A composite coating for metal surface and its preparation method

By constructing a structure of metal substrate/zirconium-based conversion film/fluorine-modified silica-epoxy resin composite surface layer, the problem of easy structural damage of superhydrophobic coatings after wear is solved, realizing a superhydrophobic coating with good adhesion and long-term anti-corrosion performance at a small thickness, which is suitable for the protection of lightweight structural components.

CN123102599APending Publication Date: 2026-11-17NINGBO UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611234375.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing superhydrophobic coatings are prone to damage to their rough surface structure after wear, scratches, or localized collapse, leading to a rapid decline in hydrophobicity and corrosion resistance. Furthermore, traditional reinforcement methods result in thicker coatings, making it difficult to balance adhesion, scratch resistance, and long-term corrosion resistance with a relatively small total thickness.

Method used

The structure employs a metal substrate/zirconium-based conversion film/fluorine-modified silica-epoxy resin composite surface layer. The zirconium-based conversion film provides interfacial chemical anchoring and bottom layer sealing, the composite surface layer provides low surface energy and micro-nano rough structure, and the epoxy resin provides a continuous shielding phase, forming an ultrathin synergistic protection system.

Benefits of technology

With a total thickness of 1.0 μm to 4.0 μm, it achieves good interfacial adhesion, resistance to mechanical damage, and long-term corrosion protection, making it suitable for surface protection of metal parts subject to assembly friction, handling contact, or slight wear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102599A_ABST
    Figure CN123102599A_ABST
Patent Text Reader

Abstract

This invention discloses a composite coating for metal surfaces and its preparation method, belonging to the field of coating technology. The method includes the following steps: immersing a pretreated metal substrate in a preheated and diluted zirconium-based conversion solution, rinsing, and baking to obtain a metal substrate with a zirconium-based conversion film on its surface; spraying a composite coating solution onto the surface of the metal substrate with the zirconium-based conversion film, and curing to obtain a composite coating. By forming a zirconium-based conversion film in situ on the surface of a metal substrate such as an aluminum alloy, a stable interface is constructed using the chemical conversion film formation between the conversion film and the metal substrate; further, a superhydrophobic composite surface layer composed of epoxy resin, curing agent, and fluorine-modified inorganic oxide nanoparticles is constructed on top, thereby forming a bilayer ultrathin composite structure of zirconium-based conversion film / composite surface layer. This allows the formed composite coating to simultaneously possess good interfacial bonding strength, surface liquid repellency, and corrosion resistance while maintaining a relatively small total thickness of the zirconium-based conversion film and composite surface layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of coating technology, specifically relating to a composite coating for metal surfaces and its preparation method. Background Technology

[0002] Metallic materials are prone to corrosion failure in humid, saline, and acidic / alkaline environments. In engineering, organic coatings or conversion films are typically used to protect metal surfaces. Organic coatings can form a shielding layer to prevent corrosive media from contacting the metal substrate, while superhydrophobic surfaces, due to their excellent water-repellent and self-cleaning properties, are also widely used in metal corrosion protection. Generally, a superhydrophobic surface is considered to possess both a micro / nano-level rough structure and a low surface energy chemical composition. Significant superhydrophobic properties are observed when the water contact angle is greater than 150° and the slip angle is less than 10°.

[0003] Existing superhydrophobic coatings are mostly constructed through nanoparticle stacking, sol-gel deposition, and surface modification with fluorine-containing components. However, the superhydrophobic properties of these coatings are highly dependent on the integrity of the surface micro / nano structure. After wear, scratches, or localized collapse, the rough surface structure is easily destroyed, leading to a rapid decline in hydrophobic properties and corrosion resistance. In addition, the interaction between nanoparticles and metal substrates usually relies mainly on physical adsorption or mechanical intercalation, resulting in insufficient interfacial bonding. Therefore, they generally suffer from problems such as insufficient adhesion, poor scratch resistance, and easy peeling, especially in ultrathin systems.

[0004] Conversion coating technology is an important pretreatment method for metal surface treatment. It forms an inorganic film layer in situ on the metal surface through a chemical conversion reaction, which can improve the bonding state of the metal / organic coating interface and enhance the adhesion of subsequent coatings. Although traditional chromate conversion coatings have good protective properties, due to the environmental and health risks posed by hexavalent chromium, chromium-free alternatives are gradually becoming the development direction.

[0005] To improve the adhesion and mechanical stability of superhydrophobic coatings, existing technologies often introduce a relatively thick organic primer, such as epoxy primer, zinc-rich primer, or polyurethane primer, between the metal substrate and the superhydrophobic topcoat. While this approach can improve the overall mechanical properties and shielding capability of the film to some extent, it typically increases the system thickness significantly, making it difficult to meet the requirements of ultra-thin protective layers for precision components, lightweight structural parts, and dimensionally sensitive applications.

[0006] Therefore, although existing technologies have made improvements in terms of surface function construction, thick film primer enhancement and conversion film interface modification, they still cannot simultaneously resolve the contradiction between "insufficient adhesion of superhydrophobic coating" and "the increase in system thickness caused by traditional enhancement methods". There is still a lack of a superhydrophobic composite protection system that can take into account adhesion, scratch resistance and long-term corrosion protection performance under the condition of relatively small total thickness. Summary of the Invention

[0007] To address the aforementioned technical problems, this invention provides a composite coating for metal surfaces and a method for preparing the same.

[0008] In a first aspect, the present invention provides a composite coating for a metal surface, specifically comprising: Metal substrate; A composite surface layer composed of epoxy resin, curing agent, and fluorine-modified inorganic oxide nanoparticles; A zirconium-based conversion film is prepared by zirconium salt, fluorine-containing promoter and auxiliary film-forming components. The zirconium-based conversion film is generated in situ on the surface of the metal substrate and is located between the metal substrate and the composite surface layer. The total thickness of the composite coating is 1~4 μm.

[0009] Furthermore, in the composite surface layer, based on the total mass percentage of the solid components, the composite surface layer comprises: 25%–45% epoxy resin; 10%–20% curing agent; and 35%–60% fluorine-modified silica nanoparticles.

[0010] Furthermore, the average particle size of the fluorine-modified inorganic oxide nanoparticles is 5~20 nm.

[0011] Secondly, the present invention also provides a method for preparing the above-mentioned composite coating on a metal surface, specifically including the following steps: The pretreated metal substrate is immersed in a preheated zirconium-based conversion solution, washed with water, and then baked to obtain a metal substrate with a zirconium-based conversion film on its surface. The composite coating is obtained by spraying the composite coating liquid onto the surface of a metal substrate with a zirconium-based conversion film and curing it. The method for preparing the zirconium-based conversion solution includes: dissolving zirconium salt, fluorine-containing promoter and auxiliary film-forming components in deionized water, and adjusting the pH to obtain the zirconium-based conversion solution; The method for preparing the composite spraying liquid includes: dispersing epoxy resin in a volatile solvent, sequentially adding a curing agent and pre-prepared fluorine-modified inorganic oxide nanoparticles, and stirring to obtain the composite spraying liquid.

