Granulation process of a food deoxidizer
By using dry or semi-dry extrusion granulation technology, combined with dendritic silica and polyamide modification, the high energy consumption and oxidation of active components in traditional deoxidizer granulation processes have been solved, achieving efficient and low-loss deoxidizer particle preparation to meet the rapid oxygen absorption requirements of food packaging.
Patent Information
- Application Number
- CN202611393693.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing food deoxidizer granulation processes suffer from high energy consumption, large equipment investment, long production cycles, easy oxidation of deoxidizing active components, and low porosity, making it difficult to meet the needs of food packaging for rapid oxygen absorption.
The dry or semi-dry process, characterized by extrusion granulation and rapid prototyping, utilizes the physical or chemical reactions initiated during the mixing process of polyamide-derived dendritic silica/calcium stearate, sodium chloride, calcium chloride, etc., to achieve efficient molding of deoxidizer powder. The construction of dendritic silica structure and hyperbranched polyamide polymer layer ensures particle porosity and strength.
It simplifies the production process, reduces energy consumption, improves the effective utilization rate and production efficiency of deoxidizer, ensures smooth oxygen flow, avoids oxidation of active components, and improves the finished product qualification rate and particle strength.
Smart Images

Figure CN123102233A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of food preservation technology, specifically a granulation process for a food deoxidizer. Background Technology
[0002] Reduced iron powder-based food deoxidizers are widely used in the preservation of pastries, nuts, and meat products. Currently, the mainstream preparation processes for granular deoxidizers are divided into two categories: wet spheronization granulation and semi-dry extrusion granulation. Wet spheronization requires a large amount of solvent, multiple spheronization processes, and subsequent high-temperature drying, resulting in a long process flow, high energy consumption, and large equipment investment. Furthermore, high-temperature drying easily causes pre-oxidation of the iron powder, reducing its deoxidizing activity, and also produces more fine powder and a lower granulation rate. Semi-dry extrusion granulation is a simpler process with less solvent usage, making it a preferred route for low-cost preparation of granular deoxidizers. However, existing semi-dry granulation systems still face several technical bottlenecks that are difficult to overcome simultaneously.
[0003] Compressed granulation technology: Due to the high-pressure impact molding process, the powder particles are extremely compressed, resulting in a significant reduction in the specific surface area of the resulting flaky deoxidizer, low internal porosity, and an overly dense structure. This severely limits the contact area between the deoxidizer and oxygen, making it difficult for oxygen to effectively penetrate into the particles. Consequently, the deoxidation reaction rate is significantly reduced, failing to meet the actual requirements of rapid oxygen absorption in food packaging. Simultaneously, the dense structure also limits the effective utilization rate of the deoxidizer, leading to a waste of active components.
[0004] Wet granulation technology: This process requires multiple granulation steps to obtain granules, but the resulting granules vary in size and require sieving and grading. The process is cumbersome and time-consuming. During granulation, the deoxidizer powder is constantly subjected to mechanical friction and shearing, and prolonged contact with moisture and salt can easily lead to unintended oxidation reactions of the active components (especially iron powder), resulting in a loss of deoxidizing performance and reduced product quality. Furthermore, a drying step is necessary after granulation to control the granule moisture content, increasing energy consumption and equipment investment, and extending the production cycle. Simultaneously, the granulation rate is low, with a large amount of fine powder failing to granulate effectively and requiring reprocessing, further reducing production efficiency.
