A method for enriching titanium dioxide from waste wind turbine blades

By employing a combined approach of gradient pyrolysis, oxidation, sieving, and acid-calcination, the problem of titanium dioxide recovery and separation in wind turbine blades has been solved, achieving efficient and environmentally friendly titanium dioxide enrichment suitable for various application scenarios.

CN123105709APending Publication Date: 2026-11-17CHINA ENERGY LONGYUAN ENVIRONMENTAL PROTECTION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611380821.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies are insufficient for effectively recovering and separating titanium dioxide from wind turbine blades, leading to resource waste and environmental pollution. Furthermore, existing pyrolysis technologies fail to completely remove residual carbon, affecting the efficiency of titanium dioxide separation and recovery.

Method used

A combined approach of gradient pyrolysis, oxidation, sieving, and acid-calcination is employed. Gradient pyrolysis separates resin and titanium dioxide, oxidation breaks down the carbon residue layer, sieving separates fibers and powder, acid treatment removes impurities, and calcination improves purity, thereby achieving efficient enrichment of titanium dioxide.

Benefits of technology

It achieves efficient separation and enrichment of titanium dioxide, obtaining high-purity and high-yield titanium dioxide products, reducing energy consumption and chemical reagent usage, reducing environmental pollution, and is suitable for various application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to a method for enriching titanium dioxide from waste wind turbine blades. The method includes the following steps: performing gradient pyrolysis on the waste wind turbine blades to obtain solid pyrolysis products; oxidizing the solid pyrolysis products to obtain oxidized solids; sieving the oxidized solids to obtain titanium dioxide-containing powder; and subjecting the titanium dioxide-containing powder to acid treatment and calcination to obtain a titanium dioxide-enriched product. This invention provides a method for enriching titanium dioxide from waste wind turbine blades, enabling efficient separation and enrichment of trace amounts of titanium dioxide, and yielding titanium dioxide products with relatively high purity and high yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the treatment of waste wind turbine blades, and more particularly to a method for enriching titanium dioxide from waste wind turbine blades. Background Technology

[0002] Wind turbine blades are primarily made of glass fiber reinforced epoxy resin composite materials, with a certain amount of titanium dioxide (TiO2) added as a UV shielding agent and white pigment. The titanium dioxide is uniformly dispersed in the resin matrix as nano / micron-sized particles. As the wind power industry enters its peak retirement period, a large number of retired blades, if not properly disposed of, will result in resource waste and environmental pollution. Furthermore, existing recycling processes do not consider the recovery of valuable metal components such as titanium dioxide.

[0003] Pyrolysis has become one of the mainstream technologies for wind turbine blade recycling due to its simple process and lack of the need for large amounts of chemical reagents. Its core is to utilize the difference in thermal stability between resin, glass fiber, and TiO2, and to achieve three-phase separation of solid, liquid, and gas by thermally decomposing and volatilizing the resin at high temperature.

[0004] The core implementation method of existing wind turbine blade pyrolysis recovery technology is as follows: the broken wind turbine blades are placed in a pyrolysis furnace and heated to 400-800℃, causing the epoxy resin to undergo thermal decomposition, generating pyrolysis gas, pyrolysis oil, and solid residue (glass fiber + a small amount of TiO2 + residual carbon). Subsequently, the solid residue is subjected to simple mechanical crushing or air classification to recover the glass fiber. However, TiO2, because it is tightly bound to residual carbon and glass fiber and is considered an impurity, is not targeted for purification and recovery. Although some technologies attempt to remove residual carbon, they only use simple mechanical grinding or high-temperature calcination methods, resulting in incomplete removal of residual carbon and the inability to separate TiO2. Summary of the Invention

[0005] To overcome at least one of the defects of the prior art, one embodiment of the present invention provides a method for enriching titanium dioxide from waste wind turbine blades, comprising the following steps: Waste wind turbine blades are subjected to gradient pyrolysis to obtain solid pyrolysis products; The solid pyrolysis product is oxidized to obtain an oxidized solid. The oxidized solid was sieved and separated to obtain a powder containing titanium dioxide; The titanium dioxide-containing powder is subjected to acid treatment-calcination to obtain the titanium dioxide product. The acid treatment-calcination process includes step a: treating the titanium dioxide-containing powder with an acid solution, followed by solid-liquid separation to obtain an acid-treated solid; then, subjecting the acid-treated solid to gradient calcination; or, The acid treatment-calcination treatment includes step b: calcining the titanium dioxide-containing powder at 400-500°C to obtain a calcined product; then, treating the calcined product with an acid solution. The gradient pyrolysis includes sequentially subjecting the waste wind turbine blades to a first heat preservation treatment at 250–350°C and a second heat preservation treatment at 500–650°C; the gradient calcination in step a includes sequentially subjecting the acid-treated solid to a third heat preservation treatment at 200–300°C and a fourth heat preservation treatment at 500–650°C.

