A macroporous anion exchange resin loaded with zirconium phosphate nanoparticles

By preparing macroporous anion exchange resin loaded with zirconium phosphate nanoparticles, the performance limitations of traditional resins in strong radiation and complex environments have been solved, resulting in an adsorption material with high efficiency and long lifespan, suitable for the treatment of radioactive nuclides and heavy metal wastewater.

CN123102307APending Publication Date: 2026-11-17余天睿
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510636561.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional polystyrene-divinylbenzene anion exchange resins are prone to molecular chain breakage and cross-linking structure destruction under strong radiation, strong acids and alkalis, or high concentrations of oxidizing substances. This leads to a decrease in ion exchange capacity and mechanical strength, and their selective adsorption capacity for specific anions is limited, making it difficult to effectively remove target pollutants in complex water systems. Existing modification methods struggle to achieve uniform dispersion of modifiers, resulting in poor stability and failing to meet the requirements of industrial applications.

Method used

A method for preparing macroporous anion exchange resin loaded with zirconium phosphate nanoparticles was adopted. Through suspension polymerization, chloromethylation and quaternization treatment, zirconium phosphate nanoparticles were chemically bonded to the macroporous resin matrix to form a stable layered structure, which enhanced its adsorption selectivity for specific anions and radiation resistance.

Benefits of technology

It improves the resin's exchange capacity and radiation resistance, extends its service life, enhances its adsorption capacity for radioactive nuclides and heavy metal ions, and maintains high-efficiency adsorption performance even under high-energy radiation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention provides a macroporous anion exchange resin loaded with zirconium phosphate nanoparticles and its preparation method. This resin, by uniformly loading zirconium phosphate nanoparticles into a macroporous polystyrene matrix to form an organic-inorganic hybrid structure, significantly improves the adsorption selectivity and capacity for specific anions, and enhances the resin's radiation resistance and mechanical strength. This invention also provides a simple and efficient preparation method, including steps such as suspension polymerization to prepare the macroporous resin, chloromethylation, quaternization, and zirconium phosphate nanoparticle loading. This resin is suitable for applications such as radionuclide separation and heavy metal wastewater treatment, providing a new approach for developing high-performance anion exchange resins.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer synthesis technology, specifically, it relates to a method for preparing a macroporous anion exchange resin loaded with zirconium phosphate nanoparticles. Background Technology

[0002] Anion exchange resins play a crucial role as key adsorbent materials in fields such as radionuclide separation, heavy metal wastewater treatment, and chemical catalysis, especially in nuclear industry wastewater treatment. However, traditional polystyrene-divinylbenzene (PS-DVB)-based anion exchange resins have significant shortcomings, severely limiting their application in challenging environments. Specifically, in the presence of strong radiation, strong acids and alkalis, or high concentrations of oxidizing agents, they are prone to molecular chain breakage and cross-linking structure destruction, leading to decreased ion exchange capacity, reduced mechanical strength, and shortened service life, severely impacting their treatment efficiency and economic viability. Furthermore, traditional resins have limited selective adsorption capacity for specific anions, making it difficult to effectively remove target pollutants in complex water systems. For example, in the presence of high concentrations of competing ions, their adsorption efficiency for radionuclides or specific heavy metal ions decreases significantly. Existing modification methods, such as simple physical blending or surface modification, often fail to achieve uniform dispersion of the modifier, resulting in poor modification effects and instability, failing to meet the needs of practical industrial applications.

[0003] In recent years, inorganic-organic hybrid materials have become a hot topic in the research of novel adsorption materials due to their combination of the high stability of inorganic materials and the high selectivity of organic materials. Among them, zirconium phosphate (ZrP), as a novel layered inorganic material, has shown great application potential in the field of adsorption due to its unique layered structure, abundant surface active sites, and excellent ion exchange performance. Its regular layered structure can effectively improve the adsorption selectivity for specific anions and exhibits good thermal stability and radiation resistance. However, the direct application of zirconium phosphate in wastewater treatment has problems such as excessively large particle size, easy agglomeration, and difficulty in separation, which limit its adsorption efficiency and practical application. Summary of the Invention

[0004] This invention provides a macroporous anion exchange resin loaded with zirconium phosphate nanoparticles and its preparation method. The anion exchange resin has good radiation resistance, and compared with existing methods, the resin obtained has high exchange capacity and good radiation resistance.

