Fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence and its preparation method

By introducing AgCl into rare-earth-doped fluoride glass to form silver nanoparticles, and utilizing the localized surface plasmon resonance effect, the problems of insufficient luminescence intensity and efficiency are solved, achieving a highly efficient mid-infrared luminescence effect, which is suitable for mid-infrared lasers and fiber amplifiers.

CN123106004APending Publication Date: 2026-11-17NORTHEAST NORMAL UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611514490.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The luminescence intensity and efficiency of existing rare-earth ion-doped fluoride glasses are insufficient, especially in the mid-infrared band. Furthermore, existing preparation methods are costly and inefficient, making them incompatible with fluoride glass melting processes, and the distribution of silver nanoparticles is uneven.

Method used

Using ZrF4-ZnF2-BaF2-SrF2-CaF2-AlF3-YF3 as the matrix and introducing AgCl as the silver source, silver nanoparticles were formed through melt casting and heat treatment. The luminescence of rare earth ions was enhanced by the localized surface plasmon resonance effect. The preparation method is simple and easy to control.

Benefits of technology

It significantly improves the luminescence intensity and efficiency in the mid-infrared band, reduces the preparation difficulty and cost, and achieves uniform precipitation of silver nanoparticles in glass, making it suitable for mid-infrared lasers and fiber amplifiers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106004A_ABST
    Figure CN123106004A_ABST
Patent Text Reader

Abstract

This invention relates to the field of rare earth luminescent material processing technology, and particularly to a fluoride glass with silver nanoparticle-enhanced rare earth ion luminescence and its preparation method. The raw material components, by molar amount, are: 21-25 parts ZrF4, 18-22 parts ZnF2, 12-16 parts BaF2, 10-15 parts SrF2, 4-8 parts CaF2, 13-17 parts AlF3, (9-x) parts YF3, x parts AgCl, and 0.5-1.5 parts ErF3, with a total molar amount of 100; wherein 0 < x ≤ 1. Using AgCl as the silver source, silver nanoparticles are formed in situ in the glass through melt casting and low-temperature heat treatment, improving ErF3 while maintaining the advantages of the fluoride glass matrix. 3+ This method improves mid-infrared luminescence intensity and efficiency, and features low equipment requirements and easy parameter control in the preparation process. Its advantage lies in the significantly enhanced luminescence intensity, making it suitable for luminescence enhancement in the mid-infrared band.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fluoride optical glass processing technology, and in particular to a fluoride glass with silver nanoparticle-enhanced rare earth ion luminescence and its preparation method. Background Technology

[0002] Rare-earth ion-doped fluoride glasses are an important class of optical matrix materials. Compared with common oxide glasses, fluoride glasses have lower phonon energies, typically around 400–600 cm⁻¹. -1 It has advantages such as wide light transmission range, high rare earth ion solubility and low non-radiative relaxation loss, and therefore has application value in mid-infrared lasers, fiber amplification and infrared light-emitting devices.

[0003] However, Er 3+ The 4f-4f transitions of rare-earth ions are parity-forbidden transitions, with limited intrinsic absorption cross-sections and radiative transition probabilities. In conventional rare-earth ion-doped fluoride glasses, even with low matrix phonon energies, the luminous intensity and efficiency may still be insufficient to meet the requirements of high-brightness, high-efficiency devices.

[0004] Existing research indicates that introducing noble metal nanoparticles, particularly silver nanoparticles, into a glass matrix can generate an enhanced local electromagnetic field around rare earth ions through localized surface plasmon resonance (LSPR), thereby increasing the excitation rate and radiative transition probability of rare earth ions. Common methods for introducing or precipitating plasmonic nanoparticles include heat treatment, ion implantation, femtosecond laser-induced precipitation, sol-gel methods, and magnetron sputtering.

[0005] For fluoride glass systems, the glass composition is easily affected by moisture, fluorine volatilization, and crystallization, resulting in a relatively narrow process window. Introducing metal nanostructures using methods such as ion implantation, femtosecond lasers, or magnetron sputtering typically presents challenges including high equipment costs, low processing efficiency, uneven nanoparticle distribution, and difficulty in integrating with batch melting processes.

[0006] The existing technology has at least the following shortcomings: (1) The luminescence intensity of rare earth ion-doped fluoride glasses without the introduction of plasmon enhancement structures is limited, especially in the mid-infrared band, and there is still room for improvement in luminescence efficiency. (2) Some methods for preparing noble metal nanoparticles require expensive equipment or complex post-processing, which is not fully compatible with the characteristics of fluoride glasses such as easy moisture absorption, easy crystallization, and narrow thermal stability window. (3) The existing technology lacks a directly implementable combination of formulas and process parameters between silver source introduction, glass melting, annealing, and silver nanoparticle precipitation, making it difficult to balance glass forming quality and luminescence enhancement effect. Therefore, a preparation method that is compatible with the fluoride glass melting and casting process, is easy to operate, and can controllably form silver nanoparticles is needed. Summary of the Invention

[0007] To address the aforementioned problems, this invention provides a fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence and its preparation method.

