Low-resistance high-density oxide target precursor and preparation method thereof

Through the combination of sand grinding method and grinding balls of different particle sizes, the grinding process of indium oxide precursor is optimized, and the problems of low density and large resistance of indium oxide precursor are solved, and the oxide target precursor with low resistance and high density are realized The preparation of the material significantly improves the overall performance.

CN118930227APending Publication Date: 2024-11-12XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD

Patent Information

Application Number
CN202411295106.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the indium oxide precursor has a low density and a large resistance. In addition, the mechanical ball milling method has insufficient research on improving the performance of the target material, so it is difficult to solve comprehensive performance problems such as plate warping through different proportions of grinding ball ratios.

Method used

The sand grinding method is used to combine grinding balls with different particle sizes. Through the sand grinding process optimization, the direct contact resistance and position barrier resistance between the powder are reduced, the density and dispersion of the precursor are improved, and the resistivity is reduced.

Benefits of technology

It effectively solves the agglomeration phenomenon, improves the density and dispersion of the precursor, significantly reduces the resistivity, and improves the comprehensive performance of the oxide target.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005045720040000101
    Figure BDA0005045720040000101
Patent Text Reader

Abstract

The invention belongs to the technical field of new materials, and discloses a preparation method of a low-resistance high-density oxide target precursor, which comprises the following steps of: sanding slurry containing an oxide precursor, and granulating; the oxide precursor contains not less than 97.5 wt% of indium oxide; the particle sizes of grinding balls used for sanding are 0.3 mm, 0.4 to 0.6 mm and 0.8 to 1.0 mm respectively; the mass ratio of the grinding balls of 0.3 mm to the grinding balls of 0.4-0.6 mm to the grinding balls of 0.8-1.0 mm is (4-7): (1-4): (1-4). According to the method, aiming at the target material with high indium oxide content, a sanding method is adopted and grinding balls with different particle sizes are matched to reduce gaps between precursor powder and reduce direct contact resistance and barrier resistance between the powder, and finally, the density of the precursor is improved, the resistance is reduced, and the agglomeration performance is improved. Meanwhile, the invention also provides a low-resistance high-density oxide target material precursor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new materials, and in particular to a low-resistance and high-density oxide target precursor and a preparation method thereof. Background Art

[0002] The excellent performance of indium oxide-based films is determined by high-density, low-resistivity indium oxide-based targets, and the source of the targets is the precursor powder. The dispersion, particle size, morphology and performance of the powder have an important influence on the film. At present, the methods for preparing powders can be roughly divided into six categories, namely liquid phase coprecipitation, hydrothermal method, solvothermal method, sol-gel method, spray pyrolysis method, and mechanical ball milling method. At present, the most frequently used methods for producing powders in industry are mainly liquid phase coprecipitation and mechanical ball milling. However, impurities such as chloride ions are easily introduced during the preparation process of liquid phase coprecipitation, and the washing process of impurities is quite troublesome, which not only increases costs, but also pollutes the environment and gradually declines. The mechanical ball milling method can be mass-produced at one time and can obtain powders of different particle sizes by controlling factors such as rotation speed and grinding medium diameter. The equipment is simple and easy to operate, and there is almost no pollution to the environment. With the increasing demand for target materials due to the development of science and technology, at present, at home and abroad, the production process of indium oxide-based target precursor powders is prepared by mechanical ball milling. However, it is found that the research on the production process of these new products, such as their particle size and performance, cannot keep up with the pace of development. Therefore, it is necessary to actively explore the influence of the production process of mechanical ball milling on indium oxide-based target precursor powders.