[0012] Zirconium-based conversion films are generated in situ through a chemical reaction between a zirconium-based conversion solution and the surface of a metal substrate. These films provide a stable interface and a shielding layer even at relatively thin thicknesses. The main functions of this layer are: firstly, to enhance the interfacial bonding strength between the metal substrate and the upper composite surface layer; secondly, to seal active sites, micropores, and local defects on the substrate surface to a certain extent; and thirdly, to serve as an interfacial support layer for subsequent organic layer deposition and curing, improving the overall stability of the composite system. The composite surface layer provides low surface energy and a micro / nano rough structure, while epoxy resin provides a continuous shielding phase. Fluorine-modified silica nanoparticles, dispersed in the epoxy resin matrix, form a surface structure with micro / nano-level roughness during curing. The fluorine-containing groups introduced on their surface significantly reduce surface energy, making it more difficult for surface droplets to spread and remain, thus creating a superhydrophobic effect. After curing, the epoxy resin forms a continuous organic network, which not only serves as a bonding medium between particles and between particles and the underlying layer but also acts as a physical shielding layer to prevent corrosive media such as water, oxygen, and ions from penetrating the substrate.

[0013] Furthermore, since the film quality of zirconium-based conversion films is closely related to the surface condition of the substrate, in order to ensure the uniformity of the coating and the interfacial bonding strength, the metal substrate undergoes a pretreatment step before film formation to remove surface oil, dust, natural oxide layers, and other impurities, and to improve surface reactivity. The pretreatment of the metal substrate specifically includes degreasing, cleaning, light etching, activation, and rinsing.

[0014] Preferably, the metal substrate can be degreased using an alkaline degreasing solution containing carbonates, silicates and / or surfactants, then rinsed with deionized water, and then subjected to appropriate activation treatment, so that the surface of the metal substrate is more conducive to the uniform growth of the subsequent zirconium-based conversion film. At the same time, the pretreated substrate should be protected from recontamination and should proceed to the conversion film formation step as soon as possible.

[0015] Furthermore, the metal substrate includes at least one of aluminum and its alloys, magnesium and its alloys, galvanized steel sheet and zinc-aluminum-magnesium coated steel sheet; preferably an aluminum alloy.

[0016] The method for preparing the zirconium-based conversion solution includes: dissolving zirconium salt, fluorine-containing promoter, and auxiliary film-forming components in deionized water, and adjusting the pH to obtain the zirconium-based conversion solution. Furthermore, the auxiliary film-forming components include metavanadate and manganese salt, which help improve the film structure and overall protective performance. Based on the mass percentage of the zirconium-based conversion solution stock solution, the zirconium-based conversion solution stock solution comprises: 0.6%–1.2% zirconium salt; 0.03%–0.15% fluorine-containing accelerator; 0.3%–0.8% metavanadate; 0.2%–4.0% manganese salt; and the balance being water.

[0017] When forming a zirconium-based conversion film in situ on a metal substrate, the zirconium-based conversion solution needs to be diluted. In this invention, the zirconium-based conversion solution is preferably diluted 4 to 6 times, and more preferably diluted to a working solution of 5 times, to balance film-forming activity, solution stability, and film uniformity. Meanwhile, based on the mass percentage of the original zirconium-based conversion solution, the contents of the zirconium salt, fluorine-containing accelerator, metavanadate, and manganese salt are controlled to be 0.6%–1.2%, 0.03%–0.15%, 0.3%–0.8%, and 0.2%–4.0%, respectively. Among these factors, excessively low zirconium salt content can lead to insufficient film coverage and poor continuity, while excessively high content can cause localized rapid deposition and uneven film formation. Insufficient fluorine-containing promoter content hinders substrate surface activation and uniform film nucleation, while excessive content can cause excessive substrate etching and reduce film density. Insufficient metavanadate content has limited effect on improving film densification and corrosion resistance, while excessive content may affect system stability and film uniformity. Insufficient manganese salt content has insufficient effect on film structure regulation, while excessive content may lead to increased byproduct deposition and affect interfacial bonding performance. Controlling each component within the above-mentioned ranges is beneficial for obtaining zirconium-based conversion films with uniform film formation, dense structure, good adhesion, and excellent corrosion resistance.

[0018] Furthermore, the zirconium salt includes hexafluorozirconate, which includes at least one of sodium hexafluorozirconate, potassium hexafluorozirconate, ammonium hexafluorozirconate, and lithium hexafluorozirconate.

[0019] Furthermore, the fluorinated accelerator includes at least one of sodium fluoride, potassium fluoride, ammonium fluoride, ammonium hydrogen fluoride, and hydrofluoric acid. The fluorinated accelerator can promote surface activation and film formation reactions.

[0020] Furthermore, the metavanadate is at least one of sodium metavanadate, potassium metavanadate, and ammonium metavanadate, and the manganese salt is at least one of manganese nitrate, manganese sulfate, and manganese chloride.

[0021] Furthermore, the pH adjustment range is 3.0 to 4.5; preferably, the pH value is 3.6.

[0022] The method for preparing the composite spraying liquid includes: dispersing epoxy resin in a volatile solvent, sequentially adding a curing agent and pre-prepared fluorine-modified inorganic oxide nanoparticles, and stirring to obtain the composite spraying liquid. The volatile solvent serves as both the dispersion medium and the spraying solvent, which helps control the system viscosity and the final film thickness; the epoxy resin acts as the film-forming framework and binder phase; the curing agent promotes resin crosslinking; and the fluorine-modified inorganic oxide nanoparticles provide the surface layer with low surface energy and a micro / nano rough structure.

[0023] Furthermore, the volatile solvent includes at least one of methanol, ethanol, n-propanol, isopropanol, and butanol.

[0024] Furthermore, in the preparation process of the composite spray liquid, the curing agent includes at least one of amine curing agents, polyamide curing agents, and modified amine curing agents. Preferably, the amine curing agent can be ethylenediamine, the polyamide curing agent can be type 650 polyamide or type 651 polyamide, and the modified amine curing agent can be Mannich modified amine or epoxy addition modified aliphatic amine.

[0025] Furthermore, the preparation method of the fluorine-modified inorganic oxide nanoparticles includes the following steps: A volatile solvent is mixed with a fluorinated silane, and the mixture is stirred to obtain a fluorinated silane premix. Inorganic oxide nanoparticles were added to an alkaline dispersion and dispersed evenly. Then, a fluorinated silane premix was added, and a surface modification reaction was carried out under programmed temperature conditions. After post-treatment, fluorine-modified inorganic oxide nanoparticles were obtained.

[0026] In this process, fluorinated silanes undergo hydrolysis and condensation reactions in a volatile organic solvent-alkaline dispersion system, and chemically combine with hydroxyl groups on the surface of inorganic oxide nanoparticles, introducing fluorinated low surface energy groups onto the surface of the nanoparticles. This provides a functional filler with low surface energy and micro-nano rough structure for subsequent composite surface layers.

