A wafer-level glass paste bonding structure and bonding method thereof

By setting annular grooves and overflow grooves on the silicon wafer, the problems of thickness and alignment misalignment in glass paste bonding are solved, and high-precision bonding of MEMS devices is achieved.

CN123105536APending Publication Date: 2026-11-17EAST CHINA INST OF OPTOELECTRONICS INTEGRATEDDEVICE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611098005.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing glass paste bonding processes, the thickness of the glass paste layer after bonding is uncontrollable, and the alignment offset is also uncontrollable, which affects the performance and accuracy of MEMS devices.

Method used

Design a wafer-level glass paste bonding structure, including setting annular grooves and overflow grooves on the silicon wafer to control the paste thickness, and achieving mechanical locking through positioning annular grooves and interlocking ring stages to ensure alignment accuracy.

Benefits of technology

This achieves precise control over the bonding layer thickness and significantly improves alignment accuracy, thereby enhancing the performance stability and precision of MEMS devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105536A_ABST
    Figure CN123105536A_ABST
Patent Text Reader

Abstract

This invention provides a wafer-level glass paste bonding structure, comprising a structural silicon wafer, a bonding silicon wafer, and a capping silicon wafer. The structural silicon wafer has a first annular groove, a second annular groove, a third annular groove, a positioning annular groove, and an overflow groove. The bonding silicon wafer has a movable MEMS structure. The capping silicon wafer has a boss, a second boss, and a insertion ring. A bonding method for this wafer-level glass paste bonding structure includes the fabrication of the first annular groove, second annular groove, third annular groove, positioning annular groove, and overflow groove on the structural silicon wafer; the fabrication of the movable MEMS structure on the bonding silicon wafer; the fabrication of the boss, second boss, and insertion ring on the capping silicon wafer; and the bonding of these three components. This invention has advantages such as simple structure, convenient implementation, precise control of bonding layer thickness, significantly improved bonding alignment accuracy, coordinated control of bonding layer thickness and alignment after bonding, precise control of bonding cavity height, and strong process compatibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of semiconductor manufacturing and microelectromechanical systems (MEMS) packaging technology, specifically to a wafer-level bonding structure and bonding method that can simultaneously and precisely control the thickness of the glass paste layer after bonding and the alignment accuracy after bonding. Background Technology

[0002] Wafer-level bonding technology is one of the core processes in semiconductor 3D integration, MEMS device packaging, optoelectronic device sealing, and microfluidic chip manufacturing. Depending on the bonding intermediate layer, common wafer-level bonding technologies include metal eutectic bonding, anodic bonding, fused bonding, polymer bonding, and glass paste bonding. Among these, glass paste bonding plays a crucial role in practical industrial applications due to its advantages such as lower requirements for wafer surface flatness, moderate process temperature (typically 400℃~500℃), ability to form good sealing structures, and relatively low cost.

[0003] In a typical glass paste bonding process, a glass paste is first applied to the bonding area of ​​a wafer using screen printing or dispensing. After pre-sintering to remove organic solvents, the wafer is aligned and bonded to another wafer in a bonding machine. Under applied temperature and pressure, the glass paste softens, flows, and eventually solidifies to form a glassy bonding layer. This bonding layer serves both as a mechanical connection and as a hermetically or non-hermetic sealed cavity, protecting sensitive internal structures (such as MEMS micromechanical structures and optical components).

[0004] However, existing glass paste bonding processes face two technical challenges: the first is the uncontrollable thickness of the bonded glass paste layer. After heating the glass paste above its softening point, its viscosity decreases significantly, leading to unpredictable flow and spreading under applied bonding pressure. Although limited compensation can be made by adjusting parameters such as the paste thickness during screen printing, bonding pressure, and heating profile, the rheological behavior of the molten glass paste is influenced by various factors, causing the thickness of the bonded paste layer to fluctuate within a range of ±3µm or even larger. This results in the bonding cavity height deviating from the design value, directly affecting key performance indicators of MEMS devices such as sensitivity, damping characteristics, and resonant frequency.

[0005] The second issue is the uncontrollable alignment misalignment during the bonding process. In the molten glass slurry state, the slurry acts as a low-viscosity lubricating medium. Under bonding pressure, the two wafers are prone to relative sliding, leading to a significant deterioration in lateral alignment accuracy after bonding. Even if the bonding equipment has sub-micron alignment accuracy at room temperature, once the temperature is raised to the glass slurry's melting temperature, the combined effects of the lubricating effect of the molten slurry and thermal expansion often result in misalignment of several micrometers or even tens of micrometers after bonding. For devices requiring high-precision alignment (such as waveguide coupling structures in optoelectronic integration and capacitive sensing structures in MEMS inertial sensors), this misalignment will directly lead to device failure.

