A Comprehensive Recovery Method for Copper-Molybdenum Sulfide Ores Based on Slurry Potential Regulation

By using three-stage slurry potential regulation and flotation reagent combination, the problem of low molybdenum recovery rate in copper-molybdenum sulfide ores was solved, achieving efficient separation and recovery of copper, molybdenum and sulfur, and improving resource utilization.

CN123102494APending Publication Date: 2026-11-17LIANGSHAN MINING CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611286000.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The recovery rate of molybdenum in existing copper-molybdenum sulfide ores is low. Traditional processes have failed to effectively improve the recovery rate of copper and molybdenum and are accompanied by the loss of sulfur resources, making it difficult to achieve efficient and comprehensive recovery of multiple metals.

Method used

A three-stage pulp potential control method is adopted to precisely control the pulp potential before and after the copper-molybdenum mixed roughing, mixed cleaning, and sulfur flotation. Combined with specific flotation reagents, this method achieves efficient separation and recovery of copper, molybdenum, and sulfur.

Benefits of technology

It significantly improved the recovery rates of copper and molybdenum as well as sulfur concentrate, realizing the full resource utilization of copper-molybdenum sulfide ores and enhancing the recovery rate and grade of molybdenum and sulfur.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102494A_ABST
    Figure CN123102494A_ABST
Patent Text Reader

Abstract

This invention relates to the field of molybdenum beneficiation technology, specifically a comprehensive recovery method for copper-molybdenum sulfide ore based on slurry potential control, comprising the following steps: S1: adjusting the slurry potential of the copper-molybdenum sulfide ore; S2: subjecting the slurry with adjusted slurry potential to copper-molybdenum roughing to obtain roughing concentrate and roughing tailings; S3: subjecting the roughing concentrate to a second slurry potential adjustment, followed by copper-molybdenum mixed cleaning to obtain copper-molybdenum mixed concentrate and copper-molybdenum mixed tailings, wherein the copper-molybdenum mixed concentrate enters the subsequent copper-molybdenum separation process; S4: subjecting the roughing tailings to copper-molybdenum scavenging to obtain scavenging froth and scavenging tailings, subjecting the scavenging tailings to a third slurry potential adjustment, followed by sulfur flotation to obtain sulfur concentrate and final tailings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of molybdenum beneficiation technology, specifically a comprehensive recovery method for copper-molybdenum sulfide ores based on slurry potential regulation. Background Technology Molybdenum, as an important strategic mineral resource, is widely used in metallurgy, electronics, chemicals, and new energy fields. Its efficient development and utilization are of great significance to national resource security and the upgrading of high-end industries. In nature, molybdenum often occurs as a by-product in copper-molybdenum sulfide ores. In these ores, molybdenum minerals are mostly fine-grained and intercalated, mainly in the form of molybdenite (MoS2), and closely associated with copper-sulfur minerals such as chalcopyrite (CuFeS2) and pyrite (FeS2), making separation difficult. Due to the susceptibility of molybdenum mineral surface properties to the influence of the pulp environment, the insufficient selectivity of conventional flotation reagents, and the complex interactions between associated minerals, the recovery rate of associated molybdenum is generally low, resulting in resource waste. In copper-molybdenum sulfide ores, molybdenum is often fine-grained and closely associated with chalcopyrite and pyrite.

[0002] Traditional recovery processes for copper-molybdenum sulfide ores involve first performing mixed flotation of copper and molybdenum for low-grade minerals, followed by separate flotation of copper and molybdenum using depressants. For high-grade minerals, direct separate flotation is performed (see "Zeng Jinming. First-principles study on flotation separation and its process in copper-molybdenum sulfide ores [D]. Central South University, 2012."). However, traditional processes primarily focus on copper and molybdenum recovery, resulting in low molybdenum recovery rates and significant sulfur loss through tailings. Furthermore, improvements to copper-molybdenum sulfide ore recovery processes are generally based on adjusting flotation reagents or depressants, maintaining the overall flotation separation logic without considering the recovery of other valuable minerals, thus offering little improvement in copper and molybdenum recovery rates.

[0003] In summary, there is an urgent need for a multi-metal integrated recovery method for copper-molybdenum sulfide ores, which can enhance the recovery of copper and molybdenum while improving the recovery rate of pyrite, thereby maximizing the utilization of mineral resources. Summary of the Invention

[0004] The purpose of this invention is to provide a comprehensive recovery method for copper-molybdenum sulfide ores based on slurry potential regulation, so as to at least improve the copper-molybdenum recovery rate and efficiently recover sulfide concentrate.