[0005] Existing semi-dry deoxidizer granulation systems generally employ a simple compounding of inorganic salts and common binders, relying on free water within the system to achieve particle bonding and molding. However, the moisture distribution within the system is difficult to control evenly, easily leading to localized moisture accumulation. Iron powder exposed to locally high moisture environments will oxidize prematurely in the early stages of storage, causing a decrease in deoxidation capacity. Simultaneously, during extrusion, the powder pores are highly susceptible to collapse under pressure, resulting in pore blockage within the particles, increased resistance to oxygen diffusion, and a reduced deoxidation rate. If the extrusion intensity is reduced to retain porosity, the formed particles lack sufficient mechanical strength, making them prone to pulverization and breakage during subsequent hammering, screening, packaging, and conveying processes, generating a large amount of fine powder. This fine powder not only causes product loss but also leads to problems such as dust inclusions during heat sealing of packaging, black spot corrosion, and other issues. Summary of the Invention
[0006] The purpose of this invention is to provide a granulation process for food deoxidizers. This invention abandons the traditional high-pressure densification molding and cumbersome wet rolling process, and instead adopts a dry or semi-dry granulation technology characterized by "extrusion granulation-rapid molding" to achieve efficient and low-loss molding of deoxidizer powder.
[0007] The objective of this invention can be achieved through the following technical solutions: A granulation process for a food deoxidizer includes the following steps: Step 1: Construct a water-oil emulsion system with calcium stearate as the core and hexadecyltrimethylammonium bromide as the emulsifier. Urea is used to adjust the pH of the system. Tetraethyl orthosilicate undergoes hydrolysis and condensation at the water-oil interface, and a dendritic silica shell grows in situ on the surface of the calcium stearate particles to obtain dendritic silica / calcium stearate.
[0008] Step 2: Under the conditions of toluene solvent and nitrogen protection reflux, 3-aminopropyltriethoxysilane is used to undergo a silanization grafting reaction with the silanol groups on the surface of dendritic silica, introducing amino active sites on the surface of the composite particles to obtain modified dendritic silica / calcium stearate.
[0009] Step 3: The modified dendritic silica / calcium stearate surface amino groups are introduced by Michael addition reaction with methyl acrylate, followed by the addition of ethylenediamine for amidation reaction, and hyperbranched polyamide-amine is grafted onto the particle surface to obtain polyamidized dendritic silica / calcium stearate.
[0010] Step 4: Mix reduced iron powder, activated carbon, polyamide-derived dendritic silica / calcium stearate, superabsorbent resin, silica, sodium chloride, calcium chloride and water to obtain a deoxidized dry powder mixture; feed the deoxidized dry powder mixture into a roller extrusion granulation equipment and extrude it into granulated flakes.
[0011] Step 5: The granulation flakes are crushed using a high-speed hammer and then screened by a drum to obtain irregular particles of the target particle size; the particles are transferred into a sealed chamber isolated from oxygen for storage to finally obtain food oxygen absorber granules, thus completing the granulation process of the food oxygen absorber.
[0012] Furthermore, the specific preparation steps for dendritic silica / calcium stearate are as follows: Calcium stearate granules, hexadecyltrimethylammonium bromide, deionized water, and urea were stirred and dissolved to obtain an aqueous solution. Then, cyclohexane and isopropanol were mixed evenly to obtain an oil solution. The oil solution was added to the aqueous solution, and the mixture was stirred for 2-3 hours at 20-25℃ and 500-600 rpm to ensure complete emulsification. Then, 10-12 mL of tetraethyl orthosilicate was added dropwise through a constant pressure dropping funnel, and the mixture was stirred for another 0.5-0.6 hours. The mixture was then heated to 70-72℃ and stirred for another 20-22 hours. After the reaction was completed, the reaction system was cooled to room temperature and centrifuged at 10000-12000 rpm for 10-12 minutes. The product was washed 2-4 times with deionized water and ethanol, and then dried under vacuum at 60-70℃ for 1-2 hours to obtain dendritic silica / calcium stearate.
[0013] Furthermore, the ratio of calcium stearate granules, hexadecyltrimethylammonium bromide, deionized water, and urea is 50-52g: 4-6g: 120-130mL: 2.4-2.6g.
[0014] Furthermore, the ratio of cyclohexane to isopropanol is 120-130 mL: 0.92-0.95 mL.