[0006] To improve thickness control, those skilled in the art have attempted to add spherical spacers or create raised limiting structures in the glass paste. To improve alignment accuracy, existing technologies primarily rely on enhancing the alignment stability of the bonding equipment or adding additional mechanical locking structures; however, these methods are either costly or have poor compatibility with glass paste processes. To date, a glass paste bonding solution that can simultaneously address both uncontrollable thickness and alignment misalignment issues is lacking. Summary of the Invention

[0007] The present invention aims to overcome the shortcomings of the prior art by providing a wafer-level glass paste bonding structure and its bonding method.

[0008] This invention provides the following technical solutions: A wafer-level glass paste bonding structure is characterized in that: it includes a structural silicon wafer, a first annular groove is provided on the bottom surface of the structural silicon wafer, a second annular groove is provided on the bottom of the first annular groove, a third annular groove is provided on the bottom of the second annular groove, a positioning annular groove is provided on the bottom of the second annular groove on both sides of the third annular groove, and a set of overflow grooves are evenly distributed on the bottom of the third annular groove. A bonded silicon wafer is provided on the bottom surface of the structural silicon wafer, and a MEMS movable structure is provided on the bonded silicon wafer; A cap silicon wafer is provided that corresponds to and matches the structural silicon wafer and the bonding silicon wafer. An annular boss is provided on the upper surface of the cap silicon wafer, and the groove inside the annular boss makes way for the movable MEMS structure. An annular second boss is provided on the upper surface of the annular boss, which corresponds to and mates with the third annular groove. On the upper surface of the bosses on both sides of the annular second boss, there are insertion ring platforms that correspond to and mate with the positioning ring grooves. The upper surface of the second boss serves as the bonding surface of the glass slurry corresponding to a set of overflow ring grooves. The height of the second boss is A, the depth of the third annular groove is B, the height of the insertion annular platform is C, and the depth of the positioning annular groove is D. A≤B, C>D.

[0009] Based on the above technical solutions, the following further technical solutions are also possible: The overflow channel is one or more combinations of annular channel, spiral channel, straight channel, grid channel, honeycomb channel, and dot matrix blind hole array; the overflow channel depth ranges from 2μm to 20μm, and the overflow channel width ranges from 5μm to 200μm.

[0010] The cross-sectional shape of the positioning ring groove and the insertion ring platform can be any one of rectangle, trapezoid, triangle, or arc; the depth of the positioning ring groove is in the range of 3μm-10μm, and the width of the positioning groove is in the range of 10μm-50μm. The height of the interposer ring ranges from 4μm to 15μm, and the width of the interposer ring ranges from 6μm to 46μm. The positioning ring groove and the interposer ring are distributed in a concentric ring shape along the wafer bonding area.

[0011] The structured silicon wafer and the cap silicon wafer are double-polished silicon wafers or SOI silicon wafers, with a thickness of 300μm-875μm.

[0012] The movable MEMS structure can be any one of the following: MEMS accelerometer, MEMS gyroscope, MEMS pressure sensor, MEMS optical sensor, MEMS radio frequency device, or MEMS microphone.

[0013] A bonding method for wafer-level glass paste structures includes the following steps: S1. Clean the structured silicon wafer, capped silicon wafer, and bonding silicon wafer respectively; S2. Processing the silicon wafer structure: Bonding alignment marks, cavity structure, overflow groove, and positioning groove are prepared sequentially through photolithography, etching, and resist removal processes; S3. The structural silicon wafer and the bonding silicon wafer are fused together, and then the MEMS movable structure is prepared by mechanical thinning, CMP, photolithography, etching and resist removal processes. S4. Processing capped silicon wafers: Bonding alignment marks, height limit blocks, and glass paste bonding surfaces are prepared sequentially through photolithography, etching, and resist removal processes; S5. Screen print glass paste on the glass paste bonding surface of the capped silicon wafer, and complete the drying and pre-sintering treatment; S6. Perform surface activation treatment on the structured silicon wafer and the capped silicon wafer respectively; S7. Perform optical alignment between the activated structured silicon wafer and the capped silicon wafer; S8. Place the two aligned wafers into the bonding machine chamber, and apply constant temperature and pressure to complete the glass slurry melting and bonding in a vacuum environment or inert gas atmosphere. Then cool the chamber to room temperature.