[0006] The present invention discloses a method for enriching titanium dioxide from waste wind turbine blades, which can achieve efficient separation and enrichment of trace amounts of titanium dioxide and obtain titanium dioxide products with relatively high purity and high yield. Detailed Implementation

[0007] Typical embodiments embodying the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various variations in different embodiments without departing from the scope of the present invention, and the description herein is for illustrative purposes only and not intended to limit the present invention.

[0008] One embodiment of the present invention provides a method for enriching titanium dioxide from spent wind turbine blades (or decommissioned wind turbine blades), comprising the following steps: Waste wind turbine blades are subjected to gradient pyrolysis to obtain solid pyrolysis products; The solid pyrolysis products are oxidized to obtain the oxidized solid. The oxidized solid was sieved and separated to obtain powder containing titanium dioxide; Titanium dioxide-containing powder is subjected to acid treatment and calcination to obtain titanium dioxide products; The acid treatment-calcination process includes the following steps: a) treating the titanium dioxide-containing powder with an acid solution, followed by solid-liquid separation to obtain the acid-treated solid; then, subjecting the acid-treated solid to gradient calcination; or, The acid treatment-calcination process includes the following step b: calcining the titanium dioxide-containing powder at 400-500°C to obtain the calcined product; then, treating the calcined product with an acid solution. The gradient pyrolysis process includes sequentially subjecting the waste wind turbine blades to a first heat preservation treatment at 250–350°C and a second heat preservation treatment at 500–650°C; the gradient calcination process in step a includes sequentially subjecting the acid-treated solid to a third heat preservation treatment at 200–300°C and a fourth heat preservation treatment at 500–650°C.

[0009] In one embodiment, the discarded wind turbine blade comprises a resin matrix, which may be a thermosetting resin, such as one or more of epoxy resin and unsaturated polyester resin. Further, the discarded wind turbine blade comprises titanium dioxide.

[0010] In one embodiment, the mass content of titanium dioxide in the waste wind turbine blade is 0.025% or more, preferably 0.05% to 0.4%.

[0011] In one embodiment, the waste wind turbine blades are pretreated before gradient pyrolysis. Further, the pretreatment includes crushing the waste wind turbine blades into blocks (e.g., 10-20 cm) of size (e.g., length) not less than 1 cm, or into powder, or other shapes as needed. Further, a jaw crusher can be used to crush the waste wind turbine blades.

[0012] In one embodiment, during the pretreatment of waste wind turbine blades, the metal inserts, sheaths, and other external components on the surface of the waste wind turbine blades are first removed, and then the blades are crushed.

[0013] In one embodiment, the gradient pyrolysis of waste wind turbine blades can be carried out in a pyrolysis furnace (e.g., a rotary pyrolysis furnace).

[0014] In one embodiment, gradient pyrolysis (segmented heating) of waste wind turbine blades can achieve complete pyrolysis of the resin while avoiding oxidation or agglomeration of titanium dioxide.

[0015] In one embodiment, waste wind turbine blades are subjected to gradient pyrolysis under the action of a protective gas.

[0016] In one embodiment, the oxygen volume content in the protective gas is less than 1 vol%, further less than 0.5 vol%, even further less than 0.1 vol%, and still further less than 0.01 vol%. A higher oxygen content in the protective gas (e.g., above 1 vol%) can lead to titanium loss. This is because titanium is mainly found in the coating and resin of the blades, and the particles are small. If there is sufficient oxygen, the organic matter in the blades is easily combusted or vaporized, resulting in a more vigorous reaction. Titanium is easily carried away, causing titanium loss and a reduced yield.

[0017] In one embodiment, the protective gas includes one or more of nitrogen and inert gases, and further, the inert gas includes argon and / or helium.

