A method for preparing Ca-LSX molecular sieves and its application in nitrogen and oxygen separation.

By using a methanol-water mixed solution for modification in the preparation of LiCa-LSX molecular sieves, the process flow is simplified, and the directional and controllable placement of lithium ions is achieved. This solves the problems of cumbersome processes and random lithium ion placement in traditional methods, improves nitrogen and oxygen separation performance and the integrity of the framework structure, and reduces costs.

CN123105672APending Publication Date: 2026-11-17WUHAN UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611313145.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing LiCa-LSX molecular sieve preparation process is cumbersome, the lithium ion placement is random, the nitrogen and oxygen separation capacity is limited, and high-temperature calcination may damage the framework structure.

Method used

LiCa-LSX molecular sieves were prepared by modifying the Li+ ions with a methanol-water mixed solution, followed by centrifugation, washing, and drying. This process avoids high-temperature calcination and utilizes the large solvation radius of Li+ ions to preferentially occupy highly active sites, simplifying the process and enabling the directional and controllable placement of lithium ions.

Benefits of technology

It achieves high-efficiency nitrogen and oxygen separation performance with a separation coefficient of 6.69, low lithium consumption, complete framework structure, energy saving, consumption reduction and emission reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105672A_ABST
    Figure CN123105672A_ABST
Patent Text Reader

Abstract

A method for preparing Ca-LSX molecular sieves and their application in nitrogen and oxygen separation includes the following steps: preparing a methanol or methanol-water mixed solution containing lithium ions; adding Ca-LSX molecular sieve powder to the methanol or methanol-water mixed solution and stirring thoroughly to obtain an intermediate mixture; centrifuging, washing, and drying the intermediate mixture to obtain LiCa-LSX molecular sieves. This application provides a method for preparing a mixed cation LiCa-LSX molecular sieve with high-efficiency nitrogen and oxygen separation performance, solving the problems of cumbersome processes, random lithium ion placement, and limited nitrogen and oxygen separation capacity in traditional cation exchange methods. It simplifies the process flow and achieves directional and controllable placement of a small amount of lithium ions and high-efficiency nitrogen and oxygen separation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to a method for preparing Ca-LSX molecular sieves and their application in nitrogen and oxygen separation. Background Technology

[0002] X-type molecular sieves have an octahedral zeolite (FAU) structure, and their silica-to-alumina ratio (SiO2 / Al2O3 = 2.0–3.0) directly affects their ion exchange performance. A lower silica-to-alumina ratio results in more framework negative charges and more non-framework cations, leading to a richer pool of adsorption and ion exchange active sites. Therefore, low silica-to-alumina ratio X-type molecular sieves (LSX, SiO2 / Al2O3 = 2.0–2.2) are widely used in nitrogen and oxygen adsorption separation. In 1992, research found that Li-LSX molecular sieves had a 50% higher nitrogen adsorption capacity than Na-LSX. Since then, Li-LSX, due to its large nitrogen adsorption capacity and high nitrogen and oxygen separation coefficient, has become the ideal core adsorbent material for pressure swing adsorption (PSA) oxygen generation technology. The key technology for preparing Li-LSX molecular sieves is to... + It is exchanged into Na / K-LSX molecular sieves. Studies have shown that when Li... + When the exchange degree is below 70%, the adsorption capacity of the molecular sieve for N2 hardly changes; only when Li... + The adsorption capacity of the molecular sieve for N2 only increases linearly when the exchange degree increases from 70% to 100%. The preparation of Li-LSX molecular sieves for Li... + High demand and the rapid development of the lithium battery industry in recent years have led to a continuous rise in lithium salt prices, making the cost of full lithium exchange molecular sieves too high.

[0003] The air separation performance of molecular sieves as adsorbents is based on the interaction between the electric field gradient of the molecular sieve cations and the quadrupole moment of N2, and this interaction is closely related to the distribution of cation sites in the molecular sieve. The cation sites of low silica-to-alumina ratio X-type molecular sieves are as follows... Figure 1 As shown. For Li-LSX molecular sieves, only the SIII site can bind to N2 (O2), because of the oxygen surrounding the framework and the small-sized Li. + The electron shielding effect makes Li at the SI' and SII positions + It cannot be effectively utilized. Therefore, only about 30% of the lithium in Li-LSX molecular sieves has an adsorption and separation effect, resulting in low lithium-ion utilization. LiCa-LSX molecular sieves use inexpensive Ca... 2+ Li replaced the non-adsorption active site in Li-LSX + This reduces the amount of lithium used while maintaining high nitrogen and oxygen separation activity.