[0014] Based on the steps described above, the following further steps can be taken: The cleaning solution used in step S1 is prepared by mixing 98% sulfuric acid and 30% hydrogen peroxide in a volume ratio of 4:1; the cleaning temperature is 120℃-130℃ and the cleaning time is 15min-20min; after cleaning, it is rinsed with deionized water for 10min and then dried in a spin dryer.

[0015] The activation process in step S6 involves treating the surface of the structured silicon wafer with VHF or DHF; and the surface of the capped silicon wafer is treated with plasma cleaning.

[0016] The inert gas used in step S8 is nitrogen or argon; the bonding temperature is 435℃-450℃, the bonding pressure is 3000N-8000N, and the holding time is 20min-50min.

[0017] The cavity depth obtained in step S2 ranges from 0.5 μm to 10 μm.

[0018] Advantages of the invention: This invention has the advantages of simple structure, convenient implementation, precise control of bonding layer thickness, significantly improved bonding alignment accuracy, coordinated control of thickness and alignment, precise control of bonding cavity height, and strong process compatibility. Attached Figure Description

[0019] Figure 1 : A schematic cross-sectional view of the silicon wafer structure provided in this invention before fusion bonding; Figure 2 This is a schematic cross-sectional view of the structural silicon wafer and the bonded silicon wafer provided in this invention, after being fused and bonded to form a movable MEMS structure. Figure 3 : A cross-sectional schematic diagram of the glass paste printed on the bonding surface of the cap silicon wafer in this embodiment of the invention; Figure 4 This is a cross-sectional schematic diagram of the silicon wafer and cap silicon wafer of the present invention after glass bonding, showing the solidification of glass slurry, excess slurry overflowing into the overflow groove, and the height limiting structure being embedded in the positioning groove; Figure 5 :yes Figure 4 A magnified view along direction A in the image. Detailed Implementation

[0020] like Figure 1-5 As shown, a wafer-level glass paste bonding structure includes a double-polished silicon wafer or an SOI silicon wafer with a thickness of 675 μm, which can be used as the structural silicon wafer 1. A first annular groove 2 is provided on the bottom surface of the structural silicon wafer 1, and a second annular groove 3 is provided near the outer side of the bottom of the first annular groove 2.

[0021] A third annular groove 4 is provided on the bottom of the second annular groove 3. A positioning annular groove 5 is provided on the bottom of the second annular groove 3 on both sides of the third annular groove 4. The depth of the positioning annular groove 5 is in the range of 5μm, and the width of the positioning groove is in the range of 30μm. The cross-section of the positioning annular groove 5 is rectangular.

[0022] A set of overflow channels 6 are evenly distributed on the bottom of the third annular channel 4. The overflow channels 6 are all annular channels with a depth of 5μm and a width of 50μm.

[0023] Furthermore, the first annular groove 2, the second annular groove 3, the third annular groove 4, the positioning annular groove 5, and a set of overflow grooves 6 are all distributed in concentric circles, and are all manufactured by photolithography, etching, and resist removal processes.

[0024] A bonded silicon wafer 7 is fused and bonded to the bottom surface of a structural silicon wafer 1. After mechanical thinning, CMP, photolithography, etching, and resist removal, a MEMS movable structure 7a is formed. The MEMS movable structure 7a is used in a MEMS gyroscope. A 575μm thick double-polished silicon wafer with a seat cap 8 is used. An annular protrusion 9 is formed on the upper surface of the cap wafer 8 through oxidation, photolithography, etching, and resist removal processes. The groove inside the annular protrusion 9 provides clearance for the MEMS movable structure 7a. The cross-section of the annular protrusion 9 is trapezoidal. A second annular protrusion 10 is formed on the upper surface of the annular protrusion 9 through thermal oxidation, photolithography, dielectric etching, silicon etching, resist removal, and oxide layer removal processes. The cross-section of the second annular protrusion 10 is also trapezoidal.

[0025] On the upper surfaces of the protrusions 9 on both sides of the annular second protrusion 10, insertion rings 11 corresponding to and cooperating with the positioning ring grooves 5 are formed by photolithography, silicon etching, and resist removal processes. The cross-sectional shape of the insertion rings 11 is rectangular with a height of 10 μm and a width of 26 μm.