[0018] In one embodiment, during gradient pyrolysis, the temperature of the first heat preservation treatment can be 250–350°C, more specifically 250–300°C, for example 252°C, 255°C, 260°C, 270°C, 280°C, 290°C, 298°C, 300°C, 302°C, 305°C, 310°C, 320°C, 330°C, or 340°C; the duration of the first heat preservation treatment can be 1–2 hours, for example 1.5 hours. This first heat preservation treatment allows the resin in the blades to undergo initial softening, and small volatile molecules to escape.

[0019] In one embodiment, the system (e.g., from room temperature) is heated to 250–350°C at a heating rate of 5–10°C / min (e.g., 5°C / min, 6°C / min, 7°C / min, 8°C / min or 9°C / min) for a first heat preservation treatment.

[0020] In one embodiment, during gradient pyrolysis, the temperature of the second heat treatment can be 500–650°C, for example, 502°C, 505°C, 510°C, 520°C, 530°C, 550°C, 560°C, 580°C, 600°C, 620°C, 640°C, 645°C, or 648°C; the duration of the second heat treatment can be 2–3 hours, for example, 2.5 hours.

[0021] In one embodiment, the resin (e.g., epoxy resin) main chain undergoes chain breakage due to the second heat preservation treatment, generating pyrolysis gas and pyrolysis oil, which can be recovered by condensation and used as chemical fuel or raw material. Furthermore, the loss of titanium dioxide is relatively low during the second heat preservation treatment.

[0022] In one embodiment, the system is heated from 250–350°C to 500–650°C at a heating rate of 5–10°C / min (e.g., 5°C / min, 6°C / min, 7°C / min, 8°C / min, or 9°C / min) for a second heat preservation treatment.

[0023] In one embodiment, the products of gradient pyrolysis include pyrolysis gas, pyrolysis oil, and solid pyrolysis products. The solid residue (i.e., solid pyrolysis products) in the pyrolysis furnace includes glass fiber (of a certain length), titanium dioxide, and residual carbon, wherein the titanium dioxide is mainly present on the surface of the glass fiber and partially encapsulated in the residual carbon layer.

[0024] In one embodiment, oxidation treatment can break the carbon-carbon bonds in the residual carbon in the solid pyrolysis products, making the dense residual carbon layer loose and brittle, thereby allowing titanium dioxide to detach from the residual carbon. In addition, oxidation treatment can also remove some impurities.

[0025] In one embodiment, the oxidation treatment of the solid pyrolysis products can be carried out in an oxidation reactor.

[0026] In one embodiment, the solid pyrolysis products are oxidized by plasma (plasma oxidation), ozone (ozone oxidation), or an oxidant solution.

[0027] In one embodiment, solid pyrolysis products can be oxidized using low-temperature plasma.

[0028] In one embodiment, the solid pyrolysis products can be oxidized by ozone at 20–30°C (e.g., 22°C, 24°C, 25°C, 26°C, or 28°C).

[0029] In one embodiment, the solid pyrolysis product is oxidized by an oxidant solution, wherein the oxidant in the oxidant solution includes hydrogen peroxide and / or sodium hypochlorite.

[0030] In one embodiment, during the oxidation process, the liquid-to-solid ratio (the ratio of liquid volume to solid mass) of the oxidant solution to the solid pyrolysis product is 3:1 to 5:1 (ml / g), for example, 4:1 ml / g.

[0031] In one embodiment, the oxidant solution is a hydrogen peroxide solution, and the mass concentration of the hydrogen peroxide solution can be 5-15%, for example 6%, 8%, 10%, 12% or 14%.

[0032] In one embodiment, the oxidant solution is a sodium hypochlorite solution, and the mass concentration of the sodium hypochlorite solution can be 10-20%, for example 12%, 14%, 15%, 16% or 18%.

[0033] In one embodiment, the solid pyrolysis product is oxidized by an oxidant solution. The oxidation temperature can be 50-70°C, or more specifically 60-70°C, for example 52°C, 54°C, 55°C, 56°C, 58°C, 60°C, 62°C, 64°C, 65°C, or 68°C.

[0034] In one embodiment, the oxidation treatment time can be 30 to 60 minutes, more specifically 30 to 40 minutes, for example 32 minutes, 35 minutes, 38 minutes, 40 minutes, 42 minutes, 45 minutes, 48 ​​minutes, 50 minutes, 52 minutes, 55 minutes, or 58 minutes.

[0035] In one embodiment, the oxidized solid-liquid mixture system is subjected to solid-liquid separation to obtain the oxidized solid.

[0036] In one embodiment, the oxidized solid is sieved to separate the fibers from the powder, yielding a titanium dioxide-containing powder. Further, the sieve can be made through a 100-200 mesh screen (e.g., 120, 140, 150, or 180 mesh).