[0027] The fluorinated silane includes perfluoroalkyltrialkoxysilanes, preferably at least one selected from 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorooctyltriethoxysilane, 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, and 1H,1H,2H,2H-perfluorodecyltriethoxysilane; preferably 1H,1H,2H,2H-perfluorodecyltrimethoxysilane.

[0028] The inorganic oxide nanoparticles are selected from at least one of silicon dioxide, aluminum oxide, titanium dioxide, and zirconium oxide; preferably, the inorganic oxide nanoparticles are silicon dioxide nanoparticles.

[0029] Preferably, in the preparation process of fluorine-modified inorganic oxide nanoparticles, the alkaline dispersion is an ammonia solution, which can be prepared by ammonium hydroxide and deionized water at a volume ratio of 1:(3-5), preferably at a volume ratio of 1:4.

[0030] Furthermore, in the process of preparing fluorine-modified inorganic oxide nanoparticles, the programmed temperature conditions are as follows: magnetic stirring at 30–50 °C for 16–24 h, followed by heating to 80–100 °C and stirring for another 4–8 h; preferably, magnetic stirring at 40 °C for 20 h, followed by heating to 90 °C and stirring for another 6 h.

[0031] Furthermore, based on the total mass percentage of the feed used to prepare fluorine-modified inorganic oxide nanoparticles, the volatile solvent is 60%–84.7%, the fluorinated silane is 0.3%–2.0%, the inorganic oxide nanoparticles are 2%–8%, and the alkaline dispersion is 13%–30%.

[0032] Furthermore, the preheating temperature is 35–55 °C, and the preheating time is 3–10 min. Preferably, the preheating temperature is 45 °C, and the preheating time is 5 min.

[0033] Furthermore, the baking temperature is 70–90 °C, and the baking time is 0.5–1.5 h. Preferably, baking is performed at 80 °C for 1 h. This baking treatment helps to stabilize the zirconium-based conversion film and provides a better adhesion base for the subsequent coating of the composite surface layer.

[0034] Furthermore, the composite coating liquid is sprayed onto the surface of the metal substrate on which the zirconium-based conversion film has been formed using a spray gun. The number of spraying times is 1 to 3, and the spraying time for each time is 10 to 20 seconds; preferably, 2 sprayings are performed, and the spraying time for each time is 15 seconds.

[0035] Furthermore, the curing temperature is 70–90 °C, and the curing time is 2–4 h; preferably, it is cured at 80 °C for 3 h.

[0036] During the spraying process, the thickness of the composite surface layer, the total thickness of the zirconium-based conversion film and the composite surface layer, and the uniformity of the film layer can be controlled by adjusting the spray gun nozzle diameter, spraying distance, atomization pressure, spraying time, and number of sprays. By combining a volatile solvent dilution system with short-time, multiple sprays, excessive surface layer buildup can be effectively avoided, thus maintaining a relatively small total thickness of the entire composite system. Preferably, the total thickness of the composite coating is controlled within 1.0–4.0 μm.

[0037] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention constructs a composite structure of “metal substrate / zirconium-based conversion film / fluorine-modified silica-epoxy resin composite surface layer” to achieve a synergistic protection system of “interface sealing + surface liquid repellency + resin shielding”. The zirconium-based conversion film provides interfacial chemical anchoring and bottom sealing, the composite surface layer provides low surface energy and micro-nano rough structure, and the epoxy resin provides a continuous shielding phase. The three work together to achieve long-term stable protection of the metal substrate. Under the condition that the total thickness of the zirconium-based conversion film and the composite surface layer is 1.0 μm~4.0 μm, it can simultaneously have good interfacial adhesion, mechanical damage resistance and long-term anti-corrosion performance. Compared with ordinary nanoparticle type superhydrophobic films, this invention is more suitable for surface protection of metal parts that are subject to assembly friction, handling contact or slight wear risk.

[0038] (2) The preparation process of this invention mainly includes substrate pretreatment, zirconium-based conversion film formation, composite spraying, and thermosetting. The process flow is clear, and the required equipment mainly consists of conventional chemical treatment devices and spraying and curing equipment, which facilitates integration with existing metal surface treatment or spraying production lines. The zirconium-based conversion film can be formed through conventional impregnation conversion, and the composite surface layer can be obtained through rapid spraying and thermosetting with a spray gun, providing a good foundation for mass production and continuous implementation. Therefore, this invention is not only suitable for laboratory research but also has the potential for further industrial application. Attached Figure Description

[0039] Figure 1 The surface state of the product in Example 1 of this invention after 400 hours of salt spray; Figure 2 This is a photograph of the surface hydrophobicity of the product in Example 1 of this invention after 400 hours of salt spray. Figure 3 This is the surface state of the blank substrate control sample of Comparative Example 1 of the present invention after 2 h of salt spray. Figure 4 The surface state of the sample with only zirconium-based conversion film formed in Comparative Example 2 after 48 hours of salt spray test; Figure 5 The surface condition of the composite surface layer sample (comparative example 3) after 36 hours of salt spraying is shown. Figure 6 For Comparative Example 4, the surface state of the sample after 132 h of salt spray after applying a zirconium-based conversion film followed by spraying with a surface layer of fluorine-free modified silica nanoparticles. Figure 7 The cross-sectional morphology of the product in Embodiment 1 of the present invention shows that the total coating thickness is approximately 1.5 μm. Detailed Implementation

[0040] To enable those skilled in the art to better understand and implement the technical solutions of this invention, the invention will be further described below with reference to specific embodiments and accompanying drawings. It should be understood that the following embodiments are for illustrative purposes only and are not intended to limit the scope of protection of this invention. All equivalent substitutions, improvements, and modifications made within the spirit and principles of this invention should be included within the scope of protection of this invention.

[0041] Unless otherwise specified, all reagents used in this invention are commercially available, and all methods used are conventional techniques in the art.

[0042] This invention provides a method for preparing a composite coating on a metal surface, mainly including the preparation of a zirconium-based conversion solution, the preparation of fluorine-modified inorganic oxide nanoparticles, the preparation of a composite spraying solution, and the construction of the composite coating. In a preferred embodiment of this invention, the inorganic oxide nanoparticles are preferably silica nanoparticles.

[0043] I. Preparation of Zirconium-based conversion solution: The preparation method of zirconium-based conversion solution is as follows: Zirconium salt, fluorine-containing accelerator, and auxiliary film-forming components are added to deionized water and stirred until fully dissolved. The pH of the solution is adjusted to 3.0–4.5, preferably 3.6, to obtain the zirconium-based conversion solution stock solution. Preferably, the zirconium-based conversion solution stock solution comprises, by mass percentage: 0.6%–1.2% zirconium salt; 0.03%–0.15% fluorine-containing accelerator; 0.3%–0.8% metavanadate; 0.2%–4.0% manganese salt; and the balance being water. In practical use, the zirconium-based conversion solution stock solution is diluted 4–6 times with deionized water, preferably to a 5-fold dilution, to balance film-forming activity, solution stability, and film uniformity, before being used for conversion treatment on metal substrate surfaces.