[0003] Mechanical ball milling, also known as high-energy ball milling, is a method of mixing raw materials and ball milling media into a ball mill container, using the gravitational potential energy of the grinding media and raw materials and the mechanical energy generated by the rotation and vibration of the ball mill to produce strong collisions and grinding between the raw materials, grinding media and the inner wall of the ball mill container, so that the raw materials are continuously ground into small particles and undergo solid phase transformation. Mechanical ball milling is mainly divided into dry ball milling and wet ball milling. Wet ball milling is currently the main ball milling method. Usually, water or organic solvent is added to the ball mill container as a reaction medium, and an appropriate amount of adhesive, dispersant, defoaming agent, etc. are added to the solid raw materials to ball mill into slurry. After filtering, washing and drying the slurry, a series of operations can be performed to prepare micron, submicron and even nanometer precursor powders.

[0004] In the applicant's prior application CN114853467B, an ITO planar target material and a preparation method thereof, a precursor powder is prepared by ball milling with a proportioned diameter of the ball milling, which is used to solve the problem of plate warping.

[0005] Plate warping is only one of the performance indicators of the target material. The comprehensive properties of the target material, such as resistivity, relative density, absolute density, and the probability of defect occurrence, cannot be solved simply by mixing different proportions of grinding balls.

[0006] The premise of improving the performance of the target material is to improve the performance of the precursor, such as the density and resistivity of the precursor. In the prior art, no technicians have conducted detailed research in this regard.

[0007] The technical problem solved in this case is how to make the density of indium oxide precursor higher and the resistance lower. Summary of the invention

[0008] The purpose of the present invention is to provide a low-resistance and high-density oxide target precursor and a preparation method thereof. The method of the present invention is aimed at a target material with a high indium oxide content. A sand grinding method is used in combination with grinding balls of different particle sizes to reduce the gap between precursor powders, reduce the direct contact resistance and barrier resistance between powders, and ultimately increase the density of the precursor, reduce resistance, and improve agglomeration performance.

[0009] At the same time, the present invention also provides a low-resistance and high-density oxide target precursor.

[0010] To achieve the above objectives, this application discloses:

[0011] A method for preparing a low-resistance and high-density oxide target precursor comprises sand-milling a slurry containing an oxide precursor and then granulating the slurry; the oxide precursor contains not less than 97.5 wt% of indium oxide;

[0012] The particle sizes of the grinding balls used in sand milling are 0.3mm, 0.4-0.6mm, and 0.8-1.0mm;

[0013] The mass ratio of 0.3 mm grinding balls, 0.4-0.6 mm grinding balls, and 0.8-1.0 mm grinding balls is 4-7:1-4:1-4.

[0014] During the research process of this invention, we found that the two key properties of the precursor powder: density and resistance are closely related to the grinding process of the precursor powder. Through the study of the previous ball milling process, it was found that the ball milling process easily leads to the agglomeration of the precursor powder, and the agglomeration will significantly increase the direct contact resistance and barrier resistance between the powders; the resistance of the precursor powder is affected by three factors respectively. The first factor is the resistance value of the prepared powder itself, which is a standard value for this patent and has negligible effect on the actual resistance; the second is the resistance generated by the contact between the powders, which can also be called direct contact resistance; the last factor is the barrier resistance of the particle interlayer contact. These two resistance values ​​have a greater impact on the actual resistance of the powder, and the actual resistance R is the sum of the three.

[0015] In the process of further research, we found that sand milling is the most effective means to solve this problem, but if the same specifications of grinding balls are used, there will still be a serious agglomeration phenomenon; after repeated experiments, it is determined that the above grinding ball particle size and weight ratio are more appropriate and can effectively solve the agglomeration phenomenon, increase density and reduce resistance. The essential reason is that the use of zirconium ball grinding media with different diameters allows the micron, submicron and nanometer-level precursor powders produced during the grinding process to be immediately broken down into small particles and dispersed to form spherical and other irregular shapes when forming large particle agglomerates. Agglomerates continue to decrease, dispersibility improves, and the average particle size of the powder gradually decreases, making the gap between the precursors smaller and more tightly combined.

[0016] At the same time, we further found that this method is more effective for precursors with high indium oxide content. The possible reason is that when the indium oxide content is high, it is more likely to aggregate significantly, and the method of the present invention can specifically solve this problem.