[0026] The upper surface of the second boss 10 serves as the glass slurry bonding surface 11a corresponding to a set of overflow annular grooves 6.

[0027] The height of the second boss 10 is A, the depth of the third annular groove 4 is B, the height of the insertion ring platform 11 is C, and the depth of the positioning annular groove 5 is D, where A≤B and C>D.

[0028] The bonding method for preparing the above-mentioned wafer-level glass paste bonding structure is characterized by comprising the following steps: S1. Clean the structural silicon wafer, cap silicon wafer, and bonding silicon wafer respectively. The cleaning solution used in step S1 is prepared by mixing 98% sulfuric acid and 30% hydrogen peroxide in a volume ratio of 4:1. The cleaning temperature is 120℃ and the cleaning time is 20min. After cleaning, rinse with deionized water for 10min and then dry with a spin dryer.

[0029] S2. Processing the silicon wafer: Bonding alignment marks, the first annular groove with a depth of 10μm, overflow groove, and positioning groove are prepared sequentially through photolithography, etching, and resist removal processes.

[0030] S3. The structural silicon wafer and the bonding silicon wafer are fused together, and then the MEMS movable structure is prepared by mechanical thinning, CMP, photolithography, etching and resist removal processes.

[0031] S4. Processing capped silicon wafers: Bonding alignment marks, height limit blocks, and glass paste bonding surfaces are prepared sequentially through photolithography, etching, and resist removal processes.

[0032] S5. Screen print glass paste 12 on the glass paste bonding surface of the cap silicon wafer, and complete the drying and pre-sintering treatment; S6. Perform surface activation treatment on the structural silicon wafer and the cap silicon wafer respectively. The activation treatment method is to use DHF to treat the surface of the structural silicon wafer and to use plasma cleaning to treat the surface of the cap silicon wafer.

[0033] S7. Perform optical alignment between the activated structured silicon wafer and the capped silicon wafer; S8. Place the two aligned wafers into the bonding machine chamber. Under vacuum or inert gas atmosphere, apply constant temperature and pressure to complete the glass slurry melting and bonding. Then cool the chamber to room temperature. The inert gas is nitrogen or argon; the bonding temperature is 440℃, the bonding pressure is 5000N, and the holding time is 30min.

[0034] The overflow groove design collects and accommodates excess glass paste squeezed out from the bonding interface during the bonding process. The presence of the overflow groove also reduces the effective bearing area on the bonding interface, allowing for predefined and controlled paste thickness in non-overflow groove areas even with fluctuations in the amount of printing paste. When the glass paste melts and is pressurized, excess paste automatically flows into the overflow groove instead of overflowing only towards the wafer edge, thus ensuring uniform paste thickness in the bonding area.

[0035] The positioning ring groove and the insertion ring form a complementary mechanical locking structure. During bonding, the insertion ring is inserted into the positioning ring groove. Due to the mechanical interference between the insertion ring and the groove wall, the relative displacement of the upper and lower wafers in the horizontal direction is strictly limited.

[0036] The first annular groove, second annular groove, third annular groove, positioning annular groove, a set of overflow grooves, boss, second boss and plug-in ring platform are all concentrically distributed multiple sets of mechanical locking structures, which can further improve the ability to resist displacement and disperse stress.

[0037] The design of A≤B and C>D allows the insertion ring stage to directly contact the positioning ring groove on the structured silicon wafer during bonding, forming a hard limit. When bonding pressure is applied, once the insertion ring stage is embedded in the positioning ring groove, the further vertical travel is limited, thereby precisely controlling the thickness of the glass paste layer after bonding.