[0037] In one embodiment, the titanium dioxide-containing powder is washed with water, dried, and then subjected to acid treatment-calcination. Further, the titanium dioxide-containing powder can be rinsed with water (e.g., deionized water).

[0038] In one embodiment, the titanium dioxide-containing powder can be washed until neutral to remove residual oxidant; the drying temperature can be 80–100°C, for example 85°C, 90°C, or 95°C.

[0039] In one embodiment, acid treatment allows trace amounts of inorganic impurities in a solid (powder containing titanium dioxide or calcined product) to react with the acid to form soluble salts, thereby removing the inorganic impurities from the solid. Further, the aforementioned inorganic impurities can be metal oxides, such as Fe₂O₃ and / or Al₂O₃.

[0040] In one embodiment, the acid solution in step a or step b includes one or more of hydrochloric acid, sulfuric acid, hydrochloric acid and hydrofluoric acid, and oxalic acid. Further, the acid solution may be a hydrochloric acid solution, a sulfuric acid solution, an oxalic acid solution, or a mixed solution of hydrochloric acid and hydrofluoric acid.

[0041] In one embodiment, the mass concentration of the acid solution in step a or step b can be 5 to 10%, for example 6%, 7%, 8% or 9%.

[0042] In one embodiment, in step a, the temperature at which the titanium dioxide-containing powder is treated with an acid solution can be 60–80°C, more specifically 60–70°C, for example 62°C, 65°C, 68°C, 70°C, 72°C, 75°C, or 78°C; the treatment time can be 40–80 min, more specifically 60–80 min, for example 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, or 75 min.

[0043] In one embodiment, the titanium dioxide-containing powder contains metal oxides, silicon impurities, etc., and the acid solution is a mixture of hydrochloric acid and hydrofluoric acid. Further, the temperature at which the titanium dioxide-containing powder is treated with the mixture of hydrochloric acid and hydrofluoric acid can be 20–30°C, for example, 22°C, 24°C, 25°C, 26°C, or 28°C.

[0044] In one embodiment, in step a, the solid-liquid mixture obtained after acid treatment can be centrifuged. Further, the separated solid (powder) can be washed (e.g., rinsed) with water until neutral to remove soluble salts, yielding the acid-treated solid.

[0045] In one embodiment, in step a, gradient calcination can remove residual organic matter and moisture from the acid-treated solid and repair the damaged titanium dioxide crystal structure during the treatment process.

[0046] In one embodiment, the gradient calcination of the acid-treated solid or the calcination of the titanium dioxide-containing powder can be carried out in a box-type calcination furnace.

[0047] In one embodiment, the gradient calcination or calcination in step a or b can be carried out in an air atmosphere.

[0048] In one embodiment, during gradient calcination, the temperature of the third holding treatment can be 200–300°C, more specifically 250–300°C, for example 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, or 290°C; the duration of the third holding treatment can be 0.5–1 hour, for example 40 minutes, 50 minutes, 55 minutes, or 58 minutes. The third holding treatment can remove residual moisture and other liquid materials from the solid.

[0049] In one embodiment, the system (e.g., from room temperature) is heated to 200-300°C at a heating rate of 2-5°C / min (e.g., 3°C / min or 4°C / min) for a third heat preservation treatment.

[0050] In one embodiment, during gradient calcination, the temperature of the fourth holding treatment can be 500–650°C, for example, 510°C, 520°C, 530°C, 550°C, 560°C, 580°C, 600°C, 620°C, or 640°C; the duration of the fourth holding treatment can be 2–3 hours, for example, 2.5 hours. This fourth holding treatment can remove trace amounts of residual carbonaceous material from titanium dioxide and stabilize its crystal form (e.g., anatase / rutile).

[0051] In one embodiment, during gradient calcination, the temperature of the system is increased from 200–300°C to 500–650°C at a heating rate of 5–10°C / min (e.g., 6°C / min, 7°C / min, 8°C / min, or 9°C / min).

[0052] In one embodiment, after the gradient calcination in step a is completed, the system is naturally cooled to room temperature to obtain a powdered titanium dioxide product with a purity of ≥96% and a recovery rate of ≥88%, which can be directly reused in high-end fields such as photovoltaics, coatings, and ceramics.

