimizer (wet high-pressure micronizer), wet jet mill, colloid mill, Masscolloider (ultrafine particle mill), (wet) bead mill, sand mill, basket mill, AD mill, etc.

[0036] As for the temperature conditions during manufacturing in the above-mentioned steps (1) and (2), it is preferable to heat the non-silicone oil and oil dispersion to a temperature of 40°C to 120°C. Below 40°C, the inorganic oxide powder cannot be uniformly dispersed in the non-silicone oil, which is therefore not preferred. However, when using volatile hydrocarbon oils, it is preferable to proceed at a temperature below 60°C to prevent the hydrocarbon oil from evaporating. It should be noted that when the temperature exceeds 120°C, the yellow iron oxide and black iron oxide in the inorganic oxide powder may change color, which is also not preferred.

[0037] If, after the above steps (1) and (2), the oily dispersion is cooled and further dispersed, the inorganic oxide powder is further micronized, achieving a more uniform dispersion in the oil, which is therefore preferable. Cooling is preferably performed to below 40°C, and more preferably to room temperature (20°C to 30°C). Examples of cooling methods include: a method of allowing natural cooling while continuously stirring; and a method of cooling the oily dispersion using a cooling device while maintaining continuous stirring. From the viewpoint of improving the dispersibility of the inorganic oxide powder in the oily dispersion, the disperser used for dispersion after cooling is preferably a wet mixing disperser, and more preferably a wet bead mill. Specific examples of wet mixing dispersers are described above. The dispersion time in the dispersion after cooling is, for example, 15 minutes to 5 hours, or 30 minutes to 3 hours.

[0038] Next, the cosmetic of the present invention will be described. The cosmetic of the present invention, by incorporating an oily dispersion prepared using the above-described manufacturing method, can produce sunscreens and other cosmetics that, despite having a high concentration of solid components, exhibit good stability over time, and thus possess high SPF values ​​and high transparency. Specific examples of the cosmetic include color cosmetics such as foundation, eyeshadow, and blush, sunscreens, hair care products, and basic cosmetics such as lotions and creams. The amount of the oily dispersion incorporated into the cosmetic is not particularly limited, but is preferably 0.1 to 90% by mass.

[0039] Furthermore, in the cosmetics of the present invention, ingredients commonly used in cosmetics, such as powders, surfactants, oils, gelling agents, polymers, beauty ingredients, moisturizers, pigments, preservatives, fragrances, etc., may be used to a extent that does not impair the effects of the present invention.

[0040] The cosmetic product of this invention can be in any form, such as powder, lotion, cream, stick, solid, spray, or multi-layer separation type.

[0041] Example

[0042] Next, the present invention will be described in more detail based on examples and comparative examples of oily dispersions manufactured by the manufacturing method of the present invention and cosmetics containing such oily dispersions, but the present invention is not limited to the following examples.

[0043] (Example 1)

[0044] 1.2 g of isostearic acid (RADIACID 0909, manufactured by Oleon) and 38.8 g of squalane were mixed and heated to 60°C. After confirming that the temperature had reached 60°C, 60 g of titanium dioxide (MP-1133, manufactured by TAYCA) was added in small, frequent additions over 10 minutes while stirring with a disperser at 2000 rpm. After the total amount of titanium dioxide was added, the mixture was further stirred at 2000 rpm for 3 hours at 60°C to obtain an oily dispersion of titanium dioxide with a solid content of 60% by mass.

[0045] (Example 2)

[0046] In Example 1, red iron oxide (R-516HP, manufactured by Titanium Industries) was used instead of titanium oxide. Otherwise, the same procedure was performed to obtain an oily dispersion of red iron oxide with a solid content concentration of 60% by mass.

[0047] (Example 3)

[0048] In Example 1, yellow iron oxide (LL-100HP, manufactured by Titanium Industries) was used instead of titanium oxide. Otherwise, the same procedure was performed to obtain an oily dispersion of yellow iron oxide with a solid content concentration of 60% by mass.

[0049] (Example 4)

[0050] In Example 1, black iron oxide (BL-100HP, manufactured by Titanium Industries) was used instead of titanium oxide. Otherwise, the same procedure was performed to obtain an oily dispersion of black iron oxide with a solid content concentration of 60% by mass.

[0051] (Example 5)

[0052] The oily dispersion obtained in Example 1 was allowed to cool to room temperature (25°C) while being stirred. It was then further dispersed and mixed for 1 hour using a wet bead mill (Shinmaru Enterprises DYNO-MILL) at a peripheral speed of 10 m / s, using 0.5 mm zirconia beads, and a filling rate of 70%, to obtain an oily dispersion of titanium dioxide with a solid content of 60% by mass. The obtained oily dispersion exhibited good dispersibility during storage at high temperatures.