[0044] II. Preparation of Fluorine-Modified Silica Nanoparticles The preparation method of fluorine-modified silica nanoparticles is as follows: First, a volatile solvent is mixed with a fluorinated silane and premixed under stirring for 0.5–2 h to obtain a fluorinated silane premix. Then, inorganic oxide nanoparticles are added to an alkaline dispersion for dispersion, preferably by ultrasonic dispersion, for 20–40 min to obtain an inorganic oxide nanoparticle dispersion. The inorganic oxide nanoparticles are preferably selected from one or more of silica, alumina, titanium dioxide, and zirconium oxide, more preferably silica nanoparticles. The alkaline dispersion is preferably an ammonia solution, which can be prepared by mixing ammonium hydroxide and deionized water at a volume ratio of 1:(3–5), preferably 1:4.

[0045] Subsequently, the fluorinated silane premix was added to the inorganic oxide nanoparticle dispersion, and a surface modification reaction was carried out under programmed temperature conditions. Preferably, the first stage reaction temperature was 30–50 °C, and the reaction time was 16–24 h; the second stage reaction temperature was 80–100 °C, and the reaction time was 4–8 h. During this process, the fluorinated silane underwent hydrolysis and condensation reactions in the volatile organic solvent-alkaline dispersion system, and chemically bonded with the hydroxyl groups on the surface of the inorganic oxide nanoparticles, introducing fluorinated low surface energy groups onto the particle surface. After the reaction, the resulting product was filtered, washed, and dried to obtain fluorinated inorganic oxide nanoparticles.

[0046] Preferably, in the preparation of fluorine-modified inorganic oxide nanoparticles, the volatile solvent is 60%–84.7%, the fluorinated silane is 0.3%–2.0%, the inorganic oxide nanoparticles are 2%–8%, and the alkaline dispersion is 13%–30%, based on the total mass percentage of the feed for preparing fluorine-modified inorganic oxide nanoparticles.

[0047] III. Preparation of Composite Spraying Liquid The preparation method of the composite spraying liquid is as follows: Epoxy resin is added to a volatile solvent and stirred for 10–20 min to fully disperse or dissolve it; then a curing agent is added and stirring is continued for 10–20 min; then pre-prepared fluorine-modified inorganic oxide nanoparticles are added and stirring is continued for 30–60 min to uniformly disperse them, thus obtaining a composite spraying liquid.

[0048] Preferably, based on the total mass percentage of the solid components in the composite surface layer, the composite surface layer comprises: 25%~45% epoxy resin; 10%~20% curing agent; and 35%~60% fluorine-modified silica nanoparticles. The volatile solvent is used to adjust the viscosity of the system and the spraying performance; the epoxy resin serves as the film-forming skeleton and binder phase; the curing agent promotes resin crosslinking; and the fluorine-modified inorganic oxide nanoparticles impart a lower surface energy and a micro / nano rough structure to the composite surface layer.

[0049] IV. Preparation of Composite Coatings The specific steps for preparing the composite coating are as follows: First, the prepared zirconium-based conversion solution is preheated, preferably at a temperature of 35–55 °C for 3–10 min. Then, the pretreated metal substrate is immersed in the zirconium-based conversion solution for conversion treatment, preferably for 3–10 min. After treatment, the sample is removed and rinsed with deionized water to remove any residual solution. The sample is then baked at 70–90 °C for 0.5–1.5 h to obtain a metal substrate with a zirconium-based conversion film. Next, the composite coating is sprayed onto the surface of the metal substrate with the zirconium-based conversion film using a spray gun, preferably 1–3 times, with each spraying session lasting 10–20 s. After spraying, the sample is cured at 70–90 °C for 2–4 h to obtain the final composite coating.

[0050] During the spraying process, the thickness of the composite surface layer, the total thickness of the composite coating, and the uniformity of the film can be controlled by adjusting the spray gun nozzle diameter, spraying distance, atomization pressure, spraying time, and number of sprays. Preferably, combining a volatile solvent dilution system with short-time, multiple sprays can effectively prevent excessive surface layer buildup, thereby maintaining a relatively small total thickness of the entire composite system. Preferably, the total thickness of the composite coating is controlled within the range of 1.0–4.0 μm.

[0051] Example 1 Preparation of Zirconium-based Conversion Solution: Taking the preparation of 1 L of zirconium-based conversion solution stock solution as an example, weigh out 9 g of potassium fluorozirconate, 0.75 g of sodium fluoride, 5 g of sodium metavanadate, and 4 g of manganese nitrate, add them to 800 mL of deionized water and stir thoroughly to dissolve. Adjust the pH of the solution to 3.6, and then dilute to 1 L with deionized water to obtain the zirconium-based conversion solution stock solution. Based on the mass percentage of the zirconium-based conversion solution stock solution, the zirconium-based conversion solution stock solution contains approximately 0.9% potassium fluorozirconate, approximately 0.075% sodium fluoride, approximately 0.5% sodium metavanadate, approximately 0.4% manganese nitrate, and the remainder is water. Before use, dilute the zirconium-based conversion solution stock solution 5 times with deionized water to obtain a 20% zirconium-based conversion solution working solution for later use.

[0052] Preparation of fluorine-modified silica nanoparticles: Based on the total mass of the feed, 100 g of ethanol and 1 g of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane were mixed and stirred under magnetic stirring for 1 h to obtain a fluorine-containing silane premix. 5 g of silica nanoparticles were added to 30 g of ammonia solution and ultrasonically dispersed for 30 min. The ammonia solution was prepared by mixing ammonium hydroxide and deionized water at a volume ratio of 1:4. The fluorine-containing silane premix and the ammonia solution of silica were mixed and magnetically stirred at 40 °C for 20 h, then heated to 90 °C and stirred for another 6 h. After the reaction, the resulting product was filtered, washed, and dried to obtain fluorine-modified silica nanoparticles with an average particle size of 10 nm. Based on the total mass percentage of the feed for preparing fluorine-modified silica nanoparticles, ethanol accounted for approximately 73.5%, fluorine-containing silane for approximately 0.7%, silica nanoparticles for approximately 3.7%, and ammonia solution for approximately 22.1%.

[0053] Preparation of the composite spraying solution: 0.4 g of epoxy resin was added to 10 mL of ethanol and stirred for 15 min to ensure complete dispersion or dissolution; then 0.2 g of ethylenediamine was added and stirring was continued for 15 min; next, 0.6 g of pre-prepared fluorine-modified silica nanoparticles were added and stirring was continued for 50 min to obtain a uniform composite spraying solution. Based on the total mass percentage of solid components in the composite surface layer, the epoxy resin in the composite surface layer is approximately 33.3%, the curing agent is approximately 16.7%, and the fluorine-modified silica nanoparticles are approximately 50.0%.