[0005] To solve the above-mentioned technical problems, the embodiments of the present invention adopt the following technical solutions: A method for preparing a macroporous anion exchange resin loaded with zirconium phosphate nanoparticles, characterized in that the preparation method includes the following steps: Step a) Styrene, divinylbenzene, initiator and porogen are mixed evenly to obtain an oil phase; dispersant, inorganic salt and water are mixed evenly to obtain an aqueous phase; the oil phase and aqueous phase are mixed at a volume ratio of 1: (2~4) and subjected to suspension polymerization at 50~90℃ for 6~12 h; the mixture is extracted with toluene, dried and sieved to obtain macroporous copolymer white spheres; Step b) Mix the macroporous copolymer white spheres obtained in step a) with the chloromethylating agent at a mass ratio of 1: (2~5), add a catalyst at a mass ratio of 1: (0.05~0.1) to the microspheres, and react at 35~55°C for 3~6 h. After the reaction is completed, wash with deionized water until neutral to obtain the chloromethylated copolymer. Step c) Mix the chloromethylated copolymer obtained in step b) with the quaternizing agent at a mass ratio of 1: (0.5~2) and react at 40~70°C for 5~10 h. After the reaction is completed, wash with deionized water until neutral to obtain macroporous anion exchange resin. Step d) Disperse the macroporous anion exchange resin obtained in step c) in deionized water, adjust the pH to 1-3 with hydrochloric acid, and slowly add zirconium salt and phosphate at a molar ratio of 1:(1-3) while stirring. React at 60-100℃ for 4-10 h. After washing and drying, obtain macroporous anion exchange resin loaded with zirconium phosphate nanoparticles.

[0006] As a preferred example, in step a), the initiator is one of benzoyl peroxide, azobisisobutyronitrile, ammonium persulfate, or potassium persulfate; the pore-forming agent is one or more of toluene, xylene, n-heptane, or liquid paraffin; the dispersant is one or more of gelatin, polyvinyl alcohol, or hydroxyethyl cellulose; and the inorganic salt is one or more of sodium chloride, sodium sulfate, or sodium phosphate.

[0007] As a preferred example, in step a), the mass ratio of styrene to divinylbenzene is 1:(0.02~0.4); the initiator is 0.5~2 wt% of the total monomer mass; the porogen is 50~150 wt% of the total monomer mass; and the mass ratio of dispersant, inorganic salt, and water is (0.5~1.5):(3~5):100.

[0008] As a preferred example, in step b), the chloromethylating agent is one of chloromethyl isooctyl ether, 1,4-dichloromethoxybutane, or methacryloyloxyethyltrimethylammonium chloride. The catalyst is one of anhydrous zinc chloride, aluminum trichloride, stannous chloride, or stannous tetrachloride.

[0009] As a preferred example, in step c), the quaternizing agent is one of trimethylamine, triethylamine, tetramethylethylenediamine, and tert-butylamine.

[0010] As a preferred example, in step d), the zirconium salt is selected from zirconium oxychloride, zirconium nitrate, or zirconium sulfate; and the phosphate is selected from phosphoric acid, disodium hydrogen phosphate, or ammonium dihydrogen phosphate.