[0053] In one embodiment, step b of the acid treatment-calcination treatment includes: calcining the titanium dioxide-containing powder (e.g., a wet, water-containing powder) at 400–500°C (e.g., 420°C, 430°C, 450°C, 460°C, or 480°C), and further at 400–420°C, for a duration of 0.5–3 hours, such as 0.6 hours, 0.8 hours, 0.9 hours, 1 hour, 1.1 hours, 1.2 hours, 1.5 hours, 2 hours, or 2.5 hours. The calcination treatment removes residual carbon and organic matter from the solid.

[0054] In one embodiment, in step b, the temperature at which the calcined product is treated with the acid solution can be 60–90°C, more specifically 65–75°C, for example 65°C, 68°C, 69°C, 70°C, 71°C, 72°C, 75°C, 78°C, 80°C, 82°C, 85°C, or 88°C; the treatment time can be 20–70 min, more specifically 25–35 min, for example 27 min, 28 min, 29 min, 30 min, 31 min, 32 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, or 65 min.

[0055] In one embodiment, in step b, the calcined product is treated with an acid solution, followed by solid-liquid separation of the system. The resulting solid is then dried to obtain a titanium dioxide product. Further, the drying temperature can be 100–120°C, for example, 110°C, 120°C, 130°C, 150°C, 160°C, or 180°C.

[0056] This invention discloses a method for enriching titanium dioxide from waste wind turbine blades. Through gradient pyrolysis, titanium dioxide is selectively purified and recovered from waste wind turbine blades, overcoming the resource utilization blind spot of existing pyrolysis technologies that only recover fiberglass. This fills the industry technology gap in the high-value recovery of titanium dioxide after pyrolysis, achieving full-component resource utilization of titanium dioxide, fiberglass, and resin pyrolysis products from wind turbine blades. Furthermore, gradient pyrolysis enables complete resin pyrolysis, avoiding the densification of residual carbon caused by single-stage high-temperature treatment, thus laying the foundation for subsequent impurity removal from residual carbon.

[0057] The present invention discloses a method for enriching titanium dioxide from waste wind turbine blades, which can effectively separate titanium dioxide from other materials (such as residual carbon). For example, the residual carbon removal rate can be above 95%, and the method avoids the problem of titanium dioxide agglomeration caused by single calcination, thus preserving the original crystal form and particle size characteristics of titanium dioxide to the greatest extent.

[0058] This invention discloses a method for enriching titanium dioxide from waste wind turbine blades. The method involves first calcining titanium dioxide-containing powder at 400–500°C, followed by acid treatment. This process removes organic matter from the titanium dioxide powder beforehand, making impurities easier to dissolve during acid treatment and shortening the treatment time. Furthermore, direct calcination of the titanium dioxide powder removes organic matter and generates micropores, facilitating a more thorough acid reaction. Additionally, the method of calcining before acid treatment eliminates the need for high-temperature calcination, significantly reducing energy consumption, and is suitable for applications such as coatings and plastic fillers where high crystal form requirements are not critical.

[0059] The present invention discloses a method for enriching titanium dioxide from waste wind turbine blades. This method has strong process adaptability and high industrial feasibility. The pyrolysis equipment is conventional equipment in the chemical and solid waste treatment industries and does not require customized modification. The segmented pyrolysis process reduces the energy consumption of resin pyrolysis, uses less chemical reagents and can be neutralized, and has no secondary pollution.

[0060] This invention discloses a method for enriching titanium dioxide from waste wind turbine blades. The recovered titanium dioxide product has high economic value, the coarse glass fiber can be directly recycled for composite material production, and the resin pyrolysis gas and pyrolysis oil can be recycled as fuel. This significantly reduces the process operating cost, conforms to the "dual carbon" and circular economy policies, and has significant economic and environmental benefits.

[0061] The following describes a method for enriching titanium dioxide from waste wind turbine blades according to one embodiment of the present invention, with reference to specific examples. The raw materials and testing or calculation methods involved in each embodiment and comparative example are as follows: 1. The resin contained in decommissioned wind turbine blades is epoxy resin, and the titanium dioxide content w1 is 0.072%; 2. The purity (i.e., titanium dioxide content) of the titanium dioxide product was determined by XRF. 3. The formula for calculating the yield of titanium dioxide products is as follows: Yield = (m2 × w2) / (m1 × w1) × 100% Where m1 is the mass of the decommissioned wind turbine blades used, w1 is the titanium dioxide content in the wind turbine blades, m2 is the mass of the obtained titanium dioxide product, and w2 is the purity of the titanium dioxide product. 4. Residual carbon content Titanium dioxide product with mass m2 was calcined at 600℃ for 2 hours to obtain residual solid with mass m3. The residual carbon content was (m2-m3) / m2×100%.