[0015] Furthermore, the specific preparation steps for modified dendritic silica / calcium stearate are as follows: Dendritic silica / calcium stearate and toluene were stirred and mixed. Then, under nitrogen protection, 3-aminopropyltriethoxysilane was slowly added dropwise to the solution. The mixture was heated to 110-120℃ and refluxed for 12-14 h. After centrifugation at 10000-12000 r / min for 10-12 min, the crude product was collected. The product was washed 2-4 times with deionized water and ethanol and dried under vacuum at 60-70℃ for 1-2 h to obtain modified dendritic silica / calcium stearate.
[0016] Furthermore, the ratio of dendritic silica / calcium stearate, toluene, and 3-aminopropyltriethoxysilane is 1-2 g: 100-120 mL: 0.9-1.2 mL.
[0017] Furthermore, the specific preparation steps for polyamidized dendritic silica / calcium stearate are as follows: Modified dendritic silica / calcium stearate, methanol, and methyl acrylate were added to a reaction vessel and stirred for 22-24 hours at 20-25°C and 500-600 rpm. After centrifugation at 10000-12000 rpm for 10-12 minutes, the crude product was collected. The crude product was washed 3-5 times with methanol to remove unreacted methyl acrylate. After vacuum drying at 60-70°C for 1-2 hours, the product was transferred to methanol and ethylenediamine and reacted at 50-60°C for 24-26 hours. After centrifugation at 10000-12000 rpm for 10-12 minutes, the crude product was collected. After washing 3-5 times with methanol, the crude product was vacuum dried at 60-70°C for 1-2 hours to obtain polyamidized dendritic silica / calcium stearate.
[0018] Furthermore, the ratio of modified dendritic silica / calcium stearate, methanol, methyl acrylate and ethylenediamine is 1-1.2g:100-130mL:4-5mL:15-20mL.
[0019] Furthermore, the mass ratio of reduced iron powder, activated carbon, polyamide-derived dendritic silica / calcium stearate, superabsorbent resin, silica, sodium chloride, calcium chloride and water is 52-58:2-4:2-4:5-10:5-8:3-4:3-4:10-15.
[0020] The beneficial effects of this invention are: 1. This invention abandons the traditional high-pressure densification molding and cumbersome wet rolling process, and instead adopts a dry or semi-dry granulation technology characterized by "extrusion granulation-rapid molding" to achieve efficient and low-loss molding of deoxidizer powder. It utilizes the rapid physical or chemical reaction triggered by polyamide dendritic silica / calcium stearate, superabsorbent resin, sodium chloride, and calcium chloride during the mixing process to extrude the powder mixture into particles with a certain porosity and strength without external ultra-high pressure and subsequent long rolling and drying.
[0021] This process avoids the problems of sharp reduction in specific surface area and decreased reactivity caused by excessive extrusion in tableting and granulation. On the other hand, it greatly simplifies the cumbersome process of multiple rounding and long-term drying required in wet granulation, effectively shortens the production cycle, reduces energy consumption, and fundamentally reduces the performance loss of deoxygenating active components caused by prolonged contact with water and the introduction of oxygen through mechanical stirring during the wet process.
[0022] 2. This invention prepares polyamide-modified dendritic silica / calcium stearate functional additives and combines them with an integrated granulation method of semi-dry instantaneous extrusion and oxygen-free sealing and shaping. This method is completely different from the complex processes of traditional high-pressure tableting and wet rolling. This invention first grows a unique dendritic silica structure on the surface of calcium stearate. This multi-level branched pore structure has stronger compressive strength and is not easily crushed or blocked during granulation and extrusion. It solves the problems of ordinary silica having regular pores, easy water retention, and pore sealing failure after extrusion. It preserves the internal pores of the particles to the greatest extent and ensures that oxygen can enter and exit smoothly.