[0008] The primary objective of this invention is to provide a fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence, comprising the following raw material components in molar amounts: 21-25 parts ZrF4, 18-22 parts ZnF2, 12-16 parts BaF2, 10-15 parts SrF2, 4-8 parts CaF2, 13-17 parts AlF3, (9-x) parts YF3, x parts AgCl, 0.5-1.5 parts ErF3, with a total molar fraction of 100; where 0 < x ≤ 1.

[0009] Preferably, the value of x is in the range of 0.1≤x≤0.3.

[0010] Preferably, the raw material composition is 23 parts ZrF4, 20 parts ZnF2, 14 parts BaF2, 12 parts SrF2, 6 parts CaF2, 15 parts AlF3, (9-x) parts YF3, x parts AgCl, and 1 part ErF3; x takes the value of 0.1, 0.2, or 0.3.

[0011] The second objective of this invention is to provide a method for preparing fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence, specifically comprising the following steps: S1. Weigh each raw material precisely according to the molar ratio to obtain a mixed powder, add a dehydrating agent, and mix evenly; heat at 800~950℃ for 0.5~1h to complete fluorination and dehydration; S2. Preheat the copper plate to 300~350℃ in advance; under the protective atmosphere of nitrogen and oxygen, melt the mixture of fluorination and dehydration in step S1 at 800~950℃ for 1.5~2.5h to obtain molten glass liquid; S3. Quickly pour the molten glass onto the surface of the preheated copper plate, then transfer it to an annealing furnace, heat it to 300~330℃ and hold it at that temperature for 2.5~3.5 hours; then cool it to room temperature. S4. Polish until the glass thickness is 2~3mm; S5. Under a nitrogen atmosphere, the polished glass is heated to 350~380℃ and kept at that temperature for 3~5 hours, then naturally cooled to room temperature to obtain fluoride glass with silver nanoparticle-enhanced rare earth ion luminescence.

[0012] Preferably, the dehydration agent accounts for 20-30% of the total mass of the mixed powder; the dehydration agent is ammonium bifluoride.

[0013] Preferably, in step S2, the copper plate is preheated to 310~320℃; the volume fractions of nitrogen and oxygen in the mixed protective gas are 95% and 5%, respectively; and it is melted at 800~900℃ for 2 hours.

[0014] Preferably, in step S3, the temperature is raised to 315~330℃ and kept at that temperature for 3 hours.

[0015] Preferably, before preparation, the copper plate is polished, cleaned, dried with nitrogen, and then dried with hot air.

[0016] Compared with the prior art, the present invention can achieve the following beneficial effects: (1) Significantly improved luminescence intensity: By introducing AgCl and forming silver nanoparticles after heat treatment, the enhanced local electromagnetic field around rare earth ions is generated by utilizing its LSPR effect, thereby improving Er 3+ The excitation rate and radiative transition probability of ions. Experiments show that the silver-doped fluoride glass prepared in this invention has a significantly higher luminescence intensity in the mid-infrared band than that of undoped silver glass of the same type.

[0017] (2) The preparation process is simple, easy to operate and easy to control: The present invention adopts the melt casting method. Only one heat treatment is required below the glass transition temperature to induce the precipitation of silver nanoparticles. There is no need for complex equipment (such as femtosecond laser, ion implanter, magnetron sputtering instrument, etc.) or to introduce reducing gas or additional chemical reagents, which greatly reduces the preparation difficulty and cost.

[0018] (3) Suitable for mid-infrared luminescence enhancement: Fluoride matrix itself has the advantages of low phonon energy and wide light transmission range. Combined with the plasmon enhancement effect of silver nanoparticles, it is particularly suitable for optical devices with high requirements for luminescence efficiency, such as mid-infrared lasers and fiber amplifiers.

[0019] In summary, this invention addresses the weakness of existing luminescent glasses in terms of luminescence intensity by providing a silver-doped fluoride luminescent glass with high luminescence intensity and efficiency. It is composed of a fluoride glass with ZrF4-ZnF2-BaF2-SrF2-CaF2-AlF3-YF3 as the matrix, ErF3 as the rare-earth luminescent center, and AgCl as the silver source, achieving stable and uniform in-situ precipitation of silver nanoparticles while ensuring glass forming quality. Attached Figure Description

[0020] Figure 1 This is a flowchart of a method for preparing fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence according to an embodiment of the present invention.

[0021] Figure 2 The results show a comparison of the luminescence intensity of the fluoride glass with silver nanoparticle-enhanced rare earth ion luminescence provided in Examples 1-3 of the present invention and the fluoride glass prepared in Comparative Example 1. The dashed line graph shows the results of Comparative Example 1, and the solid line graphs show the results of Examples 3, 2 and 1 from top to bottom. Detailed Implementation

[0022] In the following description, embodiments of the invention will be described with reference to the accompanying drawings. In the description below, the same modules are denoted by the same reference numerals. Where the same reference numerals are used, their names and functions are also the same. Therefore, their detailed description will not be repeated.