[0062] Example 1 S1: Remove the metal inserts, sheaths and other external components from the surface of the retired wind turbine blades; then, cut and break the blades into 10-20cm blocks.

[0063] S2: The block blades are fed into a rotary pyrolysis furnace, nitrogen is introduced as a protective gas, the temperature of the pyrolysis furnace is raised to 300℃ at a rate of 5℃ / min and held for 1h; then, the temperature is raised to 500℃ at a rate of 8℃ / min and held for 2.5h; the system is allowed to cool naturally to room temperature, the solid in the furnace is collected, and the solid pyrolysis product is obtained.

[0064] S3: Place the solid pyrolysis product in an oxidation reactor, add 10% hydrogen peroxide solution (liquid-solid ratio of 4:1 ml / g), and stir the reaction at 60℃ for 40 min; then, separate the solid and liquid components of the system to obtain the oxidized solid.

[0065] S4: The oxidized solid is sieved through a 100-mesh sieve to separate it into powder. The powder is then rinsed with deionized water until neutral and dried at 90°C to obtain titanium dioxide-containing powder.

[0066] S5: Mix the titanium dioxide powder with 5% hydrochloric acid, stir and react at 70°C for 60 min, and then centrifuge to obtain the acid-treated solid (containing water).

[0067] S6: The acid-treated solid is placed in a box-type calcining furnace and subjected to gradient calcination in an air atmosphere. The specific process is as follows: the temperature of the calcining furnace is increased to 250℃ at a rate of 3℃ / min and held at that temperature for 1 hour; then, the temperature is increased to 500℃ at a rate of 6℃ / min and held for 2 hours to obtain a titanium dioxide enriched product.

[0068] The purity of the titanium dioxide product was measured using the aforementioned method, and the results are shown in Table 1.

[0069] Example 2 This embodiment uses essentially the same raw materials and processes as Example 1 to enrich titanium dioxide from waste wind turbine blades. The difference lies in steps S4, S5, and S6, as detailed below: S4: The oxidized solid is separated by sieving through a 100-mesh sieve to obtain a wet powder solid; S5: Calcine the wet powdered solid at 400℃ for 1 hour to obtain the calcined product.

[0070] S6: Mix the calcined product with 5% dilute hydrochloric acid, stir and react at 70°C for 30 min, then centrifuge to separate the solid, and dry the separated solid at 110°C for 1 h to obtain titanium dioxide product.

[0071] The purity of the titanium dioxide product was measured using the aforementioned method, and the results are shown in Table 1.

[0072] Example 3 This embodiment uses the same raw materials and processes as Example 1 to enrich titanium dioxide from waste wind turbine blades. The difference is that a 200-mesh sieve is used in step S4.

[0073] The purity of the titanium dioxide product was measured using the aforementioned method, and the results are shown in Table 1.

[0074] Example 4 S1: Remove metal inserts, sheaths, and other external components from the surface of the retired wind turbine blades; then, crush the blades into 10-20cm blocks using a jaw crusher.

[0075] S2: The block blades are fed into a rotary pyrolysis furnace, nitrogen is introduced as a protective gas, the temperature of the pyrolysis furnace is raised to 250℃ at a rate of 5℃ / min and held for 2h; then, the temperature is raised to 650℃ at a rate of 8℃ / min and held for 2h; the system is allowed to cool naturally to room temperature, the solid in the furnace is collected, and the solid pyrolysis product is obtained.

[0076] S3: Place the solid pyrolysis product in an oxidation reactor, add 5% hydrogen peroxide solution (liquid-solid ratio of 5:1 ml / g), and stir the reaction at 70°C for 30 min; then, separate the solid and liquid components of the system to obtain the oxidized solid.

[0077] S4: The oxidized solid is sieved through a 100-mesh sieve to separate it into powder. The powder is then rinsed with deionized water until neutral and dried at 90°C to obtain titanium dioxide-containing powder.

[0078] S5: Mix the titanium dioxide powder with 10% hydrochloric acid, stir and react at 60°C for 80 min, and then centrifuge to obtain the acid-treated solid (containing water).