[0004] The ease of cation exchange in molecular sieve materials is mainly determined by both charge intensity and ionic radius. Some studies first mix calcined and activated Na-LSX molecular sieves with lithium salt solutions for cation exchange to obtain (Li,Na)-LSX type zeolites. Then, these zeolites are placed in calcium salt solutions for multiple cation exchanges, followed by drying and calcination to obtain (Li,Ca)-LSX type zeolite molecular sieves. This method involves multiple ion exchange, washing, drying, and calcination steps, and cannot guarantee the quality of Li... + All the adsorption sites are located at active adsorption sites, resulting in a low nitrogen adsorption capacity. Some studies have also proposed first removing the Na from the Na-LSX molecular sieve. + All exchanged to Ca 2+ Then, a small amount of lithium ions are used to exchange Ca. 2+ This method can effectively control costs, but the nitrogen-oxygen separation coefficient of the LiCa-LSX molecular sieve obtained so far is still not high.

[0005] Ion exchange in molecular sieves is typically carried out in aqueous solution; therefore, molecular sieves generally require pre-heating and dehydration before use, usually at 400 °C for at least 4 hours. In this process, cations migrate or diffuse to their equilibrium sites. For molecular sieves with mixed cations, studies have found that lighter cations tend to migrate to lower sites (SI, SI', SII). For example, in the mixed-cation CeNaCa-X molecular sieve, Na and Ca are at lower sites, while Ce(III) cations are at some external sites. In the mixed-cation NaSr-X zeolite, Na… + The ion is at the Si site, while the Sr ion is at the Si site. 2+ At the SII site. This cation distribution characteristic also exists in the LiNa-LSX molecular sieve framework. As mentioned earlier, the existing LiCa-LSX preparation process is relatively cumbersome, lithium ions are prone to migration under high-temperature calcination, and the structural integrity of the LSX molecular sieve framework is also somewhat damaged. Therefore, there is an urgent need to develop a LiCa-LSX molecular sieve preparation method that can achieve directional lithium ion placement and ensure efficient nitrogen and oxygen separation. Summary of the Invention

[0006] To address the aforementioned problems, this application proposes a method for preparing Ca-LSX molecular sieves, comprising the following steps; Prepare a methanol or methanol-water mixture containing lithium ions; The Ca-LSX molecular sieve raw powder is added to methanol or methanol-water mixture and stirred thoroughly to obtain an intermediate mixture. The intermediate mixture is centrifuged, washed, and dried to obtain LiCa-LSX molecular sieve. This application provides a method for preparing mixed cation LiCa-LSX molecular sieve with high-efficiency nitrogen-oxygen separation performance, which solves the problems of cumbersome process, random lithium ion placement, and limited nitrogen-oxygen separation capacity of traditional cation exchange methods, simplifies the process flow, and achieves effective and controllable placement of a small amount of lithium ions and high-efficiency nitrogen-oxygen separation.

[0007] Preferably, the water content in the methanol-water mixture is 5-20 wt%.

[0008] Preferably, the molar concentration of lithium ions is 0.05-0.1 mol / L.

[0009] Preferably, the lithium ions are derived from anhydrous LiCl.

[0010] Preferably, during the modification treatment, the mass ratio of Ca-LSX molecular sieve raw powder to methanol or methanol-water mixed solution is 0.8-1.2:20.

[0011] Preferably, the modification treatment temperature is 45-55℃ and the treatment time is 5-7 h.

[0012] Preferably, the centrifugal washing is performed in the following manner: Wash with deionized water during centrifugation at 7000-9000 rpm for 2-4 minutes.

[0013] Preferably, the drying temperature is 55-65℃ and the time is 20-28 h.

[0014] Preferably, the intermediate mixture is not calcined after drying. This application utilizes a methanol-water mixture to significantly solvate Li... + Radius and higher desolvation energy are favorable for Li + Prioritizing the occupation of highly active SIII sites and eliminating the need for high-temperature calcination during modification, LiCa-LSX molecular sieves offer several advantages over traditionally prepared LiCa-LSX molecular sieves: no calcination is required throughout the process, resulting in energy conservation, emission reduction, and lower consumption; the prepared LiCa-LSX molecular sieve framework is more complete than that prepared using traditional methods; it exhibits superior nitrogen and oxygen separation performance, with a separation coefficient reaching 6.69; and it requires less lithium. + Higher utilization rate.