[0011] This invention provides a macroporous anion exchange resin loaded with zirconium phosphate nanoparticles and its preparation method, which exhibits both high adsorption capacity and excellent radiation resistance. By loading zirconium phosphate nanoparticles with highly selective adsorption capacity onto a macroporous resin matrix and ensuring their stability through chemical bonding, the resin demonstrates significantly enhanced adsorption capacity for specific anions (such as radionuclides and heavy metal ions), while effectively resisting damage from high-energy radiation and extending its service life. The macroporous structure design further improves mass transfer efficiency and shortens the adsorption equilibrium time. Furthermore, the preparation method of this invention is simple, low-cost, and easy to industrialize, providing an efficient and economical solution to environmental problems such as radionuclide separation and heavy metal wastewater treatment. Detailed Implementation

[0012] The present invention will be further described below with reference to embodiments, but these are not intended to limit the scope of the invention. Example

[0013] 80 g of styrene, 10 g of divinylbenzene, 1 g of benzoyl peroxide, and 100 g of n-heptane were mixed uniformly to obtain an oil phase; 1.0 g of gelatin and 5 g of sodium chloride were dissolved in 400 mL of deionized water to obtain an aqueous phase; the oil phase and aqueous phase were mixed at a volume ratio of 1:3 and reacted at 80 °C and 300 rpm for 8 hours to obtain macroporous copolymer microspheres. The porogen was removed by toluene extraction, and the microspheres were dried and sieved to obtain macroporous copolymer white spheres.

[0014] Take 10 g of macroporous copolymer white spheres, add 30 g of chloromethyl isooctyl ether and 0.8 g of anhydrous zinc chloride, react at 50 °C for 4 hours, wash with water until neutral, and obtain chloromethylated copolymer.

[0015] Take 10 g of chloromethylated copolymer and react it with 10 g of 30 wt% trimethylamine aqueous solution at 60 °C for 8 hours. Wash with water until neutral to obtain macroporous anion exchange resin.

[0016] 10 g of macroporous anion exchange resin was dispersed in 200 mL of deionized water, and the pH was adjusted to 2.0 with hydrochloric acid. 150 mL of 0.5 mol / L zirconium oxychloride solution and 50 mL of 1.5 mol / L phosphoric acid solution were slowly added dropwise with stirring. The reaction was carried out at 90 °C for 6 hours. After washing and drying, macroporous anion exchange resin loaded with zirconium phosphate nanoparticles was obtained. Example

[0017] An oil phase was obtained by uniformly mixing 80 g styrene, 5 g divinylbenzene, 1 g benzoyl peroxide, and 100 g n-heptane. An aqueous phase was obtained by dissolving 1.0 g gelatin and 5 g sodium chloride in 400 mL deionized water. The oil and aqueous phases were mixed at a volume ratio of 1:3 and reacted at 80 °C and 300 rpm for 8 hours to obtain macroporous copolymer microspheres. The porogen was removed by toluene extraction, and the microspheres were dried and sieved to obtain macroporous copolymer white spheres.

[0018] Take 10 g of macroporous copolymer white spheres, add 30 g of chloromethyl isooctyl ether and 0.8 g of anhydrous zinc chloride, react at 50 °C for 4 hours, wash with water until neutral, and obtain chloromethylated copolymer.

[0019] Take 10 g of chloromethylated copolymer and react it with 10 g of 30 wt% trimethylamine aqueous solution at 60 °C for 8 hours. Wash with water until neutral to obtain macroporous anion exchange resin.

[0020] 10 g of macroporous anion exchange resin was dispersed in 200 mL of deionized water, and the pH was adjusted to 2.0 with hydrochloric acid. 150 mL of 0.5 mol / L zirconium oxychloride solution and 50 mL of 1.5 mol / L phosphoric acid solution were slowly added dropwise with stirring. The reaction was carried out at 90 °C for 6 hours. After washing and drying, macroporous anion exchange resin loaded with zirconium phosphate nanoparticles was obtained. Example

[0021] 80 g of styrene, 10 g of divinylbenzene, 1 g of benzoyl peroxide, 50 g of n-heptane, and 50 g of liquid paraffin were mixed evenly to obtain an oil phase. 1.0 g of gelatin and 5 g of sodium chloride were dissolved in 400 mL of deionized water to obtain an aqueous phase. The oil and aqueous phases were mixed at a volume ratio of 1:3 and reacted at 80 °C and 300 rpm for 8 hours to obtain macroporous copolymer microspheres. The porogen was removed by toluene extraction, and the microspheres were dried and sieved to obtain macroporous copolymer white spheres.