[0079] S6: The acid-treated solid is placed in a box-type calcining furnace and subjected to gradient calcination in an air atmosphere. The specific process is as follows: the temperature of the calcining furnace is increased to 300℃ at a rate of 3℃ / min and held at that temperature for 1 hour; then, the temperature is increased to 650℃ at a rate of 6℃ / min and held for 2 hours to obtain a titanium dioxide enriched product.

[0080] The purity of the titanium dioxide product was measured using the aforementioned method, and the results are shown in Table 1.

[0081] Comparative Example 1 This example uses the same raw materials and process as Example 1 to separate and enrich titanium dioxide from waste wind turbine blades. The difference is that the protective gas in step S2 is a mixture of nitrogen and oxygen, in which the volume percentage of oxygen is 1.5%.

[0082] The purity of the titanium dioxide product was measured using the aforementioned method, and the results are shown in Table 1.

[0083] Comparative Example 2 This example uses essentially the same raw materials and processes as Example 1 to enrich titanium dioxide from waste wind turbine blades. The difference is that a 40-mesh sieve is used in step S4.

[0084] The purity of the titanium dioxide product was measured using the aforementioned method, and the results are shown in Table 1.

[0085] Comparative Example 3 This example uses essentially the same raw materials and processes as Example 1 to enrich titanium dioxide from waste wind turbine blades. The difference is that a 400-mesh sieve is used in step S4.

[0086] The purity of the titanium dioxide product was measured using the aforementioned method, and the results are shown in Table 1.

[0087] Comparative Example 4 This example uses essentially the same raw materials and processes as Example 1 to enrich titanium dioxide from waste wind turbine blades. The difference lies in step S6, which is different: S6: The acid-treated solid is placed in a box-type calcining furnace and subjected to gradient calcination in an air atmosphere. The specific process is as follows: the temperature of the calcining furnace is raised to 250℃ at a rate of 5℃ / min and held at that temperature for 1 hour; then, the temperature is raised to 900℃ at a rate of 10℃ / min and held for 3 hours to obtain a titanium dioxide enriched product.

[0088] The purity of the titanium dioxide product was measured using the aforementioned method, and the results are shown in Table 1.

[0089] Comparative Example 5 This example uses essentially the same raw materials and processes as Example 1 to enrich titanium dioxide from waste wind turbine blades. The difference lies in step S6, which is different: S6: Place the acid-treated solid in a box-type calcining furnace and calcine it in an air atmosphere. The specific process is as follows: raise the temperature of the calcining furnace to 250℃ at a rate of 5℃ / min and hold it at that temperature for 1 hour.

[0090] The purity of the titanium dioxide product was measured using the aforementioned method, and the results are shown in Table 1.

[0091] Comparative Example 6 This example uses essentially the same raw materials and processes as Example 1 to enrich titanium dioxide from waste wind turbine blades. The difference is that step S3 is omitted, and the solid pyrolysis product obtained in step S2 is directly processed in step S4 and subsequent steps S5 and S6.

[0092] The purity of the titanium dioxide product was measured using the aforementioned method, and the results are shown in Table 1.

[0093] Table 1

[0094] Referring to Comparative Example 1, the difference from Example 1 is that the protective gas in step S2 contains 1.5 vol% oxygen. Further referring to the results in Table 1, it can be seen that the yield of the product in Example 1 is significantly higher than that of the product in Comparative Example 1. The presence of oxygen in the protective gas intensifies the resin decomposition reaction in the wind turbine blades, and titanium is easily carried away, leading to a decrease in yield. Therefore, the volume content of oxygen in the protective gas is preferably less than 1 vol%.

[0095] Referring to Examples 1 and 3 and Comparative Examples 2 and 3, the difference lies in the mesh size of the sieves used in step S4, which are 100 mesh, 200 mesh, 40 mesh, and 400 mesh, respectively. Further referring to the results in Table 1, it can be seen that the titanium dioxide content (or purity) of the products from Examples 1 and 3 is significantly higher than that of the product from Comparative Example 2, and the yield of the products from Examples 1 and 3 is significantly higher than that of the product from Comparative Example 3. Therefore, it is preferable to sieve the oxidized solid through a sieve of 100-200 mesh.

[0096] Referring to Examples 1 and Comparative Examples 4 and 5, the differences lie in the calcination method and temperature of step S6. Further, referring to the results in Table 1, it can be seen that the yield of the product in Comparative Example 4 is significantly lower than that of the product in Example 1, and the residual carbon content of the product in Comparative Example 5 is too high. Therefore, in step a of the acid treatment-calcination process in this embodiment of the invention, by using gradient calcination at a specific temperature, a titanium dioxide product with high purity, high yield, and low residual carbon content can be obtained.