[0005] The objective of this invention is achieved through the following technical solution: A comprehensive recovery method for copper-molybdenum sulfide ores based on slurry potential regulation includes the following steps: S1: Adjust the slurry potential of the copper-molybdenum sulfide ore using the first slurry potential adjustment; S2: The slurry after adjusting the slurry potential is subjected to copper-molybdenum roughing to obtain roughing concentrate and roughing tailings; S3: The rough concentrate is subjected to a second slurry potential adjustment, and then copper-molybdenum mixed beneficiation is carried out to obtain copper-molybdenum mixed concentrate and copper-molybdenum mixed tailings. The copper-molybdenum mixed concentrate enters the subsequent copper-molybdenum separation process. S4: The roughing tailings are subjected to copper-molybdenum scavenging to obtain scavenging froth and scavenging tailings. The scavenging tailings are then subjected to a third pulp potential adjustment, followed by sulfur flotation to obtain sulfur concentrate and final tailings.

[0006] In some embodiments, in step S1: the particle size of the raw ore in the slurry is -0.074mm, accounting for 70~75wt%; the concentration of the raw ore in the slurry is 25~35wt%.

[0007] In some embodiments, in step S1: the adjustment potential of the first slurry potential adjustment is -180mV to -160mV (measured using a Leici PHB-4 potential pH analyzer); the slurry potential adjuster used includes calcium hydroxide.

[0008] In some embodiments, in step S3: the adjustment potential of the second slurry potential adjustment is -120mV to -140mV; the slurry potential adjuster used includes calcium hydroxide.

[0009] In some embodiments, the flotation reagents used in the copper-molybdenum roughing in step S2 and the copper-molybdenum scavenging in step S4 include: Foaming agent a: includes methyl isobutyl ester and methyl isobutyl methanol; Copper-molybdenum collectors include at least one of isobutyl xanthate, mercaptobenzothiazole, and ethyl isobutyl xanthate.

[0010] In some examples, the weight ratio of methyl isobutyl methyl ester to methyl isobutyl methanol in the foaming agent a is 2~6:4~8; and the weight ratio of isobutyl xanthate, mercaptobenzothiazole and ethyl isobutyl xanthate in the copper-molybdenum collector is 2~4:3~5:1~5.

[0011] In some embodiments, the flotation reagents used in the copper-molybdenum refining process in step S3 include: Gangue inhibitors include at least two of the following: cellulose derivatives, dextrin, starch, and sodium silicate; Copper-molybdenum collectors include at least one of isobutyl xanthate, mercaptobenzothiazole, and ethyl isobutyl xanthate. Foaming agent a: includes methyl isobutyl ester and methyl isobutyl methanol.

[0012] In some examples, the copper-molybdenum mixed tailings and the scavenging foam are returned as middlings to the copper-molybdenum roughing step for recycling.

[0013] In some embodiments, in step S4, the adjustment potential of the third slurry potential adjustment is -120mV to -150mV; The slurry potential adjuster used includes sulfuric acid.

[0014] In some embodiments, in step S4, the sulfur flotation includes at least one roughing, one scavenging, and one cleaning step, and the resulting sulfur-refined tailings and sulfur-scavenging foam are returned to the sulfur flotation step for recycling as middlings.

[0015] In some examples, in step S4, the flotation reagents used for sulfur flotation include: Foaming agent b: includes methyl isobutyl ester and terpineol; Sulfur activators: including copper sulfate; Sulfur collectors: including isoamyl xanthate and butyl xanthate.

[0016] In some examples, the weight ratio of methyl isobutyl ester and terpineol in the foaming agent b is 2~5:5~8; and the weight ratio of isopentyl xanthate and butyl xanthate in the sulfur collector is 3~5:5~7.

[0017] In some embodiments, the copper-molybdenum separation process includes conventional flotation separation or separation by adjusting the slurry potential to obtain copper concentrate and molybdenum concentrate.

[0018] It is worth noting that the pulp potential adjustment method is a known method in the field of sulfide mineral flotation for improving flotation efficiency. As a key parameter reflecting the redox state in the pulp system, pulp potential can directly affect the formation of oxide films on mineral surfaces, the adsorption behavior of reagent molecules, and the degree of exposure of active sites on sulfide mineral surfaces.