[0017] In the above-mentioned method for preparing a low-resistance and high-density oxide target precursor, the mass ratio of the 0.3 mm grinding balls, the 0.4-0.6 mm grinding balls, and the 0.8-1.0 mm grinding balls is 4-6:2-4:2-4.

[0018] In the above-mentioned method for preparing a low-resistance and high-density oxide target precursor, the slurry also contains a dispersant and a binder; the dispersant in the slurry accounts for 0.1wt% to 5wt% of the slurry weight; the binder accounts for 5wt% to 20wt% of the slurry weight.

[0019] In the above-mentioned method for preparing a low-resistance and high-density oxide target precursor, the method for sand-milling the slurry containing the oxide precursor is:

[0020] Step 1: Mix other oxides except indium oxide, part of the dispersant, and water to prepare a slurry, and sand grind to obtain a first slurry;

[0021] Step 2: adding indium oxide and the remaining dispersant to the first slurry, mixing and slurrying, and sand-milling to obtain a second slurry;

[0022] Step 3: Mix the second slurry and the binder to prepare a slurry, and sand grind the slurry to obtain a third slurry;

[0023] The particle sizes of the grinding balls used in the sand milling in steps 1 to 3 are 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm, respectively; the mass ratio of 0.3 mm grinding balls, 0.4-0.6 mm grinding balls, and 0.8-1.0 mm grinding balls is 4-7:1-4:1-4.

[0024] In the above-mentioned method for preparing a low-resistance and high-density oxide target precursor, the dispersant is one or more of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate, a polycarboxylic acid compound, a polyvinyl salt or sodium hexadecylbenzene sulfonate;

[0025] The binder is a mixture of polyvinyl alcohol and polyethylene glycol, polyvinyl alcohol or polyvinyl butyral, or both.

[0026] In the above-mentioned method for preparing a low-resistance and high-density oxide target precursor, the process parameters of the sand milling in step 1 are: a rotation speed of 800 to 1600 rpm, and a grinding time of 5 to 9 hours;

[0027] The process parameters of the sand milling in step 2 are: a rotation speed of 800 to 1600 rpm and a grinding time of 8 to 12 h;

[0028] The process parameters of the sand grinding in step 3 are: rotation speed of 800 to 1600 rpm, and grinding time of 2 to 4 hours.

[0029] In the above-mentioned method for preparing a low-resistance and high-density oxide target precursor, the oxide precursor contains not less than 98wt% of indium oxide; the oxide precursor also contains one or more combinations of cerium oxide, titanium oxide, tantalum oxide, molybdenum oxide, praseodymium oxide, and zinc oxide.

[0030] In the above-mentioned method for preparing a low-resistance and high-density oxide target precursor, the oxide precursor is composed of indium oxide powder, cerium oxide powder, titanium oxide powder, and tantalum oxide powder; the weight ratio of indium oxide powder, cerium oxide powder, titanium oxide powder, and tantalum oxide powder is: 97.5~99.7:0.1~1:0.1~1:0.1~0.5.

[0031] In the above-mentioned method for preparing the low-resistance and high-density oxide target precursor, the granulation process is: the slurry is granulated by spraying, and then mixed and screened to obtain the oxide target precursor, wherein the process parameters of the spray granulation are: the air outlet temperature is 60-70°C, and the atomizer frequency is 80-160Hz.

[0032] At the same time, the present invention also discloses a low-resistance and high-density oxide target precursor, which is prepared by any of the above methods.

[0033] This application has at least the following beneficial effects:

[0034] During the grinding stage, the present invention uses grinding balls with different diameters of the medium, compared with the fixed medium grinding diameter, so that the agglomerates are continuously reduced, the dispersibility is improved, the average particle size of the powder is gradually reduced, the gap is smaller, and the combination is tighter, thereby obtaining a low-resistance and high-density oxide target precursor powder. DETAILED DESCRIPTION

[0035] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. In the description of the present invention, it should be noted that, if no specific conditions are specified in the embodiments, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0036] Example 1

[0037] A low-resistance and high-density oxide target precursor is prepared by the following steps:

[0038] Step 1: weigh 99.1 kg of indium oxide, 0.2 kg of cerium oxide, 0.5 kg of titanium oxide, 0.2 kg of tantalum oxide, 8.1 kg of dispersant polyvinyl pyrrolidone and 3.1 kg of binder polyethylene glycol for later use. The particle size of each of the above oxide powders is 200 to 500 nm;

[0039] Step 2: Pour 0.2 kg of cerium oxide, 0.5 kg of titanium oxide, 0.2 kg of tantalum oxide and 3.1 kg of dispersant polyvinyl pyrrolidone weighed in step 1 into a slurry bucket filled with pure water for pre-dispersion at a dispersing speed of 100 rpm. After 30 minutes of dispersion, slurry 1 is obtained, wherein the polyvinyl pyrrolidone dispersant accounts for 5% of the total mass of cerium oxide powder, tantalum oxide powder and titanium oxide powder, and the solid content of the slurry is 60%;

[0040] Step 3: The slurry 1 obtained in step 2 is pumped into a 10L sand mill equipped with zirconium balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm in a weight ratio of 5:3:2 by a pneumatic diaphragm pump for grinding, wherein the grinding speed is 1100 rpm, the ball-to-material ratio is 0.18, and the grinding time is 6 hours to obtain slurry 2;

[0041] Step 4: add 99.1 kg of indium oxide and 5 kg of dispersant polyvinyl pyrrolidone weighed in step 1 to the slurry 2 obtained in step 3 for pre-dispersion at a dispersing speed of 100 rpm. After 40 minutes of dispersion, a slurry 3 is obtained, wherein the polyvinyl pyrrolidone dispersant accounts for 5% of the total mass of the cerium oxide powder, the tantalum oxide powder, and the titanium oxide powder, and the solid content of the slurry is 65%;

[0042] Step 5: The slurry 3 obtained in step 4 was pumped into a 10L sand mill equipped with zirconium balls of 0.3 mm, 0.4-0.6 mm, 0.8-1.0 mm and a weight ratio of 5:3:2 by a pneumatic diaphragm pump for grinding, wherein the grinding speed was 1100 rpm, the grinding time was 11 h, and the ball-to-material ratio was 0.18, to obtain slurry 4;

[0043] Step 6: Add 3.1 kg of binder polyethylene glycol to the slurry 4 obtained in step 5 for pre-dispersion, the dispersion speed is 100 rpm, and after 40 minutes of dispersion, a slurry 5 is obtained, wherein the binder polyethylene glycol accounts for 10% of the total mass of the added powder and the binder;

[0044] Step 7: The slurry 5 obtained in step 6 was pumped into a 10L sand mill equipped with zirconium balls of 0.3 mm, 0.4-0.6 mm, 0.8-1.0 mm and a weight ratio of 5:3:2 by a pneumatic diaphragm pump for grinding. The grinding speed was 1100 rpm, the ball-to-material ratio was 0.18, and the grinding time was 2 h to obtain slurry 6;

[0045] Step 8: The slurry obtained in step 7 is fed into a parallel flow spray drying tower for spray granulation, followed by mixing and sieving to obtain a mixed oxide target precursor powder, wherein the air outlet temperature is 75° C. and the atomizer frequency is 120 Hz.

[0046] Step 9: Measure its resistance, density, average particle size and agglomeration coefficient.

[0047] Example 2

[0048] The preparation of a low-resistance and high-density oxide target precursor is basically the same as that in Example 1, except that the sand mill in steps 3, 5, and 7 is equipped with zirconium balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm in a weight ratio of 4:3:3.

[0049] Example 3

[0050] The preparation of a low-resistance and high-density oxide target precursor is basically the same as that in Example 1, except that the sand mill in steps 3, 5, and 7 is equipped with zirconium balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm in a weight ratio of 7:4:4.

[0051] Example 4

[0052] The preparation of a low-resistance and high-density oxide target precursor is basically the same as that in Example 1, except that the oxide composition is: 97.5 kg indium oxide, 1 kg cerium oxide, 1 kg titanium oxide, and 0.5 kg tantalum oxide.