[0097] Referring to Comparative Example 6, the difference from Example 1 is that the solid pyrolysis product of step S2 was not oxidized. Further referring to the results in Table 1, it can be seen that the purity and yield of the product in Example 1 are significantly higher than those in Comparative Example 6. Therefore, oxidizing the solid pyrolysis product can improve the purity and yield of the recovered titanium dioxide product.

[0098] Unless otherwise specified, the terms used in this invention have the meanings commonly understood by those skilled in the art.

[0099] The embodiments described in this invention are for illustrative purposes only and are not intended to limit the scope of protection of this invention. Those skilled in the art can make various other substitutions, changes and improvements within the scope of this invention. Therefore, this invention is not limited to the above embodiments, but is only defined by the claims.

Claims

1. A method for enriching titanium dioxide from waste wind turbine blades, comprising the following steps: Waste wind turbine blades are subjected to gradient pyrolysis to obtain solid pyrolysis products; The solid pyrolysis product is oxidized to obtain an oxidized solid. The oxidized solid was sieved and separated to obtain a powder containing titanium dioxide; The titanium dioxide-containing powder is subjected to acid treatment-calcination to obtain the titanium dioxide product. in, The acid treatment-calcination process includes step a: treating the titanium dioxide-containing powder with an acid solution, followed by solid-liquid separation to obtain an acid-treated solid; then, subjecting the acid-treated solid to gradient calcination; or, The acid treatment-calcination treatment includes step b: calcining the titanium dioxide-containing powder at 400-500°C to obtain a calcined product; then, treating the calcined product with an acid solution. The gradient pyrolysis includes sequentially subjecting the waste wind turbine blades to a first heat preservation treatment at 250–350°C and a second heat preservation treatment at 500–650°C; the gradient calcination in step a includes sequentially subjecting the acid-treated solid to a third heat preservation treatment at 200–300°C and a fourth heat preservation treatment at 500–650°C.

2. The method according to claim 1, wherein, The waste wind turbine blades are subjected to gradient pyrolysis under the action of a protective gas; and / or The sieving and separation is performed using a 100-200 mesh sieve. And / or, The temperature of the first heat preservation treatment is 250-300℃.

3. The method according to claim 2, wherein, The protective gas includes one or more of nitrogen and inert gases; and / or, The oxygen content in the protective gas is less than 1 vol.

4. The method according to claim 1, wherein, In the gradient pyrolysis, the first heat treatment lasts for 1–2 hours; and / or, the second heat treatment lasts for 2–3 hours; and / or, The solid pyrolysis products are subjected to the oxidation treatment by plasma, ozone, or an oxidant solution, wherein the oxidant includes hydrogen peroxide and / or sodium hypochlorite; and / or... In step b, the titanium dioxide-containing powder is calcined at 400–420°C.

5. The method according to claim 4, wherein, The oxidant solution is a hydrogen peroxide solution, and the mass concentration of the hydrogen peroxide solution is 5-15%; or... The oxidant solution is a sodium hypochlorite solution, and the mass concentration of the sodium hypochlorite solution is 10-20%.

6. The method according to claim 5, wherein, The oxidation treatment temperature is 50–70°C; and / or, The oxidation treatment time is 30 to 60 minutes.

7. The method according to claim 5, wherein, The oxidation treatment temperature is 60–70°C; and / or, The oxidation treatment time is 30 to 40 minutes.

8. The method according to claim 1, wherein, The acid solution includes one or more of hydrochloric acid, sulfuric acid, hydrofluoric acid, and oxalic acid; and / or, The temperature of the third heat preservation treatment is 250–300°C; and / or, In step b, the temperature at which the calcined product is treated with the acid solution is 60–90°C, and / or the treatment time is 20–70 min.

9. The method according to claim 1, wherein, The mass concentration of the acid solution is 5-10%; and / or, In step a, the temperature at which the titanium dioxide-containing powder is treated with the acid solution is 60–80°C, and / or the treatment time is 40–80 min.

10. The method according to claim 1, wherein, The titanium dioxide-containing powder is calcined at 400–500°C for 0.5–3 hours; and / or, In the gradient calcination, the third heat preservation treatment lasts for 0.5 to 1 hour; and / or, the fourth heat preservation treatment lasts for 2 to 3 hours.