[0015] On the other hand, this application also discloses the application of LiCa-LSX molecular sieves in nitrogen and oxygen separation.

[0016] This application can bring the following beneficial effects: 1. This application provides a method for preparing a mixed cation LiCa-LSX molecular sieve with high-efficiency nitrogen-oxygen separation performance, in order to solve the problems of cumbersome process, random lithium ion placement and limited nitrogen-oxygen separation capacity of traditional cation exchange methods, simplify the process flow, and realize the directional and controllable placement of a small amount of lithium ions and high-efficiency nitrogen-oxygen separation.

[0017] 2. This application utilizes a methanol-water mixture to significantly solubilize Li + Radius and higher desolvation energy are favorable for Li + Prioritizing the occupation of highly active SIII sites and eliminating the need for high-temperature calcination during modification, LiCa-LSX molecular sieves offer several advantages over traditionally prepared LiCa-LSX molecular sieves: no calcination is required throughout the process, resulting in energy conservation, emission reduction, and lower consumption; the prepared LiCa-LSX molecular sieve framework is more complete than that prepared using traditional methods; it exhibits superior nitrogen and oxygen separation performance, with a separation coefficient reaching 6.69; and it requires less lithium. + Higher utilization rate. Attached Figure Description

[0018] The accompanying drawings, which are included to provide a further understanding of this application and form part of this application, illustrate exemplary embodiments and are used to explain this application, but do not constitute an undue limitation of this application. In the drawings: Figure 1 This is a diagram showing the distribution of cation sites in Li-LSX type molecular sieves.

[0019] Figure 2 The bar chart shows the nitrogen and oxygen adsorption capacity of the examples and comparative examples (25°C, 101.3 kPa). Detailed Implementation

[0020] To clearly illustrate the technical features of this solution, the following detailed description, in conjunction with the accompanying drawings, will be provided.

[0021] like Figure 1-2 As shown, a method for preparing Ca-LSX molecular sieves includes the following steps: preparing a methanol or methanol-water mixed solution containing lithium ions; The Ca-LSX molecular sieve raw powder is added to methanol or methanol-water mixture and stirred thoroughly to obtain an intermediate mixture. The intermediate mixture was centrifuged, washed, and dried to obtain LiCa-LSX molecular sieve.

[0022] The water content in the methanol-water mixture is 5-20 wt%.

[0023] The molar concentration of lithium ions is 0.05-0.1 mol / L.

[0024] The lithium ions are derived from anhydrous LiCl.

[0025] During the modification process, the mass ratio of Ca-LSX molecular sieve raw powder to methanol or methanol-water mixed solution is 0.8-1.2:20.

[0026] The modification treatment temperature is 45-55℃, and the treatment time is 5-7 h.

[0027] The centrifugal washing is performed in the following manner: Wash with deionized water during centrifugation at 7000-9000 rpm for 2-4 minutes.

[0028] The drying temperature is 55-65℃, and the time is 20-28 h.

[0029] The intermediate mixture is not roasted after drying.

[0030] Application of LiCa-LSX molecular sieves prepared by the above method in nitrogen and oxygen separation.

[0031] The following is a specific example: Example 1 S101. Prepare a methanol solution containing lithium ions; The molar concentration of lithium ions in the LiCl aqueous solution is 0.05 mol / L; the source of lithium ions is anhydrous LiCl.

[0032] S102. Add Ca-LSX type molecular sieve raw powder to methanol or methanol-water mixture and stir thoroughly to obtain intermediate mixture; The modification treatment was carried out at a temperature of 45℃ for 7 hours.

[0033] During the modification process, the mass ratio of Ca-LSX molecular sieve raw powder to methanol or methanol-water mixed solution is 0.8:20.

[0034] S103. The intermediate mixture is centrifuged, washed, and dried to obtain LiCa-LSX molecular sieve.

[0035] The centrifugal washing is performed in the following manner: The sample was washed with deionized water during centrifugation at a speed of 7000 rpm for 4 minutes.

[0036] The drying temperature was 55°C and the time was 28 hours.

[0037] Example 2 The specific implementation method of this embodiment is the same as that of Embodiment 1, except that the exchange solvent is LiCl. A methanol-water mixture with a water content of 5%.

[0038] Example 3 The specific implementation method of this embodiment is the same as that of Embodiment 1, except that the exchange solvent is LiCl. A methanol-water mixture with a water content of 10%.