[0053] Example 5

[0054] The preparation of a low-resistance and high-density oxide target precursor is basically the same as that in Example 1, except that the oxide composition is: 99.7 kg indium oxide, 0.1 kg cerium oxide, 0.1 kg titanium oxide, and 0.1 kg tantalum oxide.

[0055] Example 6

[0056] The preparation of a low-resistance and high-density oxide target precursor is basically the same as that in Example 1, except that the grinding time in step 3 is 5 hours; the grinding time in step 5 is 8 hours, and the grinding time in step 7 is 3 hours.

[0057] Example 7

[0058] The preparation of a low-resistance and high-density oxide target precursor is basically the same as that in Example 1, except that the grinding time in step 3 is 9 hours; the grinding time in step 5 is 12 hours, and the grinding time in step 7 is 4 hours.

[0059] Comparative Example 1

[0060] It is substantially the same as Example 1, except that: the sand mill in steps 3, 5, and 7 is equipped with 0.3 mm zirconium balls, and the ball-to-material volume ratio is 0.18.

[0061] Comparative Example 2

[0062] It is substantially the same as Example 1, except that the sand mill in steps 3, 5, and 7 is equipped with zirconium balls of 0.4 to 0.6 mm, and the ball-to-material volume ratio is 0.18.

[0063] Comparative Example 3

[0064] It is substantially the same as Example 1, except that the sand mill in steps 3, 5, and 7 is equipped with zirconium balls of 0.8 to 1.0 mm, and the ball-to-material volume ratio is 0.18.

[0065] Comparative Example 4

[0066] It is substantially the same as Example 1, except that the sand mill in steps 3, 5, and 7 is equipped with zirconium balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm in a weight ratio of 2:3:3.

[0067] Comparative Example 5

[0068] It is substantially the same as Example 5, except that the sand mill in steps 3, 5, and 7 is equipped with zirconium balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm in a weight ratio of 2:3:3.

[0069] Comparative Example 6

[0070] It is substantially the same as Example 6, except that the sand mill in steps 3, 5, and 7 is equipped with zirconium balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm in a weight ratio of 4:5:5.

[0071] Performance Testing

[0072] The test items include resistance, density, average particle size and agglomeration coefficient;

[0073] The test results are shown in Table 1 below;

[0074] Table 1 Test results

[0075]

[0076] Result analysis:

[0077] 1. It can be seen from Examples 1 to 7 that the agglomeration problem can be substantially solved by appropriate grinding ball particle size and weight ratio, which can improve density and reduce resistance; within the experimental parameter range, the precursor powder particle size obtained by using different grinding medium diameters is smaller, which makes the gaps between the powders smaller and the combination is tighter, resulting in higher density and reduced direct contact resistance and barrier resistance of particle interlayer contact. At the same time, the agglomeration coefficient is affected by the powder particle size, making the powder more dispersed and having better fluidity. Examples 4, 5, 6, and 7 illustrate that changes in the parameter range of component ratio and grinding time will not lead to a decrease in powder performance;

[0078] 2. Comparative Examples 1, 2, and 3 show that a single grinding medium diameter cannot effectively refine and crush large particles into small particles, thereby causing agglomeration to intensify; Comparative Examples 4, 5, and 6 show that the grinding medium diameter ratio has a greater influence on the powder performance. The higher the ratio, the larger the particle size, the lower the ratio, and the more serious the agglomeration.

[0079] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. A method for preparing a low-resistance and high-density oxide target precursor, characterized in that: Sand-grinding a slurry containing an oxide precursor, and then granulating the slurry; the oxide precursor contains not less than 97.5 wt % of indium oxide; The particle sizes of the grinding balls used in sand milling are 0.3mm, 0.4-0.6mm, and 0.8-1.0mm; The mass ratio of 0.3 mm grinding balls, 0.4-0.6 mm grinding balls, and 0.8-1.0 mm grinding balls is 4-7:1-4:1-4.