[0022] Take 10 g of macroporous copolymer white spheres, add 30 g of chloromethyl isooctyl ether and 0.8 g of anhydrous zinc chloride, react at 50 °C for 4 hours, wash with water until neutral, and obtain chloromethylated copolymer.

[0023] Take 10 g of chloromethylated copolymer and react it with 10 g of 30 wt% trimethylamine aqueous solution at 60 °C for 8 hours. Wash with water until neutral to obtain macroporous anion exchange resin.

[0024] 10 g of macroporous anion exchange resin was dispersed in 200 mL of deionized water, and the pH was adjusted to 2.0 with hydrochloric acid. 150 mL of 0.5 mol / L zirconium oxychloride solution and 50 mL of 1.5 mol / L phosphoric acid solution were slowly added dropwise with stirring. The reaction was carried out at 90 °C for 6 hours. After washing and drying, macroporous anion exchange resin loaded with zirconium phosphate nanoparticles was obtained. Example

[0025] 80 g of styrene, 10 g of divinylbenzene, 1 g of benzoyl peroxide, and 100 g of n-heptane were mixed uniformly to obtain an oil phase; 1.0 g of gelatin and 5 g of sodium chloride were dissolved in 400 mL of deionized water to obtain an aqueous phase; the oil phase and aqueous phase were mixed at a volume ratio of 1:3 and reacted at 80 °C and 300 rpm for 8 hours to obtain macroporous copolymer microspheres. The porogen was removed by toluene extraction, and the microspheres were dried and sieved to obtain macroporous copolymer white spheres.

[0026] Take 10 g of macroporous copolymer white spheres, add 30 g of chloromethyl isooctyl ether and 0.8 g of anhydrous zinc chloride, react at 50 °C for 4 hours, wash with water until neutral, and obtain chloromethylated copolymer.

[0027] Take 10 g of chloromethylated copolymer and react it with 10 g of 30 wt% trimethylamine aqueous solution at 60 °C for 8 hours. Wash with water until neutral to obtain macroporous anion exchange resin.

[0028] 10 g of macroporous anion exchange resin was dispersed in 200 mL of deionized water, and the pH was adjusted to 2.0 with hydrochloric acid. 225 mL of 0.5 mol / L zirconium oxychloride solution and 75 mL of 1.5 mol / L phosphoric acid solution were slowly added dropwise with stirring. The reaction was carried out at 90 °C for 6 hours. After washing and drying, macroporous anion exchange resin loaded with zirconium phosphate nanoparticles was obtained. Example

[0029] 80 g of styrene, 10 g of divinylbenzene, 1 g of benzoyl peroxide, and 100 g of n-heptane were mixed uniformly to obtain an oil phase; 1.0 g of gelatin and 5 g of sodium chloride were dissolved in 400 mL of deionized water to obtain an aqueous phase; the oil phase and aqueous phase were mixed at a volume ratio of 1:3 and reacted at 80 °C and 300 rpm for 8 hours to obtain macroporous copolymer microspheres. The porogen was removed by toluene extraction, and the microspheres were dried and sieved to obtain macroporous copolymer white spheres.

[0030] Take 10 g of macroporous copolymer white spheres, add 30 g of chloromethyl isooctyl ether and 0.8 g of anhydrous zinc chloride, react at 50 °C for 4 hours, wash with water until neutral, and obtain chloromethylated copolymer.

[0031] Take 10 g of chloromethylated copolymer and react it with 10 g of 30 wt% tetramethylethylenediamine aqueous solution at 60 °C for 8 hours. Wash with water until neutral to obtain macroporous anion exchange resin.

[0032] 10 g of macroporous anion exchange resin was dispersed in 200 mL of deionized water, and the pH was adjusted to 2.0 with hydrochloric acid. 150 mL of 0.5 mol / L zirconium oxychloride solution and 50 mL of 1.5 mol / L phosphoric acid solution were slowly added dropwise with stirring. The reaction was carried out at 90 °C for 6 hours. After washing and drying, macroporous anion exchange resin loaded with zirconium phosphate nanoparticles was obtained.