[0039] Example 4 The specific implementation method of this embodiment is the same as that of Embodiment 1, except that the exchange solvent is LiCl. A methanol-water mixture with a water content of 20%.

[0040] Example 5 S501. Prepare a methanol solution containing lithium ions; The molar concentration of lithium ions in the LiCl aqueous solution is 0.1 mol / L; the source of lithium ions is anhydrous LiCl.

[0041] S502. Add Ca-LSX type molecular sieve raw powder to methanol or methanol-water mixture and stir thoroughly to obtain intermediate mixture; The modification treatment was carried out at a temperature of 55℃ for 5 hours.

[0042] During the modification process, the mass ratio of Ca-LSX molecular sieve raw powder to methanol or methanol-water mixed solution is 1.2:20.

[0043] S503. The intermediate mixture is centrifuged, washed, and dried to obtain LiCa-LSX molecular sieve.

[0044] The centrifugal washing is performed in the following manner: The sample was washed with deionized water during centrifugation at a speed of 9000 rpm for 2 minutes.

[0045] The drying temperature was 65°C and the time was 20 hours.

[0046] Comparative Example 1: The specific implementation method of this comparative example is the same as that of Example 1, except that the exchange solvent is an aqueous LiCl solution.

[0047] Comparative Example 2 The specific implementation method of this comparative example is the same as that of comparative example 1, except that the exchange temperature is 40 ℃.

[0048] Comparative Example 3 The specific implementation method of this comparative example is the same as that of comparative example 1, except that the exchange temperature is 60 ℃.

[0049] Comparative Example 4 The specific implementation method of this comparative example is the same as that of Example 1, except that a traditional liquid-phase ion exchange method is used. The exchange method specifically includes the following steps: 1 g of Ca-LSX molecular sieve powder was added to 20 mL of 2.5 mol / L LiCl aqueous solution, and stirred continuously at 25 °C for 6 h with a magnetic stir bar. The mixture was washed by centrifugation with deionized water and dried at 60 °C for 24 hours to obtain LiCa-LSX molecular sieve prepared by the traditional liquid-phase ion exchange method.

[0050] Comparative Example 5 The specific implementation method of this comparative example is the same as that of comparative example 4, except that the Ca-LSX type molecule is used. The raw powder was activated by calcining at 150 ℃ for 2 h and then at 400 ℃ for 2 h before modification began.

[0051] Comparative Example 6 The specific implementation method of this comparative example is the same as that of comparative example 4, except that the dried product is used in this example. The LiCa-LSX molecular sieve was calcined at 150 °C for 2 h and at 400 °C for 2 h.

Claims

1. A method for preparing Ca-LSX molecular sieves, characterized in that: Includes the following steps; Prepare a methanol or methanol-water mixture containing lithium ions; The Ca-LSX molecular sieve raw powder was added to methanol or methanol-water mixture and stirred thoroughly to obtain an intermediate mixture. The intermediate mixture was centrifuged, washed, and dried to obtain LiCa-LSX molecular sieve.

2. The method for preparing a Ca-LSX molecular sieve as described in claim 1, characterized in that: The water content in the methanol-water mixture is 5-20 wt%.

3. The method for preparing a Ca-LSX molecular sieve as described in claim 1, characterized in that: The molar concentration of lithium ions is 0.05-0.1 mol / L.

4. The method for preparing a Ca-LSX molecular sieve as described in claim 3, characterized in that: The lithium ions are derived from anhydrous LiCl.

5. The method for preparing a Ca-LSX molecular sieve as described in claim 1, characterized in that: During the modification process, the mass ratio of Ca-LSX molecular sieve raw powder to methanol or methanol-water mixed solution is 0.8-1.2:

20.

6. The method for preparing a Ca-LSX molecular sieve as described in claim 5, characterized in that: The modification treatment temperature is 45-55℃, and the treatment time is 5-7 h.

7. The method for preparing a Ca-LSX molecular sieve as described in claim 1, characterized in that: The centrifugal washing is performed in the following manner: Wash with deionized water during centrifugation at 7000-9000 rpm for 2-4 minutes.

8. The method for preparing a Ca-LSX molecular sieve as described in claim 1, characterized in that: The drying temperature is 55-65℃, and the time is 20-28 h.

9. The method for preparing a Ca-LSX molecular sieve as described in claim 1, characterized in that: The intermediate mixture is not roasted after drying.

10. The application of the LiCa-LSX molecular sieve prepared according to any one of claims 1-9 in nitrogen and oxygen separation.