[0053] (Example 6)

[0054] 4 g of isostearic acid (RADIACID 0909, manufactured by Oleon) and 46 g of isododecane were mixed and heated to 50°C. After confirming the temperature reached 50°C, 50 g of particulate titanium dioxide (MT-100SA, manufactured by TAYCA) was added in small, frequent additions over 9 minutes while stirring at 2000 rpm using a disperser. After the complete amount of particulate titanium dioxide was added, the mixture was dispersed for 2 hours using a wet bead mill (Shinmaru Enterprises DYNO-MILL) at a peripheral speed of 10 m / s, Φ0.5 mm zirconium oxide beads, a 70% fill rate, and 50°C, to obtain an oily dispersion of particulate titanium dioxide with a solid content of 50% by mass. The obtained oily dispersion exhibited good dispersibility during high-temperature storage.

[0055] (Example 7)

[0056] Except that the heating temperature was changed to 90°C in Example 1, the same procedure was performed to obtain an oily dispersion of titanium dioxide with a solid content concentration of 60% by mass.

[0057] (Example 8)

[0058] 1.2 g of isostearic acid (RADIACID 0909, manufactured by Oleon) and 38.8 g of cetyl octanoate were mixed and heated to 60°C. After confirming that the temperature had reached 60°C, 60 g of titanium dioxide (MP-1133, manufactured by TAYCA) was added in small, frequent additions over 10 minutes while stirring with a disperser at 2000 rpm. After the total amount of titanium dioxide was added, the mixture was further stirred at 60°C for 3 hours to obtain an oily dispersion of titanium dioxide with a solid content of 60% by mass.

[0059] (Example 9)

[0060] In Example 8, tricaprylic acid glyceride was used instead of cetyl octanoate, and otherwise the same procedure was performed to obtain an oily dispersion of titanium dioxide with a solid content concentration of 60% by mass.

[0061] (Example 10)

[0062] 2 g of octyltriethoxysilane (triethoxyoctylsilane, AES-3083, manufactured by Shin-Etsu Chemical Co., Ltd.) and 58 g of light liquid isoalkanes were heated to 50°C. After confirming that the temperature had reached 50°C, 40 g of particulate zinc oxide (MZ-500, manufactured by TAYCA) was added in small, frequent additions over 8 minutes while stirring at 2000 rpm using a disperser. After the total amount of particulate zinc oxide had been added, the mixture was further stirred at 50°C for 3 hours to obtain an oily dispersion of particulate zinc oxide with a solid content concentration of 40% by mass.

[0063] (Example 11)

[0064] 1.4 g of octyltriethoxysilane (triethoxyoctylsilane, AES-3083, manufactured by Shin-Etsu Chemical Co., Ltd.) and 28.6 g of light liquid isoalkanes were heated to 40°C. After confirming that the temperature had reached 40°C, 70 g of zinc oxide (ZnO-SO5, manufactured by Sumitomo Osaka Cement Co., Ltd.) was added in small, frequent additions over 11 minutes while stirring at 2000 rpm using a disperser. After the total amount of zinc oxide was added, the mixture was further stirred at 40°C for 3 hours to obtain an oily dispersion of zinc oxide with a solid content concentration of 70% by mass.

[0065] (Example 12)

[0066] 1.2 g of octyltriethoxysilane (triethoxyoctylsilane, AES-3083, manufactured by Shin-Etsu Chemical Co., Ltd.) and 38.8 g of liquid paraffin were heated to 110°C. After confirming that the temperature had reached 110°C, 60 g of titanium dioxide (MP-1133, manufactured by TAYCA) was added in small, frequent additions over 10 minutes while stirring at 2000 rpm using a disperser. After the total amount of titanium dioxide was added, the mixture was further stirred at 110°C for 3 hours to obtain an oily dispersion of titanium dioxide with a solid content of 60% by mass.

[0067] (Example 13)

[0068] In Example 12, the heating temperature was changed to 120°C, but otherwise the same procedure was followed, resulting in an oily dispersion of titanium dioxide with a solid content concentration of 60% by mass.