[0023] 3. This invention constructs a hyperbranched polyamide polymer functional layer on the surface of the functional additive through silane grafting, addition and amidation modification. During the powder mixing stage, the functional additive can uniformly lock in the moisture of the system and avoid local water accumulation that would cause premature oxidation and failure of the iron powder. During the extrusion granulation stage, a small amount of moisture can be released under mechanical pressure to help the iron powder and auxiliary materials to bond evenly and easily form granules.
[0024] 4. The polyamide-derived dendritic silica / calcium stearate of the present invention has a large number of active groups on its surface. During the particle shaping process, they can overlap and cross-link with each other to form a stable three-dimensional network structure inside the particle. This solves the problem of loose particles and easy powdering and shedding caused by the large number of pores in the traditional semi-dry granulation method. At the same time, it takes into account both high air permeability and high particle strength. The present invention does not require high pressure compaction, long-term rounding and high-temperature drying. The process is simpler and the production cycle is shorter. It significantly reduces production energy consumption and equipment costs, and effectively improves the one-time forming rate of particles and the qualified rate of finished products. Attached Figure Description
[0025] Figure 1 Image of the finished product from the granulation of food deoxidizer. Detailed Implementation
[0026] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0027] Example 1: A granulation process for a food deoxidizer, comprising the following steps: S1: Dissolve 50g of calcium stearate granules, 4g of hexadecyltrimethylammonium bromide, 120mL of deionized water, and 2.4g of urea by stirring to obtain an aqueous solution; then mix 120mL of cyclohexane and 0.92mL of isopropanol to obtain an oil solution; add the oil solution to the aqueous solution and stir for 2h at 20℃ and 500r / min to fully emulsify it. Then add 10mL of tetraethyl orthosilicate dropwise through a constant pressure dropping funnel and continue stirring for 0.5h. Heat to 70℃ and continue stirring for 20h. After the reaction is complete, cool the reaction system to room temperature, centrifuge at 10000r / min for 10min, wash the product twice with deionized water and ethanol, and dry under vacuum at 60℃ for 1h to obtain dendritic silica / calcium stearate.
[0028] S2: Mix 1g of dendritic silica / calcium stearate with 100mL of toluene, and then slowly add 0.9mL of 3-aminopropyltriethoxysilane to the solution under nitrogen protection. Heat to 110℃ and reflux for 12h. Centrifuge at 10000r / min for 10min to collect the crude product. Wash the product twice with deionized water and ethanol, and dry it under vacuum at 60℃ for 1h to obtain modified dendritic silica / calcium stearate.
[0029] S3: 1g of modified dendritic silica / calcium stearate, 60mL of methanol and 4mL of methyl acrylate were added to a reaction vessel and stirred at 20℃ and 500r / min for 22h. After centrifugation at 10000r / min for 10min, the crude product was collected. The crude product was washed three times with methanol to remove unreacted methyl acrylate. After vacuum drying at 60℃ for 1h, the product was transferred to 40mL of methanol and 15mL of ethylenediamine and reacted at 50℃ for 24h. After centrifugation at 10000r / min for 10min, the crude product was collected. The crude product was washed three times with methanol and vacuum dried at 60℃ for 1h to obtain polyamidized dendritic silica / calcium stearate.
[0030] S4: Add 52g of reduced iron powder, 2g of activated carbon, 2g of polyamide-derived dendritic silica / calcium stearate, 5g of superabsorbent resin, 5g of silica, 3g of sodium chloride, 3g of calcium chloride and 10g of water into a mixer and stir thoroughly to achieve microscopic uniform dispersion of each component in a dry state, thus obtaining a deoxidized dry powder mixture.
[0031] S5: The deoxidized dry powder mixture is placed in a roller extrusion granulation equipment. Under the extrusion of the equipment, the originally dry powder is destroyed due to the instantaneous extrusion, and the water is released. The superabsorbent resin quickly absorbs the solution broken by physical extrusion and swells. Sodium chloride and calcium chloride absorb water and agglomerate, which produces stickiness at room temperature and binds the surrounding iron powder, activated carbon and other particles together, and quickly binds them into granulated flakes.