Claims

1. A wafer level glass paste bonding structure, characterized in that: It includes a structural silicon wafer (1), a first annular groove (2) is provided on the bottom surface of the structural silicon wafer (1), a second annular groove (3) is provided on the bottom of the first annular groove (2), a third annular groove (4) is provided on the bottom of the second annular groove (3), a positioning annular groove (5) is provided on the bottom of the second annular groove (3) on both sides of the third annular groove (4), and a set of overflow grooves (6) are evenly distributed on the bottom of the third annular groove (4). A bonding silicon wafer (7) is provided on the bottom surface of the structural silicon wafer (1), and a MEMS movable structure is provided on the bonding silicon wafer (7); A cap silicon wafer (8) is provided to correspond to and cooperate with the structural silicon wafer (1) and the bonding silicon wafer (7). An annular boss (9) is provided on the upper surface of the cap silicon wafer (8). The groove inside the annular boss (9) makes way for the MEMS movable structure. On the upper surface of the annular boss (9), there is an annular second boss (10) that corresponds to and cooperates with the third annular groove (4). On the upper surface of the bosses (9) on both sides of the annular second boss (10), there are plug-in ring platforms (11) that correspond to and cooperate with the positioning ring groove (5). The upper surface of the second boss (10) serves as the glass slurry bonding surface (11a) corresponding to a set of overflow ring grooves (6). The height of the second boss (10) is A, the depth of the third annular groove (4) is B, the height of the insertion ring (11) is C, and the depth of the positioning annular groove (5) is D. A≤B, C>D.

2. The wafer level glass paste bonding structure of claim 1, wherein: The overflow groove (6) is one or more of the following: annular groove, spiral groove, straight groove, grid groove, honeycomb groove, and dot matrix blind hole array; the overflow groove depth ranges from 2μm to 20μm, and the overflow groove width ranges from 5μm to 200μm.

3. The wafer level glass paste bonding structure as claimed in claim 1, wherein: The cross-sectional shape of the positioning ring groove (5) and the insertion ring platform (11) is any one of rectangle, trapezoid, triangle and arc; the depth of the positioning ring groove (5) is in the range of 3μm-10μm, and the width of the positioning groove is in the range of 10μm-50μm; The height of the insertion ring (11) ranges from 4μm to 15μm, and the width of the insertion ring (11) ranges from 6μm to 46μm. The positioning ring groove (5) and the insertion ring (11) are distributed in a concentric ring shape along the wafer bonding area.

4. The wafer level glass paste bonding structure of claim 1, wherein: The structured silicon wafer (1) and the cap silicon wafer (8) are double-polished silicon wafers or SOI silicon wafers, with a thickness of 300μm-875μm.

5. The wafer level glass paste bonding structure as claimed in claim 1, wherein: The aforementioned movable MEMS structure can be applied to any type of device among MEMS accelerometers, MEMS gyroscopes, MEMS pressure sensors, MEMS optical sensors, MEMS RF devices, and MEMS microphones.

6. A bonding method for preparing a wafer level glass paste bonded structure according to any one of claims 1 to 8, characterized by: Includes the following steps: S1. Clean the structured silicon wafer, capped silicon wafer, and bonding silicon wafer respectively; S2. Processing the silicon wafer structure: Bonding alignment marks, first ring groove, overflow groove, and positioning ring groove are prepared sequentially through photolithography, etching, and resist removal processes; S3. The structural silicon wafer and the bonding silicon wafer are fused together, and then the MEMS movable structure is prepared by mechanical thinning, CMP, photolithography, etching and resist removal processes. S4. Processing capped silicon wafers: Bonding alignment marks, height limit blocks, and glass paste bonding surfaces are prepared sequentially through photolithography, etching, and resist removal processes; S5. Screen print glass paste on the glass paste bonding surface of the capped silicon wafer, and complete the drying and pre-sintering treatment; S6. Perform surface activation treatment on the structured silicon wafer and the capped silicon wafer respectively; S7. Perform optical alignment between the activated structured silicon wafer and the capped silicon wafer; S8. Place the two aligned wafers into the bonding machine chamber, and apply constant temperature and pressure to complete the glass slurry melting and bonding in a vacuum environment or inert gas atmosphere. Then cool the chamber to room temperature.

7. The method of claim 6, wherein the method further comprises: The cleaning solution used in step S1 is prepared by mixing 98% sulfuric acid and 30% hydrogen peroxide in a volume ratio of 4:1; the cleaning temperature is 120℃-130℃ and the cleaning time is 15min-20min; after cleaning, it is rinsed with deionized water for 10min and then dried in a spin dryer.

8. The method of claim 6, wherein the method further comprises: The activation process in step S6 involves treating the surface of the structured silicon wafer with VHF or DHF; and the surface of the capped silicon wafer is treated with plasma cleaning.

9. The method of claim 6, wherein the method further comprises: The inert gas used in step S8 is nitrogen or argon; the bonding temperature is 435℃-450℃, the bonding pressure is 3000N-8000N, and the holding time is 20min-50min.

10. The method of claim 7, wherein the method further comprises: The cavity depth obtained in step S2 ranges from 0.5 μm to 10 μm.