[0069] (Example 14)

[0070] 2g of oleic acid and 58g of liquid paraffin were heated to 90°C. After confirming that the temperature had reached 90°C, 40g of micro-particle zinc oxide (MZ-500, manufactured by TAYCA) was added in small, frequent additions over 8 minutes while stirring with a disperser at 2000 rpm. After the entire amount of micro-particle zinc oxide had been added, the mixture was stirred further at 90°C for 3 hours to obtain an oily dispersion of micro-particle zinc oxide with a solid content concentration of 40% by mass.

[0071] (Example 15)

[0072] 1.0 g of isostearic acid (RADIACID 0909, manufactured by Oleon) and 59.0 g of ethylhexyl methoxycinnamate were mixed and heated to 50°C. After confirming that the temperature had reached 50°C, 40 g of titanium dioxide (MP-1133, manufactured by TAYCA) was added in small, frequent additions over 8 minutes while stirring with a disperser at 2000 rpm. After the total amount of titanium dioxide was added, the mixture was further stirred at 50°C for 3 hours to obtain an oily dispersion of titanium dioxide with a solid content of 40% by mass.

[0073] (Example 16)

[0074] 1.2 g of carboxylic acid-modified organosilicon (ES-5800 Formulation Aid, manufactured by Dow Toray) and 38.8 g of isododecane were mixed and heated to 50°C. After confirming that the temperature had reached 50°C, 60 g of titanium dioxide (MP-1133, manufactured by TAYCA) was added in small, frequent additions over 10 minutes while stirring with a disperser at 2000 rpm. After the total amount of titanium dioxide was added, the mixture was further stirred at 50°C with a disperser at 2000 rpm for 3 hours to obtain an oily dispersion of titanium dioxide with a solid content of 60% by mass.

[0075] (Example 17)

[0076] 1.2 g of pyrrolidone carboxylic acid-modified organosilicon (SENSASIL PCA-LQ-(AP), Croda Japan) and 38.8 g of isododecane were mixed and heated to 50°C. After confirming that the temperature had reached 50°C, 60 g of titanium dioxide (MP-1133, TAYCA) was added in small, frequent additions over 10 minutes while stirring with a disperser at 2000 rpm. After the total amount of titanium dioxide was added, the mixture was further stirred at 50°C with a disperser at 2000 rpm for 3 hours to obtain an oily dispersion of titanium dioxide with a solid content of 60% by mass.

[0077] (Comparative Example 1)

[0078] In Example 1, the temperature was changed from 60°C to 30°C, but otherwise the same procedure was followed, resulting in an oily dispersion of titanium dioxide with a solid content concentration of 60% by mass.

[0079] (Comparative Example 2)

[0080] Without using any treatment agents, 40g of squalane was heated to 60°C. After confirming that the temperature had reached 60°C, 60g of titanium dioxide (MP-1133, manufactured by TAYCA) was added in small, frequent additions over 10 minutes while stirring with a disperser at 2000 rpm. After the complete amount of titanium dioxide had been added, the mixture was further stirred at 60°C for 3 hours to obtain an oily dispersion of titanium dioxide with a solid content of 60% by mass.

[0081] (Comparative Example 3)

[0082] Without using a treatment agent, 40g of isododecane was heated to 50°C. After confirming that the temperature had reached 50°C, 60g of surface-treated titanium dioxide (OTS-2 CR-50, manufactured by Daito Kasei Corporation) was added in small, frequent additions over 10 minutes while stirring at 2000 rpm using a disperser. After adding all the surface-treated titanium dioxide, the mixture was further stirred at 50°C for 3 hours to obtain an oily dispersion of titanium dioxide with a solid content concentration of 60% by mass.

[0083] Next, the evaluation method for dispersion stability used in the examples will be described. The redispersibility (with sufficient shaking under particle sedimentation conditions) of samples that had been prepared for 1 day and samples that had been stored at 40°C for 1 month was visually observed.

[0084] Evaluation benchmark 1 day later

[0085] ○: The dispersed particles are uniform, and no aggregation was observed.

[0086] △: The dispersed particles are basically uniform, and slight agglomeration was observed.

[0087] ×: The dispersed particles are not uniform, and significant aggregation has been observed.

[0088] Evaluation benchmarks after 1 month

[0089] ○: The dispersed particles are uniform, and no aggregation was observed.

[0090] △: The dispersed particles are basically uniform, and slight agglomeration was observed.

[0091] ×: No redispersion of particles was observed; sedimentation or significant aggregation was observed.

[0092] The results of evaluating the oily dispersions of Examples 1-17 and Comparative Examples 1-3 using the above evaluation method are recorded in Table 1.