[0032] S6: The pellets are granulated by hammering with a spiked club at 1200 r / min, and then sieved through a 2 mm drum screen to obtain irregular particles. The irregular particles are placed in a sealed finished product chamber to isolate oxygen for storage and allow moisture to be reabsorbed, ensuring that the particles have sufficient strength and preventing the iron powder from reacting continuously, thus obtaining a food deoxidizer and completing the granulation process of the food deoxidizer.
[0033] Example 2: A granulation process for a food deoxidizer, comprising the following steps: S1: Dissolve 51g of calcium stearate granules, 5g of cetyltrimethylammonium bromide, 125mL of deionized water, and 2.5g of urea by stirring to obtain an aqueous solution; then mix 125mL of cyclohexane and 0.935mL of isopropanol to obtain an oil solution; add the oil solution to the aqueous solution and stir at 22.5℃ and 550r / min for 2.5h to fully emulsify it. Then add 11mL of tetraethyl orthosilicate dropwise through a constant pressure dropping funnel and continue stirring for 0.55h. Heat to 71℃ and continue stirring for 21h. After the reaction is complete, cool the reaction system to room temperature, centrifuge at 11000r / min for 11min, wash the product three times with deionized water and ethanol, and dry under vacuum at 65℃ for 1.5h to obtain dendritic silica / calcium stearate.
[0034] S2: Mix 1.5g of dendritic silica / calcium stearate with 110mL of toluene. Then, under nitrogen protection, slowly add 1.05mL of 3-aminopropyltriethoxysilane to the solution. Heat to 115℃ and reflux for 13h. Centrifuge at 11000r / min for 11min to collect the crude product. Wash the product three times with deionized water and ethanol. Dry under vacuum at 65℃ for 1.5h to obtain modified dendritic silica / calcium stearate.
[0035] S3: 1.1 g of modified dendritic silica / calcium stearate, 70 mL of methanol and 4.5 mL of methyl acrylate were added to a reaction vessel and stirred at 22.5 °C and 550 r / min for 23 h. After centrifugation at 11000 r / min for 11 min, the crude product was collected. The crude product was washed four times with methanol to remove unreacted methyl acrylate. After vacuum drying at 65 °C for 1.5 h, the product was transferred to 45 mL of methanol and 17.5 mL of ethylenediamine and reacted at 55 °C for 25 h. After centrifugation at 11000 r / min for 11 min, the crude product was collected. The crude product was washed four times with methanol and vacuum dried at 65 °C for 1.5 h to obtain polyamidized dendritic silica / calcium stearate.
[0036] S4: Add 55g of reduced iron powder, 3g of activated carbon, 3g of polyamide-derived dendritic silica / calcium stearate, 7.5g of superabsorbent resin, 6.5g of silica, 3.5g of sodium chloride, 3.5g of calcium chloride and 12.5g of water to a mixer and stir thoroughly to achieve microscopic uniform dispersion of each component in a dry state, thus obtaining a deoxidized dry powder mixture.
[0037] S5: The deoxidized dry powder mixture is placed in a roller extrusion granulation equipment. Under the extrusion of the equipment, the originally dry powder is destroyed due to the instantaneous extrusion, and the water is released. The superabsorbent resin quickly absorbs the solution broken by physical extrusion and swells. Sodium chloride and calcium chloride absorb water and agglomerate, which produces stickiness at room temperature and binds the surrounding iron powder, activated carbon and other particles together, and quickly binds them into granulated flakes.
[0038] S6: The granulated flakes are crushed by hammering with a spiked club at 1300 r / min, and then sieved through a 3 mm drum screen to obtain irregular granules. The irregular granules are placed in a sealed finished product chamber to isolate oxygen for storage and allow moisture to be reabsorbed, ensuring that the granules have sufficient strength and preventing the iron powder from reacting continuously, thus obtaining a food deoxidizer and completing the granulation process of the food deoxidizer.