[0033] Example Exchange capacity (mmol / g) Crushing strength (MPa) <![CDATA[Radiation resistance (10 6 Capacity retention rate after Gy gamma-ray irradiation, %)]]> 1 3.5 2.8 90 2 3.2 2.5 84 3 3.8 2.9 92 4 4.1 3.0 95 5 3.7 2.7 91

Claims

1. A method for preparing a macroporous anion exchange resin loaded with zirconium phosphate nanoparticles, characterized in that, The preparation method of this material includes the following steps: Step a) Styrene, divinylbenzene, initiator and porogen are mixed evenly to obtain an oil phase; dispersant, inorganic salt and water are mixed evenly to obtain an aqueous phase; the oil phase and aqueous phase are mixed at a volume ratio of 1: (2~4) and subjected to suspension polymerization at 50~90℃ for 6~12 h; the mixture is extracted with toluene, dried and sieved to obtain macroporous copolymer white spheres; Step b) Mix the macroporous copolymer white spheres obtained in step a) with the chloromethylating agent at a mass ratio of 1: (2~5), add a catalyst at a mass ratio of 1: (0.05~0.1) to the microspheres, and react at 35~55°C for 3~6 h. After the reaction is completed, wash with deionized water until neutral to obtain the chloromethylated copolymer. Step c) Mix the chloromethylated copolymer obtained in step b) with the quaternizing agent at a mass ratio of 1: (0.5~2) and react at 40~70°C for 5~10 h. After the reaction is completed, wash with deionized water until neutral to obtain macroporous anion exchange resin. Step d) Disperse the macroporous anion exchange resin obtained in step c) in deionized water, adjust the pH to 1-3 with hydrochloric acid, and slowly add zirconium salt and phosphate at a molar ratio of 1:(1-3) while stirring. React at 60-100℃ for 4-10 hours. After washing and drying, obtain macroporous anion exchange resin loaded with zirconium phosphate nanoparticles.

2. The method for preparing a macroporous anion exchange resin loaded with zirconium phosphate nanoparticles according to claim 1, characterized in that: In step a), the initiator is one of benzoyl peroxide, azobisisobutyronitrile, ammonium persulfate, or potassium persulfate; the pore-forming agent is one or more of toluene, xylene, n-heptane, or liquid paraffin; the dispersant is one or more of gelatin, polyvinyl alcohol, or hydroxyethyl cellulose; and the inorganic salt is one or more of sodium chloride, sodium sulfate, or sodium phosphate.

3. The method for preparing a macroporous anion exchange resin loaded with zirconium phosphate nanoparticles according to claim 1, characterized in that: In step a), the mass ratio of styrene to divinylbenzene is 1:(0.02~0.4); the initiator is 0.5~2 wt% of the total monomer mass; the porogen is 50~150 wt% of the total monomer mass; and the mass ratio of dispersant, inorganic salt, and water is (0.5~1.5):(3~5):

100.

4. The method for preparing a macroporous anion exchange resin loaded with zirconium phosphate nanoparticles according to claim 1, characterized in that: In step b), the chloromethylating agent is one of chloromethyl isooctyl ether, 1,4-dichloromethoxybutane, or methacryloyloxyethyltrimethylammonium chloride. The catalyst is one of anhydrous zinc chloride, aluminum trichloride, stannous chloride, or stannous tetrachloride.

5. The method for preparing a macroporous anion exchange resin loaded with zirconium phosphate nanoparticles according to claim 1, characterized in that: In step c), the quaternizing agent is one of trimethylamine, triethylamine, tetramethylethylenediamine, and tert-butylamine.

6. The method for preparing a macroporous anion exchange resin loaded with zirconium phosphate nanoparticles according to claim 1, characterized in that: In step d), the zirconium salt is selected from zirconium oxychloride, zirconium nitrate, or zirconium sulfate; the phosphate is selected from phosphoric acid, disodium hydrogen phosphate, or ammonium dihydrogen phosphate.