[0019] However, in the field of copper-molybdenum sulfide ore flotation, the recovery method generally employed is a combination of copper-molybdenum mixed flotation and copper suppression followed by molybdenum separation. The pulp potential adjustment method is typically used only for the copper-molybdenum separation process. By precisely controlling the pulp potential, chalcopyrite is suppressed while molybdenite floats smoothly, thus utilizing the significant difference in floatability between the two minerals to achieve copper and molybdenum separation. However, because sulfide minerals such as pyrite have excellent floatability and readily react with collectors, a large amount of pyrite enters the copper-molybdenum mixed concentrate during the initial copper-molybdenum mixed flotation stage, increasing the difficulty of subsequent refining and limiting the recovery rate of the molybdenum concentrate.

[0020] The process of this invention involves three stages of slurry potential regulation, and through three-stage precise control, it achieves efficient separation and recovery of copper-molybdenum concentrate and sulfur concentrate. The first pulp potential adjustment occurs before the copper-molybdenum mixed roughing process, controlling the pulp potential at -180mV to -160mV. Under this condition, molybdenite floats smoothly due to its natural hydrophobicity, chalcopyrite is recovered by reacting with the collector, while pyrite is strongly suppressed and enters the roughing tailings. The second pulp potential adjustment occurs before the copper-molybdenum mixed concentrate cleaning process, controlling the pulp potential at -120mV to -140mV. Under this condition, residual pyrite and gangue minerals are suppressed, reducing the burden on subsequent copper-molybdenum separation stages and recovering high-grade copper-molybdenum mixed products. The third pulp potential adjustment occurs before the sulfur roughing process. At this time, the tailings mainly contain pyrite, gangue, and other impurity minerals. Controlling the pulp potential at -120mV to -150mV activates pyrite, restores its surface chemical activity, and improves its floatability, allowing high-grade sulfur concentrate to be obtained through subsequent flotation.

[0021] The beneficial effects of this invention are as follows: The process of this invention provides a comprehensive recovery method for copper-molybdenum sulfide ores based on slurry potential control. Unlike the traditional process that only uses slurry potential control during copper suppression and molybdenum flotation, this method introduces potential control before copper and molybdenum roughing and combines it with three precise controls in the cleaning and sulfur recovery stages. This achieves efficient comprehensive recovery of sulfur resources while significantly improving the recovery rate of associated molybdenum, providing a new path for the full resource utilization of complex copper-molybdenum sulfide ores. Attached Figure Description

[0022] Figure 1 This is a schematic diagram of the process flow of Embodiment 1 of the present invention. Detailed Implementation

[0023] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings, but the scope of protection of the present invention is not limited to the following description.

[0024] Example 1 This embodiment provides a comprehensive recovery method for copper-molybdenum sulfide ore, and the specific method is as follows: The flotation reagent composition used in this embodiment is as follows: Copper-molybdenum collector a: Isobutyl xanthate, mercaptobenzothiazole, and ethyl isobutyl xanthate are formulated in a weight ratio of 3:4:3.

[0025] Foaming agent a: Methyl isobutyl methyl ester and methyl isobutyl methanol are prepared in a weight ratio of 3:7.

[0026] Copper-molybdenum collector b: mercaptobenzothiazole and ethyl isobutyl xanthate are prepared in a weight ratio of 4.5:5.5.

[0027] Foaming agent b: Methyl isobutyl methyl ester and methyl isobutyl methanol are prepared in a weight ratio of 3.5:6.5.

[0028] Sulfur collector: isoamyl xanthate and butyl xanthate are prepared in a weight ratio of 4:6.

[0029] Gangue inhibitor: Dextrin and starch are mixed in a weight ratio of 3:7.