[0039] Example 3: A granulation process for a food deoxidizer, comprising the following steps: S1: 52g of calcium stearate granules, 6g of hexadecyltrimethylammonium bromide, 130mL of deionized water and 2.6g of urea were stirred and dissolved to obtain an aqueous solution; then 130mL of cyclohexane and 0.95mL of isopropanol were mixed evenly to obtain an oil solution; the oil solution was added to the aqueous solution and stirred at 25℃ and 600r / min for 3h to fully emulsify it. Then, 12mL of tetraethyl orthosilicate was added dropwise through a constant pressure dropping funnel, and stirring was continued for 0.6h. The mixture was heated to 72℃ and stirred for 22h. After the reaction was completed, the reaction system was cooled to room temperature, centrifuged at 12000r / min for 12min, and the product was washed 4 times with deionized water and ethanol and dried under vacuum at 70℃ for 2h to obtain dendritic silica / calcium stearate.
[0040] S2: Mix 2g of dendritic silica / calcium stearate with 120mL of toluene. Then, under nitrogen protection, slowly add 1.2mL of 3-aminopropyltriethoxysilane to the solution. Heat to 120℃ and reflux for 14h. Centrifuge at 12000r / min for 12min to collect the crude product. Wash the product four times with deionized water and ethanol. Dry under vacuum at 70℃ for 2h to obtain modified dendritic silica / calcium stearate.
[0041] S3: 1.2 g of modified dendritic silica / calcium stearate, 80 mL of methanol and 5 mL of methyl acrylate were added to a reaction vessel and stirred at 25 °C and 600 r / min for 24 h. After centrifugation at 12000 r / min for 12 min, the crude product was collected. The crude product was washed 5 times with methanol to remove unreacted methyl acrylate. After vacuum drying at 70 °C for 2 h, the product was transferred to 50 mL of methanol and 20 mL of ethylenediamine and reacted at 60 °C for 26 h. After centrifugation at 12000 r / min for 12 min, the crude product was collected. The crude product was washed 5 times with methanol and vacuum dried at 70 °C for 2 h to obtain polyamidized dendritic silica / calcium stearate.
[0042] S4: Add 58g of reduced iron powder, 4g of activated carbon, 4g of polyamide-derived dendritic silica / calcium stearate, 10g of superabsorbent resin, 8g of silica, 4g of sodium chloride, 4g of calcium chloride and 15g of water into a mixer and stir thoroughly to achieve microscopic uniform dispersion of each component in a dry state, so as to obtain a deoxidized dry powder mixture.
[0043] S5: The deoxidized dry powder mixture is placed in a roller extrusion granulation equipment. Under the extrusion of the equipment, the originally dry powder is destroyed due to the instantaneous extrusion, and the water is released. The superabsorbent resin quickly absorbs the solution broken by physical extrusion and swells. Sodium chloride and calcium chloride absorb water and agglomerate, which produces stickiness at room temperature and binds the surrounding iron powder, activated carbon and other particles together, and quickly binds them into granulated flakes.
[0044] S6: The pellets are granulated by hammering with a spiked club at 1400 r / min, and then sieved through a 4 mm drum screen to obtain irregular granules. The irregular granules are placed in a sealed finished product chamber to isolate oxygen for storage and allow moisture to be reabsorbed, ensuring that the granules have sufficient strength and preventing the iron powder from reacting continuously, thus obtaining a food deoxidizer and completing the granulation process of the food deoxidizer.
[0045] Comparative Example 1: Based on Example 3, the polyamidized dendritic silica / calcium stearate in step S4 was omitted.
[0046] Comparative Example 2: Based on Example 3, the polyamidized dendritic silica / calcium stearate in step S4 was replaced with the modified dendritic silica / calcium stearate in step S2.
[0047] Comparative Example 3: Based on Example 3, the polyamidized dendritic silica / calcium stearate in step S4 was replaced with the dendritic silica / calcium stearate in step S1.