2. The method for preparing a low-resistance and high-density oxide target precursor according to claim 1, characterized in that: The mass ratio of the 0.3 mm grinding balls, the 0.4-0.6 mm grinding balls, and the 0.8-1.0 mm grinding balls is 4-6:2-4:2-4.

3. The method for preparing a low-resistance and high-density oxide target precursor according to claim 1, characterized in that: The slurry further contains a dispersant and a binder; the dispersant in the slurry accounts for 0.1wt% to 5wt% of the slurry weight; the binder accounts for 5wt% to 20wt% of the slurry weight.

4. The method for preparing a low-resistance and high-density oxide target precursor according to claim 1, characterized in that: The method of sand milling the slurry containing the oxide precursor is as follows: Step 1: Mix other oxides except indium oxide, part of the dispersant, and water to prepare a slurry, and sand grind to obtain a first slurry; Step 2: adding indium oxide and the remaining dispersant to the first slurry, mixing and slurrying, and sand-milling to obtain a second slurry; Step 3: Mix the second slurry and the binder to prepare a slurry, and sand grind the mixture to obtain a third slurry; The particle sizes of the grinding balls used in the sand milling in steps 1 to 3 are 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm, respectively; the mass ratio of 0.3 mm grinding balls, 0.4-0.6 mm grinding balls, and 0.8-1.0 mm grinding balls is 4-7:1-4:1-4.

5. The method for preparing a low-resistance and high-density oxide target precursor according to claim 4, characterized in that: The dispersant is one or more of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate, polycarboxylic acid compounds, polyvinyl salts or sodium hexadecylbenzene sulfonate; The binder is a mixture of polyvinyl alcohol and polyethylene glycol, polyvinyl alcohol or polyvinyl butyral, or both.

6. The method for preparing a low-resistance and high-density oxide target precursor according to claim 4, characterized in that: The process parameters of the sand milling in step 1 are: a rotation speed of 800 to 1600 rpm and a grinding time of 5 to 9 hours; The process parameters of the sand milling in step 2 are: a rotation speed of 800 to 1600 rpm and a grinding time of 8 to 12 h; The process parameters of the sand grinding in step 3 are: rotation speed of 800 to 1600 rpm, and grinding time of 2 to 4 hours.

7. The method for preparing a low-resistance and high-density oxide target precursor according to claim 1, characterized in that: The oxide precursor contains no less than 98 wt % of indium oxide; the oxide precursor also contains one or more combinations of cerium oxide, titanium oxide, tantalum oxide, molybdenum oxide, praseodymium oxide and zinc oxide.

8. The method for preparing a low-resistance and high-density oxide target precursor according to claim 1, characterized in that: The oxide precursor is composed of indium oxide powder, cerium oxide powder, titanium oxide powder and tantalum oxide powder; the weight ratio of indium oxide powder, cerium oxide powder, titanium oxide powder and tantalum oxide powder is 97.5-99.7:0.1-1:0.1-1:0.1-0.

5.

9. The method for preparing a low-resistance and high-density oxide target precursor according to any one of claims 1 to 8, characterized in that: The granulation process is as follows: the slurry is granulated by spraying, and then mixed and sieved to obtain an oxide target precursor, wherein the process parameters of the spray granulation are: the air outlet temperature is 60-70° C., and the atomizer frequency is 80-160 Hz.

10. A low-resistance and high-density oxide target precursor, characterized in that: The method is prepared by any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of indium tin oxide grinding balls

    CN111807832A

  • Treatment method of high-density ITO target material powder

    CN113800900A

  • Indium oxide target material and preparation method thereof

    CN114059025A

  • High-mobility indium titanium cerium tantalum oxide target material and preparation method thereof

    CN116639956A

  • Indium titanium tantalum cerium oxide target material, preparation method thereof and coated glass sheet

    CN116768603A

Cited By

  • Preparation method of high-entropy oxide nanoparticles

    CN122233448A