[0030] S1: Take copper-molybdenum sulfide ore A (mineral sample from the western Sichuan mining area, containing 0.70% copper, 0.012% molybdenum, and 3.25% sulfur), crush and grind the ore to a fineness of -0.074mm (70%), adjust the pulp concentration to 30%, and transfer it to a flotation cell for stirring; while stirring the pulp in the flotation cell, add calcium hydroxide as a pulp potential adjuster to adjust the pulp potential to -173mV (measured using a Leici PHB-4 potential pH analyzer); S2: Add 60g / t of copper-molybdenum collector a and 30g / t of frother a to the slurry after adjusting the slurry potential, and carry out copper-molybdenum mixed roughing to obtain copper-molybdenum mixed rough concentrate and copper-molybdenum mixed flotation roughing tailings; S3: The copper-molybdenum mixed rough concentrate is regrinded to -0.037mm (85wt%) to fully liberate the copper-molybdenum mineral particles. The pulp concentration is adjusted to 15wt%. Calcium hydroxide is added as a potential adjuster to adjust the pulp potential to -130mV. Gangue inhibitor 10g / t is added. Copper-molybdenum collector b 10g / t and frother b 5g / t are added sequentially for copper-molybdenum mixed beneficiation to obtain copper-molybdenum mixed concentrate and copper-molybdenum mixed beneficiation tailings. The copper-molybdenum mixed beneficiation tailings are returned to the previous operation S2 as middlings.

[0031] S4: The copper-molybdenum mixed roughing tailings are subjected to two-stage scavenging. During the scavenging process, copper-molybdenum collector a 20g / t+10g / t and frother a 10g / t+0g / t are added to obtain scavenging foam product and scavenging tailings. The scavenging foam product is returned to the previous step S2 as middlings. S5: After adjusting the slurry potential to -120mV, add 200g / t of copper sulfate (sulfur activator), 60g / t of sulfur collector, and 30g / t of frother (foaming agent b) to the scavenging tailings for sulfur roughing. The sulfur roughing froth then undergoes two stages of cleaning: the first stage adds 20g / t of sulfur collector, while the second stage does not add any reagents, yielding sulfur concentrate and middlings. The middlings are returned for a first-stage sulfur roughing process. The sulfur roughing tailings undergo a first-stage sulfur scavenging process with 20g / t of sulfur collector added. The scavenging froth is then returned for another sulfur roughing process. The scavenged tailings are the final tailings.

[0032] Example 2 This embodiment provides a comprehensive recovery method for copper-molybdenum sulfide ore, which is the same as in Embodiment 1, except that the source of the recovered copper-molybdenum sulfide ore is different and some experimental parameters are different, as detailed below: S1: Take copper-molybdenum sulfide ore B (mineral sample from the eastern Yunnan mining area, containing 0.53% copper, 0.010% molybdenum, and 2.89% sulfur), crush and grind the ore to a fineness of -0.074mm (75%), adjust the pulp concentration to 28%, and transfer it to a flotation cell for stirring; while stirring the pulp in the flotation cell, add calcium hydroxide as a pulp potential adjuster to adjust the pulp potential to -160mV; S2: Add 50g / t of copper-molybdenum collector a and 20g / t of frother a to the slurry after adjusting the slurry potential, and carry out copper-molybdenum mixed roughing to obtain copper-molybdenum mixed rough concentrate and copper-molybdenum mixed flotation roughing tailings; S3: The copper-molybdenum mixed rough concentrate is regrinded to -0.037mm (90wt%) to fully liberate the copper-molybdenum mineral particles. The pulp concentration is adjusted to 18wt%. Calcium hydroxide is added as a potential adjuster to adjust the pulp potential to -120mV. Gangue inhibitor 15g / t is added. Copper-molybdenum collector b 30g / t and frother b 15g / t are added sequentially for copper-molybdenum mixed beneficiation to obtain copper-molybdenum mixed concentrate and copper-molybdenum mixed beneficiation tailings. The copper-molybdenum mixed beneficiation tailings are returned to the previous operation S2 as middlings.

[0033] S4: The copper-molybdenum mixed roughing tailings are subjected to three-stage scavenging. During the scavenging process, copper-molybdenum collector a 30g / t+10g / t+0g / t and frother a 10g / t+5g / +0g / t are added to obtain scavenging froth product and scavenging tailings. The scavenging froth product is returned to the previous step S2 as middlings. S5: After adjusting the slurry potential to -150mV, add 500g / t of copper sulfate (sulfur activator), 80g / t of sulfur collector, and 40g / t of frother (sulfur frothing agent) to the scavenging tailings for sulfur roughing. The sulfur roughing froth then undergoes two stages of cleaning: 20g / t of sulfur collector is added in the first stage, and 10g / t in the second stage, yielding sulfur concentrate and middlings. The middlings are returned for a first-stage sulfur roughing process. The sulfur roughing tailings undergo two stages of sulfur scavenging: 20g / t of sulfur collector is added in the first stage, and 10g / t in the second stage. The scavenging froth is returned for another sulfur roughing process. The scavenged tailings are the final tailings.