[0048] The performance of the food oxygen absorbers prepared in Examples 1-3 and Comparative Examples 1-3 was tested. The oxygen absorbers were placed in food packaging bags at a concentration of 1.3% of the food mass. The packaging bags were then placed at 25-28°C for 2 days, and the oxygen absorption rate was tested. The bags were then stored at 25-28°C for 3 months, and the moisture regain rate was tested. The specific oxygen absorption rate and moisture regain rate results are shown in Table 1. Table 1
[0049] As shown in Table 1, Comparative Example 1 directly removed the polyamide-derived dendritic silica / calcium stearate functional additive. The system lacked a structure capable of regulating moisture and reinforcing particles, resulting in uneven moisture distribution during powder mixing, easily leading to localized water accumulation and premature oxidation and deactivation of the reduced iron powder. Simultaneously, during extrusion granulation, the powder pores were easily collapsed, making it difficult for oxygen to enter the particle interior and hindering the deoxidation reaction. Furthermore, the inability to form a cross-linked structure within the particles resulted in low particle strength, easy pulverization and powder loss in the finished product, ultimately reducing the oxygen absorption capacity of the final product. Moisture in the system easily migrated outwards, causing severe rehydration of the preserved food.
[0050] In Comparative Example 2, the polyamide-modified dendritic silica / calcium stearate was replaced with only amino-modified dendritic silica / calcium stearate without a grafted polyamide layer. While this additive retained the dendritic structure, which could protect the pores from compression and blockage to some extent, it lacked a surface polyamide functional layer, thus failing to achieve controllable water-locking and water-releasing effects, and also lacking strong cross-linking and toughening capabilities. The powder system still exhibited localized moisture accumulation issues, and the iron powder underwent slight premature oxidation, resulting in a loosely structured and insufficiently strong molded particles.
[0051] In Comparative Example 3, the polyamide-derived dendritic silica / calcium stearate was replaced with dendritic silica / calcium stearate. This material only possesses a basic porous structure and lacks amino and polyamide active functional groups on its surface. Therefore, it cannot uniformly stabilize the moisture content of the system, nor can it crosslink and reinforce the particles after extrusion molding. The problem of uneven moisture distribution in the system is more severe, the premature oxidation of iron powder is higher, the granulated product is most prone to pulverization and powder loss, and the deoxidation stability is poor.
[0052] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the invention.
Claims
1. A granulation process for a food deoxidizer, characterized in that, Includes the following steps: Step 1: Construct a water-oil emulsion system with calcium stearate as the core and hexadecyltrimethylammonium bromide as the emulsifier. Urea is used to adjust the pH of the system. Tetraethyl orthosilicate undergoes hydrolysis and condensation at the water-oil interface, and a dendritic silica shell grows in situ on the surface of the calcium stearate particles to obtain dendritic silica / calcium stearate. Step 2: Under the conditions of toluene solvent and nitrogen protection reflux, 3-aminopropyltriethoxysilane is used to undergo a silanization grafting reaction with the silanol groups on the surface of dendritic silica to introduce amino active sites on the surface of composite particles, thereby obtaining modified dendritic silica / calcium stearate. Step 3: ester groups are introduced by Michael addition reaction between the amino groups on the surface of modified dendritic silica / calcium stearate and methyl acrylate, followed by the addition of ethylenediamine for amidation reaction, and hyperbranched polyamide-amine is grafted onto the particle surface to obtain polyamidized dendritic silica / calcium stearate. Step 4: Mix reduced iron powder, activated carbon, polyamide-derived dendritic silica / calcium stearate, superabsorbent resin, silica, sodium chloride, calcium chloride and water to obtain a deoxidized dry powder mixture; feed the deoxidized dry powder mixture into a roller extrusion granulation equipment and extrude it into granulated flakes. Step 5: The granulation flakes are crushed using a high-speed hammer and then screened by a drum to obtain irregular particles of the target particle size; the particles are transferred into a sealed chamber isolated from oxygen for storage to finally obtain food oxygen absorber granules, thus completing the granulation process of the food oxygen absorber.