[0054] Preparation of the composite coating: The substrate was degreased using an alkaline degreasing agent specifically for aluminum alloys, then rinsed with deionized water, and subsequently activated to complete the pretreatment of the aluminum alloy substrate. A 20% zirconium-based conversion solution was heated to 45°C and preheated for 5 minutes, and the pretreated metal substrate was immersed in the solution for 5 minutes. After treatment, the sample was removed and rinsed with deionized water. The sample was then baked at 80°C for 1 hour to obtain a metal substrate with a zirconium-based conversion film on its surface. The superhydrophobic composite coating solution was sprayed onto the surface of the metal substrate with the zirconium-based conversion film using a spray gun, with two spraying operations, each lasting 15 seconds. After spraying, the sample was cured at 80°C for 3 hours to obtain the final composite coating with a thickness of 1.5 μm. The cross-sectional morphology of the product is as follows. Figure 7 As shown.

[0055] Example 2 Preparation of Zirconium-based Conversion Solution: Taking the preparation of 1 L of zirconium-based conversion solution stock solution as an example, weigh out 6 g of potassium fluorozirconate, 0.3 g of sodium fluoride, 3 g of sodium metavanadate, and 2 g of manganese nitrate, add them to approximately 800 mL of deionized water and stir thoroughly to dissolve. Adjust the pH of the solution to 3.0, and then dilute to 1 L with deionized water to obtain the zirconium-based conversion solution stock solution. Based on the mass percentage of the zirconium-based conversion solution stock solution, the zirconium-based conversion solution stock solution contains approximately 0.6% potassium fluorozirconate, approximately 0.03% sodium fluoride, approximately 0.3% sodium metavanadate, approximately 0.2% manganese nitrate, and the remainder is water. Before use, dilute the zirconium-based conversion solution stock solution 4 times with deionized water to obtain a 25% zirconium-based conversion solution working solution for later use.

[0056] Preparation of fluorine-modified silica nanoparticles: Based on the total mass percentage of the feed materials for preparing fluorine-modified silica nanoparticles, 84.7 g of ethanol and 0.3 g of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane were mixed and stirred under magnetic stirring for 0.5 h to obtain a fluorine-containing silane premix. 2.0 g of silica nanoparticles with an average particle size of 5 nm were added to 13.0 g of ammonia solution and ultrasonically dispersed for 20 min, wherein the ammonia solution was prepared by mixing ammonium hydroxide and deionized water at a volume ratio of 1:5. Subsequently, the fluorine-containing silane premix was added to the silica-ammonia dispersion and magnetically stirred at 30 ℃ for 16 h, and then the temperature was raised to 80 ℃ and stirred for another 4 h. After the reaction was completed, the obtained product was filtered, washed and dried to obtain fluorine-modified silica nanoparticles. Based on the total mass percentage of the ingredients, ethanol accounts for 84.7%, fluorinated silanes account for 0.3%, silica nanoparticles account for 2.0%, and alkaline dispersion accounts for 13.0%.

[0057] Preparation of the composite spraying liquid: 0.45 g of epoxy resin was added to 10 mL of ethanol and stirred for 10 min to ensure complete dispersion or dissolution; then 0.20 g of type 650 polyamide curing agent was added, and stirring was continued for 10 min; next, 0.35 g of pre-prepared fluorine-modified silica nanoparticles were added, and stirring was continued for 30 min to obtain a uniform composite spraying liquid. Based on the total mass percentage of solid components in the composite surface layer, the epoxy resin constitutes approximately 45%, the curing agent approximately 20%, and the fluorine-modified silica nanoparticles approximately 35.0%.

[0058] Preparation of the composite coating: The aluminum alloy substrate was degreased using an alkaline degreasing solution formulated with sodium carbonate, sodium metasilicate, and a nonionic surfactant. The substrate was then rinsed with deionized water and activated to complete the pretreatment. A 20% zirconium-based conversion solution was heated to 35 °C and preheated for 3 min. The pretreated aluminum alloy substrate was then immersed in the solution for 3 min. After treatment, the sample was removed and rinsed with deionized water. The sample was then baked at 70 °C for 0.5 h to obtain a metal substrate with a zirconium-based conversion film. The composite coating solution was sprayed onto the surface of the metal substrate with the zirconium-based conversion film using a spray gun, with each spraying session lasting 10 s. After spraying, the sample was cured at 70 °C for 2 h to obtain the final composite coating, with a total thickness of approximately 1.0 μm.

[0059] Example 3 Preparation of Zirconium-based Conversion Solution: Taking the preparation of 1 L of zirconium-based conversion solution stock solution as an example, weigh 12 g of potassium fluorozirconate, 1.5 g of sodium fluoride, 8 g of sodium metavanadate, and 40 g of manganese nitrate, add them to approximately 800 mL of deionized water and stir thoroughly to dissolve. Adjust the pH of the solution to 4.5, and then dilute to 1 L with deionized water to obtain the zirconium-based conversion solution stock solution. Based on the mass percentage of the zirconium-based conversion solution stock solution, the zirconium-based conversion solution stock solution contains approximately 1.2% potassium fluorozirconate, approximately 0.15% sodium fluoride, approximately 0.8% sodium metavanadate, approximately 4.0% manganese nitrate, and the remainder is water. Before use, dilute the zirconium-based conversion solution stock solution 6 times with deionized water.

[0060] Preparation of fluorine-modified silica nanoparticles: Based on the total mass percentage of the feed materials for preparing fluorine-modified silica nanoparticles, 60 g of isopropanol and 2 g of 1H,1H,2H,2H-perfluorooctyltriethoxysilane were mixed and stirred under magnetic stirring for 2 h to obtain a fluorine-containing silane premix. 8 g of silica nanoparticles with an average particle size of 20 nm were added to 30 g of ammonia solution and ultrasonically dispersed for 40 min. The ammonia solution was prepared by mixing ammonium hydroxide and deionized water at a volume ratio of 1:3. Subsequently, the fluorine-containing silane premix was added to the silica-ammonia dispersion, and the mixture was magnetically stirred at 50 ℃ for 24 h, then heated to 100 ℃ and stirred for another 8 h. After the reaction was completed, the resulting product was filtered, washed, and dried to obtain fluorine-modified silica nanoparticles. Based on the total mass percentage of the feed materials, isopropanol accounted for 60.0%, fluorine-containing silane for 2.0%, silica nanoparticles for 8.0%, and the alkaline dispersion for 30.0%.

[0061] Preparation of the composite spraying liquid: 0.25 g of epoxy resin was added to 10 mL of ethanol and stirred for 20 min to ensure complete dispersion or dissolution; then 0.15 g of type 651 polyamide curing agent was added, and stirring was continued for 20 min; then 0.60 g of pre-prepared fluorine-modified silica nanoparticles were added, and stirring was continued for 60 min to obtain a uniform composite spraying liquid. Based on the total mass percentage of solid components in the composite surface layer, the epoxy resin content is approximately 25.0%, the curing agent content is approximately 15.0%, and the fluorine-modified silica nanoparticles content is approximately 60.0%.