[0034] Comparative Example 1 This comparative example provides a comprehensive recovery method for copper-molybdenum sulfide ore, which directly uses copper-molybdenum mixed flotation to recover the ore without adjusting the slurry potential. The specific method is as follows: S1: Take copper-molybdenum sulfide ore A, crush and grind the ore to a fineness of -0.074mm accounting for 70%, adjust the slurry concentration to 30%, and transfer it into the flotation cell for stirring; S2: Add 60g / t of copper-molybdenum collector a and 30g / t of frother a to the slurry, and carry out copper-molybdenum mixed roughing to obtain copper-molybdenum mixed rough concentrate and copper-molybdenum mixed flotation roughing tailings; S3: The copper-molybdenum mixed rough concentrate is regrinded to -0.037mm (85wt%) to fully liberate the copper-molybdenum mineral particles. The pulp concentration is adjusted to 15wt%. Gangue inhibitor 10g / t is added, followed by copper-molybdenum collector b 10g / t and frother b 5g / t for mixed copper-molybdenum beneficiation. Copper-molybdenum mixed concentrate and copper-molybdenum mixed beneficiation tailings are obtained. The copper-molybdenum mixed beneficiation tailings are returned to the previous operation S2 as middlings.

[0035] S4: The copper-molybdenum mixed roughing tailings are subjected to two-stage scavenging. During the scavenging process, copper-molybdenum collector a 20g / t+10g / t and frother a 10g / t+0g / t are added to obtain scavenging foam product and scavenging tailings. The scavenging foam product is returned to the previous step S2 as middlings. S5: Add 200g / t of copper sulfate (sulfur activator), 60g / t of sulfur collector, and 30g / t of frother (foaming agent b) to the scavenging tailings for sulfur roughing. The sulfur roughing froth then undergoes two stages of cleaning: the first stage adds 20g / t of sulfur collector, while the second stage does not add any reagents, yielding sulfur concentrate and middlings. The middlings are returned for a first-stage sulfur roughing process. The sulfur roughing tailings undergo a first-stage sulfur scavenging process with 20g / t of sulfur collector added. The scavenging froth is then returned for another sulfur roughing process. The scavenged tailings are the final tailings.

[0036] Comparative Example 2 This comparative example provides a comprehensive recovery method for copper-molybdenum sulfide ore. The difference from Example 1 is that only the potential of the raw ore slurry is adjusted. The specific method is as follows: S1: Take copper-molybdenum sulfide ore A, crush and grind the ore to a fineness of -0.074mm accounting for 70%, adjust the slurry concentration to 30%, and transfer it into the flotation cell for stirring; while stirring the slurry in the flotation cell, add calcium hydroxide as a slurry potential adjuster to adjust the slurry potential to -173mV; S2: Add 60g / t of copper-molybdenum collector a and 30g / t of frother a to the slurry after adjusting the slurry potential, and carry out copper-molybdenum mixed roughing to obtain copper-molybdenum mixed rough concentrate and copper-molybdenum mixed flotation roughing tailings; S3: The copper-molybdenum mixed rough concentrate is regrinded to -0.037mm (85wt%) to fully liberate the copper-molybdenum mineral particles. The pulp concentration is adjusted to 15wt%. Gangue inhibitor 10g / t is added, followed by copper-molybdenum collector b 10g / t and frother b 5g / t for mixed copper-molybdenum beneficiation. Copper-molybdenum mixed concentrate and copper-molybdenum mixed beneficiation tailings are obtained. The copper-molybdenum mixed beneficiation tailings are returned to the previous operation S2 as middlings.

[0037] S4: The copper-molybdenum mixed roughing tailings are subjected to two-stage scavenging. During the scavenging process, copper-molybdenum collector a 20g / t+10g / t and frother a 10g / t+0g / t are added to obtain scavenging foam product and scavenging tailings. The scavenging foam product is returned to the previous step S2 as middlings. S5: Sulfur roughing is performed by adding 200g / t of copper sulfate (sulfur activator), 60g / t of sulfur collector, and 30g / t of frother (b). The sulfur roughing froth undergoes two stages of cleaning: the first stage adds 20g / t of sulfur collector, and the second stage does not add any reagents, yielding sulfur concentrate and middlings. The middlings are returned for a final sulfur roughing stage. The sulfur roughing tailings undergo a final sulfur scavenging stage with 20g / t of sulfur collector added. The scavenging froth is returned for a final sulfur roughing stage, and the scavenged tailings are the final tailings.