2. The granulation process for a food deoxidizer according to claim 1, characterized in that, The mass ratio of the reduced iron powder, activated carbon, polyamide-derived dendritic silica / calcium stearate, superabsorbent resin, silica, sodium chloride, calcium chloride and water is 52-58:2-4:2-4:5-10:5-8:3-4:3-4:10-15.
3. The granulation process for a food deoxidizer according to claim 1, characterized in that, The specific preparation steps for the dendritic silica / calcium stearate are as follows: Calcium stearate granules, hexadecyltrimethylammonium bromide, deionized water, and urea were stirred and dissolved to obtain an aqueous solution. Then, cyclohexane and isopropanol were mixed evenly to obtain an oil solution. The oil solution was added to the aqueous solution, and the mixture was stirred for 2-3 hours at 20-25℃ and 500-600 rpm to ensure complete emulsification. Then, 10-12 mL of tetraethyl orthosilicate was added dropwise through a constant pressure dropping funnel, and the mixture was stirred for another 0.5-0.6 hours. The mixture was then heated to 70-72℃ and stirred for another 20-22 hours. After the reaction was completed, the reaction system was cooled to room temperature and centrifuged at 10000-12000 rpm for 10-12 minutes. The product was washed 2-4 times with deionized water and ethanol, and then dried under vacuum at 60-70℃ for 1-2 hours to obtain dendritic silica / calcium stearate.
4. The granulation process for a food deoxidizer according to claim 3, characterized in that, The ratio of calcium stearate granules, hexadecyltrimethylammonium bromide, deionized water, and urea is 50-52g: 4-6g: 120-130mL: 2.4-2.6g.
5. The granulation process for a food deoxidizer according to claim 3, characterized in that, The ratio of cyclohexane to isopropanol is 120-130 mL: 0.92-0.95 mL.
6. The granulation process for a food deoxidizer according to claim 1, characterized in that, The specific preparation steps for the modified dendritic silica / calcium stearate are as follows: Dendritic silica / calcium stearate and toluene were stirred and mixed. Then, under nitrogen protection, 3-aminopropyltriethoxysilane was slowly added dropwise to the solution. The mixture was heated to 110-120℃ and refluxed for 12-14 h. After centrifugation at 10000-12000 r / min for 10-12 min, the crude product was collected. The product was washed 2-4 times with deionized water and ethanol and dried under vacuum at 60-70℃ for 1-2 h to obtain modified dendritic silica / calcium stearate.
7. The granulation process for a food deoxidizer according to claim 6, characterized in that, The ratio of dendritic silica / calcium stearate, toluene and 3-aminopropyltriethoxysilane is 1-2g: 100-120mL: 0.9-1.2mL.
8. The granulation process for a food deoxidizer according to claim 1, characterized in that, The specific preparation steps for the polyamidized dendritic silica / calcium stearate are as follows: Modified dendritic silica / calcium stearate, methanol, and methyl acrylate were added to a reaction vessel and stirred for 22-24 hours at 20-25°C and 500-600 rpm. After centrifugation at 10000-12000 rpm for 10-12 minutes, the crude product was collected. The crude product was washed 3-5 times with methanol to remove unreacted methyl acrylate. After vacuum drying at 60-70°C for 1-2 hours, the product was transferred to methanol and ethylenediamine and reacted at 50-60°C for 24-26 hours. After centrifugation at 10000-12000 rpm for 10-12 minutes, the crude product was collected. After washing 3-5 times with methanol, the crude product was vacuum dried at 60-70°C for 1-2 hours to obtain polyamidized dendritic silica / calcium stearate.
9. The granulation process for a food deoxidizer according to claim 8, characterized in that, The ratio of modified dendritic silica / calcium stearate, methanol, methyl acrylate and ethylenediamine is 1-1.2g:100-130mL:4-5mL:15-20mL.