[0062] Preparation of the composite coating: The aluminum alloy substrate was degreased using an alkaline degreasing solution formulated with sodium carbonate, sodium metasilicate, and a nonionic surfactant. The substrate was then rinsed with deionized water and activated to complete the pretreatment. The prepared zirconium-based conversion solution was heated to 55 °C and preheated for 10 min. The pretreated aluminum alloy substrate was then immersed in the solution for 10 min. After treatment, the sample was removed and rinsed with deionized water. The sample was then baked at 90 °C for 1.5 h to obtain a metal substrate with a zirconium-based conversion film. The composite coating solution was sprayed onto the surface of the metal substrate with the zirconium-based conversion film using a spray gun, with three coats applied, each lasting 20 s. After spraying, the sample was cured at 90 °C for 4 h to obtain the final composite coating, with a total thickness of approximately 4.0 μm.

[0063] Example 4 Preparation of Zirconium-based Conversion Solution: Taking the preparation of 1 L of zirconium-based conversion solution stock solution as an example, weigh out 10 g of ammonium hexafluorozirconate, 1.0 g of ammonium fluoride, 6 g of ammonium metavanadate, and 10 g of manganese sulfate, add them to approximately 800 mL of deionized water and stir thoroughly to dissolve. Adjust the pH of the solution to 4.0, and then dilute to 1 L with deionized water to obtain the zirconium-based conversion solution stock solution. Based on the mass percentage of the zirconium-based conversion solution stock solution, the zirconium-based conversion solution stock solution contains approximately 1.0% ammonium hexafluorozirconate, approximately 0.10% ammonium fluoride, approximately 0.6% ammonium metavanadate, approximately 1.0% manganese sulfate, and the remainder is water. Before use, dilute the zirconium-based conversion solution stock solution 5 times with deionized water to obtain a 20% zirconium-based conversion solution working solution for later use.

[0064] Preparation of fluorine-modified silica nanoparticles: Based on the total mass percentage of the feed materials for preparing fluorine-modified silica nanoparticles, 75.0 g of n-propanol and 1.2 g of 1H,1H,2H,2H-perfluorooctyltriethoxysilane were mixed and stirred under magnetic stirring for 1.5 h to obtain a fluorine-containing silane premix. 6.0 g of silica nanoparticles with an average particle size of 15 nm were added to 17.8 g of ammonia solution and ultrasonically dispersed for 30 min, wherein the ammonia solution was prepared by mixing ammonium hydroxide and deionized water at a volume ratio of 1:4. Subsequently, the fluorine-containing silane premix was added to the silica-ammonia dispersion and magnetically stirred at 40 ℃ for 20 h, and then the temperature was raised to 90 ℃ and stirred for another 6 h. After the reaction was completed, the obtained product was filtered, washed and dried to obtain fluorine-modified silica nanoparticles. Based on the total mass percentage of the feed, n-propanol accounts for 75.0%, fluorinated silanes for 1.2%, silica nanoparticles for 6.0%, and alkaline dispersion for 17.8%.

[0065] Preparation of the composite spraying liquid: 0.40 g of epoxy resin was added to 10 mL of ethanol and stirred for 15 min to ensure complete dispersion or dissolution; then 0.10 g of modified amine curing agent was added, and stirring was continued for 15 min; next, 0.50 g of pre-prepared fluorine-modified silica nanoparticles were added, and stirring was continued for 45 min to obtain a uniform composite spraying liquid. Based on the total mass percentage of solid components in the composite surface layer, the epoxy resin comprises approximately 40%, the curing agent approximately 10%, and the fluorine-modified silica nanoparticles approximately 50%.

[0066] Preparation of the composite coating: The galvanized steel substrate was degreased using an alkaline degreasing solution prepared with sodium carbonate, sodium metasilicate, and a nonionic surfactant. After rinsing with deionized water, the substrate underwent activation treatment to complete the pretreatment. The prepared zirconium-based conversion solution was heated to 45 °C and preheated for 6 min. The pretreated galvanized steel substrate was then immersed in the solution for 6 min. After treatment, the sample was removed and rinsed with deionized water. The sample was then baked at 80 °C for 1 h to obtain a metal substrate with a zirconium-based conversion film. The composite coating solution was sprayed onto the surface of the metal substrate with the zirconium-based conversion film using a spray gun, with two spraying passes, each lasting 15 s. After spraying, the sample was cured at 85 °C for 3 h to obtain the final composite coating, with a total thickness of approximately 2.5 μm.

[0067] Comparative Example 1 An aluminum alloy substrate that has undergone conventional cleaning treatment was selected as a blank substrate control sample without the application of zirconium-based conversion film or composite surface layer.

[0068] Comparative Example 2 Unlike Example 1, the aluminum alloy substrate was treated according to the zirconium-based conversion film preparation steps in Example 1 to form a zirconium-based conversion film, without spraying a composite surface layer.

[0069] Comparative Example 3 Unlike Example 1, no zirconium-based conversion coating treatment was performed; instead, the prepared composite coating liquid was directly sprayed onto the surface of the aluminum alloy substrate.

[0070] Comparative Example 4 Unlike Example 1, fluorine-modified silica nanoparticles were not added to the topcoat formulation after the zirconium-based conversion film was applied.

[0071] Test methods This invention applies relevant performance tests to the products obtained in the above embodiments and comparative examples, including abrasion resistance tests, hydrophobicity tests, and corrosion resistance tests. Specifically, the abrasion resistance is tested using a sandpaper abrasion test, the hydrophobicity is tested using the water contact angle and sliding angle, and the corrosion resistance is tested using a neutral salt spray test. The water contact angles after abrasion in Table 1 are the results obtained for each sample after the same preset number of abrasion cycles to ensure comparability between different samples. If necessary, electrochemical impedance spectroscopy can be used to further evaluate the corrosion resistance of the products.

[0072] Test Example 1 The abrasion resistance of the product is tested using a sandpaper abrasion test: the sample is placed face down on a fixed sandpaper surface, a certain load is applied to the sample, and the sample is rubbed back and forth or unidirectionally along the sandpaper surface to evaluate the abrasion resistance of the composite coating. Preferably, 1000-grit sandpaper can be used as the abrasive, a 100 g load is applied to the sample surface, and moving 10 cm along the sandpaper surface constitutes one abrasion cycle. After abrasion treatment according to a preset number of cycles, the change in the water contact angle of the sample surface is measured, or the maximum number of abrasion cycles corresponding to the sample surface still maintaining a superhydrophobic state is recorded. Preferably, the water contact angle after the same number of abrasion cycles or the number of abrasion cycles maintaining a superhydrophobic state is used as the abrasion resistance evaluation parameter.

[0073] Test Example 2 The hydrophobic properties of the product were tested using water contact angle and sliding angle: A contact angle meter was used to test the hydrophobic properties of the sample surface. During the test, a certain volume of deionized water droplet (preferably 5 μL) was placed on the sample surface, and the static water contact angle was measured. Then, the sample was slowly tilted, and the tilt angle at which the droplet began to roll was recorded as the sliding angle. Preferably, at least three different locations were selected for parallel testing of each sample, and the average value was taken as the final result. Preferably, the static water contact angle and sliding angle were used as parameters for evaluating hydrophobic properties.