[0038] Comparative Example 3 This comparative example provides a comprehensive recovery method for copper-molybdenum sulfide ore. The difference from Example 1 is that the potential of the raw ore slurry is not adjusted. The specific method is as follows: S1: Take copper-molybdenum sulfide ore A, crush and grind the ore to a fineness of -0.074mm accounting for 70%, adjust the slurry concentration to 30%, and transfer it into the flotation cell for stirring; S2: Add 60g / t of copper-molybdenum collector a and 30g / t of frother a to the slurry after adjusting the slurry potential, and carry out copper-molybdenum mixed roughing to obtain copper-molybdenum mixed rough concentrate and copper-molybdenum mixed flotation roughing tailings; S3: The copper-molybdenum mixed rough concentrate is regrinded to -0.037mm (85wt%) to fully liberate the copper-molybdenum mineral particles. The pulp concentration is adjusted to 15wt%. Calcium hydroxide is added as a potential adjuster to adjust the pulp potential to -130mV. Gangue inhibitor 10g / t is added. Copper-molybdenum collector b 10g / t and frother b 5g / t are added sequentially for copper-molybdenum mixed beneficiation to obtain copper-molybdenum mixed concentrate and copper-molybdenum mixed beneficiation tailings. The copper-molybdenum mixed beneficiation tailings are returned to the previous operation S2 as middlings.

[0039] S4: The copper-molybdenum mixed roughing tailings are subjected to two-stage scavenging. During the scavenging process, copper-molybdenum collector a 20g / t+10g / t and frother a 10g / t+0g / t are added to obtain scavenging foam product and scavenging tailings. The scavenging foam product is returned to the previous step S2 as middlings. S5: After adjusting the slurry potential to -120mV, add 200g / t of copper sulfate (sulfur activator), 60g / t of sulfur collector, and 30g / t of frother (foaming agent b) to the scavenging tailings for sulfur roughing. The sulfur roughing froth then undergoes two stages of cleaning: the first stage adds 20g / t of sulfur collector, while the second stage does not add any reagents, yielding sulfur concentrate and middlings. The middlings are returned for a first-stage sulfur roughing process. The sulfur roughing tailings undergo a first-stage sulfur scavenging process with 20g / t of sulfur collector added. The scavenging froth is then returned for another sulfur roughing process. The scavenged tailings are the final tailings.

[0040] Experimental Example This experimental example is used to detect the component content of the copper-molybdenum mixed concentrates obtained in Examples 1-2 and Comparative Examples 1-3, and to calculate the yield and grade, as detailed below:

[0041] As can be seen, compared with the traditional method of Comparative Example 1, Example 1 significantly improved the molybdenum recovery rate in copper-molybdenum concentrate from 64.15% to 83.84% and the sulfur recovery rate in sulfur concentrate from 45.68% to 70.30% through three-stage slurry potential control, while maintaining a stable sulfur concentrate grade of 38.25%, achieving efficient synergistic recovery of copper, molybdenum, and sulfur resources. Comparing Comparative Examples 2 and 3 with Example 1, it can be seen that Comparative Example 2 only controlled the potential of the raw ore, and its molybdenum recovery rate (78.22%) and sulfur recovery rate (57.44%) were significantly lower than those of Example 1; Comparative Example 3 only controlled the potential in the cleaning and sulfur flotation stages without pre-roughing control, and its molybdenum recovery rate (72.54%) and sulfur recovery rate (50.87%) were also much lower than those of Example 1. Furthermore, the sulfur grade of the copper-molybdenum concentrate in Example 1 was only 25.34%, far lower than the 34.68% in Comparative Example 1. This demonstrates that the first pulp potential adjustment successfully suppressed pyrite in the roughing stage, while the third adjustment effectively activated pyrite in the tailings. This indicates that the three pulp potential adjustments are indispensable and have a significant synergistic effect, jointly ensuring a high recovery rate of associated molybdenum and efficient comprehensive recovery of sulfur resources.