[0093]

[0094] The oily dispersions of Examples 1-17 of the present invention exhibited good dispersibility after one day of manufacturing and after storage at 40°C for one month. Furthermore, it is evident that the oily dispersions of the present invention demonstrate superior dispersibility, particularly over time, compared to the oily dispersions of Comparative Examples 1-3. Additionally, it is also evident that the oily dispersions of the present invention exhibit superior dispersibility over time compared to the case using pre-surface-treated inorganic oxide powders (Comparative Example 3).

[0095] (Example 18: Oil-based foundation)

[0096] The oil-based foundation was obtained by dispersing and mixing the formulations described in Table 2 using a homogenizer. The oil-based foundation of Example 18 exhibited good dispersion stability.

[0097]

[0098] (Example 19: Sunscreen)

[0099] The sunscreen was prepared according to the formulation described in Table 3 by the following method. The sunscreen of Example 19 exhibits good dispersion stability.

[0100]

[0101] (Preparation method)

[0102] Ingredients (1) to (5) were mixed. A pre-mixed and dissolved aqueous solution of ingredients (6) to (9) was added to the mixture while stirring with a homogenizer to obtain the target water-in-oil sunscreen.

[0103] The oil-based foundation of Example 18 and the sunscreen of Example 19 are cosmetics with good pigment dispersion stability.

[0104] Industrial applicability

[0105] The oily dispersion manufactured by the method of the present invention is characterized by high uniform dispersibility of easily agglomerated inorganic oxide powders in oils. Furthermore, this oily dispersion can provide cosmetics with good dispersion stability and has high industrial applicability.

Claims

1. A method for manufacturing an oily dispersion, comprising a method for manufacturing an oily dispersion containing the following components (A) to (C), (A) Inorganic oxide powders that have not undergone hydrophobication treatment; (B) Non-silicone oils, (C) At least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid-modified organosilicon, and pyrrolidone carboxylic acid-modified organosilicon. This manufacturing method has the following characteristics: Step (1) involves heating an oil obtained by dissolving or dispersing component (C) in component (B) at a temperature of 40°C to 120°C while simultaneously adding component (A) to the oil; and (2) A further mixing process is performed on the dispersion after the addition of the full amount of component (A) at a temperature of 40°C to 120°C.

2. The method for manufacturing an oily dispersion according to claim 1, wherein, The concentration of solid components (A) in the oily dispersion is 25% by mass or more.

3. The method for manufacturing an oily dispersion according to claim 1 or 2, wherein, In the process (2), a mixing machine or a wet mixing and dispersing machine is used for mixing.

4. The method for manufacturing an oily dispersion according to claim 1 or 2, wherein, After step (2), the oily dispersion is cooled and further dispersed using a wet mixing disperser.

5. The method for manufacturing an oily dispersion according to claim 3, wherein, After all the steps of the manufacturing method described in claim 3, the oily dispersion is cooled and further dispersed using a wet mixing and dispersing machine.

6. A cosmetic product comprising an oily dispersion manufactured by the manufacturing method of claim 1 or 2.

7. A cosmetic product comprising an oily dispersion manufactured by the manufacturing method of claim 3.

8. A cosmetic product comprising an oily dispersion manufactured by the manufacturing method of claim 4.

9. A cosmetic product comprising an oily dispersion manufactured by the manufacturing method of claim 5.

10. An oily dispersion comprising: (A) Inorganic oxide powders that have not undergone hydrophobication treatment; (B) Non-silicone oils, (C) At least one compound selected from organosilicon compounds, higher fatty acids, carboxylic acid-modified organosilicon, and pyrrolidone carboxylic acid-modified organosilicon. in, The component (A) is uniformly or substantially uniformly dispersed at a solid content concentration of 25% by mass or more.

11. The oily dispersion according to claim 10, wherein, The concentration of solid components in component (A) is 40% by mass or more and 80% by mass or less than that of the oily dispersion. The content of component (B) is 20-70% by mass of the oily dispersion. The content of component (C) is 1 to 10 parts by mass relative to 100 parts by mass of component (A).

12. A cosmetic product comprising the oily dispersion of claim 10 or 11.

Citation Information

Patent Citations

  • Production of hydrophobic powder

    JP1985163973A

  • Coloring solution

    JP1987177070A

  • Powder oily dispersion having ultra dispersion stability and cosmetic formulated with the same

    JP2002080748A

  • Disperse composition and cosmetic in which the same composition is formulated

    JP2005171145A

  • Treated metal-oxide powder, and metal-oxide dispersion by using the same

    JP2007291379A