[0074] Test Example 3 The corrosion resistance of products is tested using a neutral salt spray test: The corrosion resistance of samples is evaluated using a neutral salt spray test. Samples are placed in a salt spray chamber, and a 5 wt.% NaCl solution is used as the spray medium. A continuous salt spray corrosion test is conducted at 35°C. The surface condition of the samples is observed at preset time intervals, and the time when obvious corrosion, blistering, peeling, or failure occurs is recorded. Alternatively, the degree of corrosion on the sample surface is compared after a specified salt spray test time. Preferably, the salt spray resistance time is used as the evaluation parameter for corrosion resistance.

[0075] The test data are shown in Table 1: Table 1 Performance data of the examples and comparative examples From Table 1 and Figures 1-3As shown, Comparative Example 1 is an untreated blank aluminum alloy substrate with a water contact angle of only 75.4° and a sliding angle greater than 90°, exhibiting no hydrophobic properties whatsoever. Its salt spray resistance time is only 2 hours, indicating that the blank aluminum alloy substrate is highly susceptible to corrosion failure in salt-containing corrosive environments. In contrast, the composite coating prepared in Example 1 has a water contact angle as high as 163.8° and a sliding angle as low as 4.5°, achieving a superhydrophobic state. Its salt spray resistance time is as long as 400 hours, 200 times that of the blank substrate. This comparative result fully demonstrates that the bilayer structure of "zirconium-based conversion film + fluorine-modified silica-epoxy resin composite surface layer" constructed in this invention can significantly improve the surface hydrophobicity and corrosion resistance of metal substrates, achieving effective protection for the metal substrate.

[0076] From Table 1 and Figure 4 As shown, Comparative Example 2 only forms a zirconium-based conversion film on the aluminum alloy surface, with a film thickness of approximately 0.1 μm. Its water contact angle is 98.6°, and its sliding angle is greater than 90°, indicating a lack of hydrophobicity. The salt spray resistance time is 48 h, which is an improvement over the blank substrate, but the protective effect remains very limited. Example 1 further constructs a composite surface layer on top of the zirconium-based conversion film, increasing the water contact angle by 65.2° to achieve superhydrophobicity, reducing the sliding angle from greater than 90° to 4.5°, and increasing the salt spray resistance time from 48 h to 400 h, an increase of approximately 8.3 times. This comparison shows that although the zirconium-based conversion film can provide some underlying protection and interface improvement, it cannot impart superhydrophobic properties to the surface when used alone, and its corrosion resistance is also relatively limited. Only through synergy with a composite surface layer can excellent liquid repellency and long-term corrosion protection be achieved simultaneously.

[0077] From Table 1 and Figure 5As shown, Comparative Example 3 did not undergo zirconium-based conversion coating treatment; instead, a composite surface layer was directly sprayed onto the aluminum alloy surface. The film thickness was approximately 1.2 μm, with an initial water contact angle of 151.3°. Although the static water contact angle exceeded 150°, the sliding angle was 12.4°, failing to meet the superhydrophobic standard (sliding angle <10°). After wear, the water contact angle decreased to 138.5°, indicating poor wear resistance. The salt spray resistance time was only 36 h, even lower than Comparative Example 2, which only contained a zirconium-based conversion coating. Example 1, by introducing a zirconium-based conversion coating as an intermediate layer, achieved a water contact angle increase of 12.5° and a sliding angle decrease of 7.9°, while maintaining a total film thickness (1.5 μm) comparable to Comparative Example 3 (1.2 μm). After wear, the water contact angle increased by 15.7°, and the salt spray resistance time significantly increased from 36 h to 400 h, an improvement of more than 10 times. This comparison fully demonstrates that the introduction of zirconium-based conversion film can significantly enhance the interfacial bonding strength between the composite surface layer and the metal substrate. It not only improves the initial hydrophobicity of the coating, but more importantly, it greatly improves the wear resistance and corrosion resistance of the coating, solving the technical problems of insufficient adhesion, easy peeling, and poor corrosion resistance of single superhydrophobic coatings.

[0078] From Table 1 and Figure 6 As shown, Comparative Example 4, after applying a zirconium-based conversion film, was coated with a surface layer containing no fluorine-modified silica nanoparticles. The total film thickness was approximately 1.0 μm, with a water contact angle of only 97.4° and a sliding angle greater than 90°, completely lacking superhydrophobic properties. Its salt spray resistance time was 132 h, which, although improved compared to Comparative Examples 2 and 3, was still far lower than Example 1. Example 1, by introducing fluorine-modified silica nanoparticles into the composite surface layer, achieved a water contact angle increased by 66.4° and a sliding angle decreased from greater than 90° to 4.5°, achieving superhydrophobic properties, while maintaining a film thickness (1.5 μm) comparable to Comparative Example 4 (1.0 μm). Its salt spray resistance time increased from 132 h to 400 h, an increase of approximately 3.0 times. This comparison shows that fluorine-modified silica nanoparticles are a key component in constructing superhydrophobic surface micro-nano rough structures and low surface energy. They not only endow the coating with excellent liquid repellency, but also synergistically form a more complete shielding structure with the epoxy resin matrix, further improving the corrosion resistance of the coating.

[0079] Based on the above individual comparison results, the following overall conclusions can be drawn: Significant synergistic effect: This invention achieves synergistic effects among its components by constructing a two-layer ultrathin composite structure of "metal substrate / zirconium-based conversion film / fluorine-modified silica-epoxy resin composite surface layer". The zirconium-based conversion film provides interfacial chemical anchoring and bottom sealing, the composite surface layer provides low surface energy and micro-nano rough structure, and the epoxy resin provides a continuous shielding phase. The synergistic effect of these three components enables the composite coating to simultaneously possess excellent interfacial adhesion, superhydrophobic properties, and long-term corrosion resistance under ultrathin conditions.

[0080] Excellent and stable superhydrophobic properties: The composite coatings prepared in the embodiments of this invention all have water contact angles above 156° and sliding angles below 9°, achieving a superhydrophobic state. Among them, Example 1 has a water contact angle as high as 163.8° and a sliding angle as low as 4.5°, exhibiting the best superhydrophobic performance. After a sandpaper abrasion test, the water contact angle of Example 1 still remained at 154.2°, indicating that the superhydrophobic properties of the composite coating of this invention have good wear resistance stability and can continue to play a liquid-repellent and self-cleaning role in scenarios with slight wear.

[0081] Significantly improved corrosion resistance: The salt spray resistance time of the composite coating of this invention is significantly better than that of the comparative examples. Example 1 shows a salt spray resistance time of up to 400 hours, which is 200 times that of the blank substrate (2 hours), 8.3 times that of the zirconium-based conversion film alone (48 hours), 11.1 times that of the composite surface layer alone (36 hours), and 3.0 times that of the composite coating without nanoparticles (132 hours). This result fully demonstrates that the double-layer composite structure of this invention can effectively block the penetration of corrosive media into the metal substrate, significantly improving the corrosion resistance life of the metal material.