[0042] The above description is merely a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the forms disclosed herein and should not be construed as excluding other embodiments. It can be used in various other combinations, modifications, and environments, and can be altered within the scope of the concept described herein through the above teachings or related technologies or knowledge. Modifications and variations made by those skilled in the art that do not depart from the spirit and scope of the present invention should be within the protection scope of the appended claims.

Claims

1. A comprehensive recovery method for copper-molybdenum sulfide ores based on slurry potential regulation, characterized in that, Includes the following steps: S1: Adjust the slurry potential of the copper-molybdenum sulfide ore using the first slurry potential adjustment. S2: The slurry after adjusting the slurry potential is subjected to copper-molybdenum roughing to obtain roughing concentrate and roughing tailings; S3: The rough concentrate is subjected to a second slurry potential adjustment, and then copper-molybdenum mixed beneficiation is carried out to obtain copper-molybdenum mixed concentrate and copper-molybdenum mixed tailings. The copper-molybdenum mixed concentrate enters the subsequent copper-molybdenum separation process. S4: The roughing tailings are subjected to copper-molybdenum scavenging to obtain scavenging froth and scavenging tailings. The scavenging tailings are then subjected to a third pulp potential adjustment, followed by sulfur flotation to obtain sulfur concentrate and final tailings.

2. The comprehensive recovery method for copper-molybdenum sulfide ore based on slurry potential regulation according to claim 1, characterized in that, In step S1: the particle size of the raw ore in the slurry is -0.074mm, accounting for 70~75wt%; the concentration of the raw ore in the slurry is 25~35wt%.

3. The comprehensive recovery method for copper-molybdenum sulfide ore based on slurry potential regulation according to claim 1, characterized in that, In step S1: the adjustment potential of the first slurry potential adjustment is -180mv to -160mv; the slurry potential adjuster used includes calcium hydroxide.

4. The comprehensive recovery method for copper-molybdenum sulfide ore based on slurry potential regulation according to claim 1, characterized in that, In step S3: the adjustment potential of the second slurry potential adjustment is -120mV to -140mV; the slurry potential adjuster used includes calcium hydroxide.

5. The comprehensive recovery method for copper-molybdenum sulfide ores based on slurry potential regulation according to claim 1, characterized in that, The flotation reagents used in the copper-molybdenum roughing in step S2 and the copper-molybdenum scavenging in step S4 include: Foaming agent a: includes methyl isobutyl ester and methyl isobutyl methanol; Copper-molybdenum collectors include at least one of isobutyl xanthate, mercaptobenzothiazole, and ethyl isobutyl xanthate.

6. The comprehensive recovery method for copper-molybdenum sulfide ores based on slurry potential regulation according to claim 1, characterized in that, The flotation reagents used in the copper-molybdenum refining process in step S3 include: Gangue inhibitors include at least two of the following: cellulose derivatives, dextrin, starch, and sodium silicate; Copper-molybdenum collectors include at least one of isobutyl xanthate, mercaptobenzothiazole, and ethyl isobutyl xanthate. Foaming agent a: includes methyl isobutyl ester and methyl isobutyl methanol.

7. The comprehensive recovery method for copper-molybdenum sulfide ores based on slurry potential regulation according to any one of claims 1-6, characterized in that: The copper-molybdenum mixed tailings and the scavenging foam are returned as middlings to the copper-molybdenum roughing step for recycling.

8. The comprehensive recovery method for copper-molybdenum sulfide ore based on slurry potential regulation according to claim 1, characterized in that, In step S4, the adjustment potential for the third slurry potential adjustment is -120mV to -150mV; The slurry potential modifier used includes sulfuric acid.

9. The comprehensive recovery method for copper-molybdenum sulfide ore based on slurry potential regulation according to claim 1, characterized in that, In step S4, the sulfur flotation includes at least one roughing, one scavenging, and one cleaning step. The sulfur-refined tailings and sulfur-scavenging foam obtained are returned to the sulfur flotation step for recycling as middlings.

10. The comprehensive recovery method for copper-molybdenum sulfide ores based on slurry potential regulation according to claim 8, characterized in that, In step S4, the flotation reagents used in the sulfur flotation include: Foaming agent b: includes methyl isobutyl ester and methyl isobutyl methanol; Sulfur activators: including copper sulfate; Sulfur collectors: including isoamyl xanthate and butyl xanthate.