[0082] The ultra-thin system offers significant advantages: the total thickness of the composite coating in this invention is only 1.0~4.0 μm, classifying it as an ultra-thin protective system. At this thickness, this invention simultaneously achieves excellent adhesion, superhydrophobicity, and corrosion resistance, successfully resolving the contradiction between "insufficient adhesion of superhydrophobic coatings" and "the increase in system thickness caused by traditional reinforcement methods" in existing technologies. It is particularly suitable for precision components, lightweight structural parts, and applications sensitive to dimensional tolerances.

[0083] The process is highly feasible: The preparation process of this invention mainly includes substrate pretreatment, zirconium-based conversion into film, composite spraying and thermosetting, etc. The process flow is clear, and the required equipment are all conventional chemical treatment devices and spraying and curing equipment, which can be easily connected with existing metal surface treatment or spraying production lines, and has good prospects for mass production and industrial application.

[0084] In summary, the metal surface composite coating and its preparation method provided by this invention, through the synergistic effect of zirconium-based conversion film and fluorine-modified inorganic oxide nanoparticle-epoxy resin composite surface layer, simultaneously achieve excellent interfacial bonding strength, superhydrophobic properties, wear resistance stability and long-term corrosion resistance in an ultrathin system, which has significant technological progress and practical value.

[0085] It should be noted that when numerical ranges are involved in this invention, it should be understood that both endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as in the embodiments, preferred embodiments are described in this invention to avoid redundancy. Although preferred embodiments of this invention have been described, those skilled in the art, once they understand the inventive concept of this invention, can make other changes and modifications to these embodiments, and all such changes and modifications fall within the scope of this invention.

[0086] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. If such modifications and variations fall within the scope of equivalents of this invention, then this invention also intends to include these modifications and variations.

Claims

1. A composite coating for a metal surface, characterized in that, include: Metal substrate; A composite surface layer composed of epoxy resin, curing agent, and fluorine-modified inorganic oxide nanoparticles; A zirconium-based conversion film is prepared by zirconium salt, fluorine-containing promoter and auxiliary film-forming components. The zirconium-based conversion film is generated in situ on the surface of the metal substrate and is located between the metal substrate and the composite surface layer. The total thickness of the composite coating is 1.0~4.0 μm.

2. The composite coating according to claim 1, characterized in that, The composite surface layer comprises, by weight percentage of the total solid components, 25-45% epoxy resin, 10-20% curing agent, and 35-60% fluorine-modified silica nanoparticles.

3. The composite coating according to claim 1, characterized in that, The average particle size of the fluorine-modified inorganic oxide nanoparticles is 5~20 nm.

4. The method for preparing a composite coating on a metal surface according to any one of claims 1 to 3, characterized in that, Includes the following steps: The pretreated metal substrate is immersed in a preheated zirconium-based conversion solution, washed with water, and then baked to obtain a metal substrate with a zirconium-based conversion film on its surface. The composite coating is obtained by spraying the composite coating liquid onto the surface of a metal substrate with a zirconium-based conversion film and curing it. The method for preparing the zirconium-based conversion solution includes: dissolving zirconium salt, fluorine-containing promoter, and auxiliary film-forming components in deionized water, and adjusting the pH to obtain the zirconium-based conversion solution; The method for preparing the composite spraying liquid includes: dispersing epoxy resin in a volatile solvent, sequentially adding a curing agent and pre-prepared fluorine-modified inorganic oxide nanoparticles, and stirring to obtain the composite spraying liquid.

5. The preparation method according to claim 4, characterized in that, The preparation method of the fluorine-modified inorganic oxide nanoparticles includes the following steps: A volatile solvent is mixed with a fluorinated silane, and the mixture is stirred to obtain a fluorinated silane premix. Inorganic oxide nanoparticles were added to an alkaline dispersion and dispersed evenly. Then, a fluorinated silane premix was added, and a surface modification reaction was carried out under programmed temperature conditions. After post-treatment, fluorine-modified inorganic oxide nanoparticles were obtained.

6. The preparation method according to claim 5, characterized in that, Based on the total mass percentage of the feed materials used to prepare fluorine-modified inorganic oxide nanoparticles, the volatile solvent is 60%–84.7%, the fluorinated silane is 0.3%–2.0%, the inorganic oxide nanoparticles are 2%–8%, and the alkaline dispersion is 13%–30%.

7. The preparation method according to claim 4, characterized in that, The metal substrate includes at least one of aluminum and its alloys, magnesium and its alloys, galvanized steel sheet, and zinc-aluminum-magnesium coated steel sheet. And / or, the auxiliary film-forming components include metavanadate and manganese salt, and the zirconium-based conversion solution stock solution comprises, by mass percentage: 0.6%–1.2% zirconium salt; 0.03%–0.15% fluorine-containing accelerator; 0.3%–0.8% metavanadate; 0.2%–4.0% manganese salt; the balance being water; And / or, the zirconium salt includes at least one of sodium hexafluorozirconate, potassium hexafluorozirconate, ammonium hexafluorozirconate, and lithium hexafluorozirconate; And / or, the fluorine-containing accelerator includes at least one of sodium fluoride, potassium fluoride, ammonium fluoride, ammonium hydrogen fluoride, and hydrofluoric acid; And / or, the auxiliary film-forming component includes metavanadate and manganese salt, wherein the metavanadate is at least one of sodium metavanadate, potassium metavanadate, and ammonium metavanadate, and the manganese salt is at least one of manganese nitrate, manganese sulfate, and manganese chloride; And / or, the curing agent includes at least one of amine curing agents, polyamide curing agents, and modified amine curing agents; And / or, the volatile solvent includes at least one of methanol, ethanol, n-propanol, isopropanol, and butanol.

8. The preparation method according to claim 5, characterized in that, The inorganic oxide nanoparticles are selected from at least one of silicon dioxide, aluminum oxide, titanium dioxide, and zirconium oxide; And / or, the fluorinated silane comprises a perfluoroalkyltrialkoxysilane, preferably at least one selected from 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorooctyltriethoxysilane, 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, and 1H,1H,2H,2H-perfluorodecyltriethoxysilane.

9. The preparation method according to claim 4, characterized in that, The preheating temperature is 35–55 °C, and the preheating time is 3–10 min; and / or, the conversion treatment time is 3–10 min; And / or, the dilution factor is 4 to 6 times; And / or, the baking temperature is 70–90 °C, and the baking time is 0.5–1.5 h; And / or, the number of spraying applications is 1 to 3, and the spraying time for each application is 10 to 20 seconds; And / or, the curing temperature is 70–90 °C, and the curing time is 2–4 h; And / or, the pH adjustment range is 3.0 to 4.

5.

10. The preparation method according to claim 5, characterized in that, The programmed heating conditions are as follows: magnetic stirring at 30–50 °C for 16–24 h, followed by heating to 80–100 °C and stirring for another 4–8 h.