[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and do not constitute a limitation thereof.

[0024] This invention provides a fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence, comprising the following raw material components in molar amounts: 21-25 parts ZrF4, 18-22 parts ZnF2, 12-16 parts BaF2, 10-15 parts SrF2, 4-8 parts CaF2, 13-17 parts AlF3, (9-x) parts YF3, x parts AgCl, 0.5-1.5 parts ErF3, with a total molar fraction of 100. Where 0 < x ≤ 1, preferably 0.1 ≤ x ≤ 0.3; when increasing the molar amount of AgCl, the molar amount of YF3 is reduced by the same amount; Specifically, the raw material composition is 23 parts ZrF4, 20 parts ZnF2, 14 parts BaF2, 12 parts SrF2, 6 parts CaF2, 15 parts AlF3, (9-x) parts YF3, x parts AgCl, and 1 part ErF3, where x = 0.1, 0.2, or 0.3.

[0025] The above components constitute a heptazirconium-based fluoride glass matrix, with ZrF4 serving as the main glass network forming element, constructing a stable amorphous fluoride framework. A design using an equal amount of AgCl replacing YF3 introduces silver ion precursors uniformly into the matrix without compromising glass-forming properties. ErF3 acts as the luminescent center, achieving 2.7 μm mid-infrared characteristic emission via 4f-4f electron transitions. AgCl serves as the silver source, reducing it to elemental silver nanoparticles through a subsequent dedicated heat treatment process. After melting, annealing, and low-temperature nitrogen heat treatment, the prepared fluoride glass exhibits uniformly dispersed spherical silver nanoparticles within the glass matrix, without significant agglomeration or surface enrichment. The silver nanoparticles generate localized surface plasmon resonance (LSPR) effects, with ErF3... 3+ A high-intensity local electromagnetic field is formed around the ions, which on the one hand enhances Er 3+ On the one hand, it increases the absorption efficiency of the pump excitation light, and on the other hand, it increases Er. 3+ The radiative transition probability is significantly reduced, and the non-radiative relaxation loss is reduced, ultimately resulting in a substantial increase in luminescence intensity in the 2.7μm mid-infrared band, thus overcoming the weakness of traditional rare-earth-doped fluoride glasses.

[0026] The preparation method of the above-mentioned silver nanoparticle-enhanced rare-earth ion luminescence fluoride glass is shown in the flowchart below. Figure 1 As shown, the specific steps include the following: S1. Weigh each raw material precisely according to the molar ratio to obtain a mixed powder; add a dehydrating agent to the mixed powder, the mass of the dehydrating agent being 15-30% of the total mass of the mixed powder, and stir thoroughly until the powder is uniformly mixed; after mixing, heat at 800-950℃ for 0.5-1h to complete fluorination and dehydration; In some embodiments, the weighing of each raw material is carried out in a dry, nitrogen-filled glove box; the dehydration aid is ammonium bifluoride (NH4HF2), and the mass of ammonium bifluoride accounts for 1 / 5 or 4 / 15 of the total mass of the mixed powder; the mixed powder is transferred to a clean platinum crucible, placed in a tube furnace, and heated at 800°C, 850°C, or 900°C for 0.5 h.

[0027] S2. Preheat the copper plate to 300~350℃ in advance; transfer the platinum crucible that has been fluorinated and dehydrated into a high-temperature melting furnace, continuously introduce a mixed protective gas of nitrogen and oxygen, and melt at 800~950℃ for 1.5~2.5h to obtain molten glass. In some embodiments, the preheating temperature of the copper plate is 310°C, 315°C, or 320°C; the volume fractions of nitrogen and oxygen in the mixed protective gas are 95% and 5%, respectively; and melting is performed at 800°C, 850°C, or 900°C for 2 hours.

[0028] S3. Quickly pour the molten glass onto the surface of the preheated copper plate, then transfer it to an annealing furnace and heat it to 300~330℃ and hold it at that temperature for 2.5~3.5 hours; slowly cool it to room temperature to eliminate internal thermal stress in the glass and prevent cracking and crystallization. In some embodiments, the temperature is kept constant at 315°C, 325°C, or 330°C for 3 hours.

[0029] S4. Polishing is performed using an optical polishing machine. After polishing, the glass thickness is controlled at 2~3mm to ensure uniform heat treatment and light transmittance requirements for spectral testing. In some embodiments, the thickness of the polished glass is 3 mm.

[0030] S5. Under a nitrogen atmosphere, the polished glass is heated to 350~380℃ and kept at that temperature for 3~5 hours, then naturally cooled to room temperature, so that the silver species inside the glass can form silver nanoparticles in situ, thus obtaining fluoride glass with silver nanoparticle-enhanced rare earth ion luminescence. In some embodiments, the nitrogen gas is 100% high-purity nitrogen gas; the temperature is raised to 350°C, 360°C or 380°C and kept at a constant temperature for 4 hours.

[0031] All instruments must be thoroughly cleaned and dried before preparation; copper plates can be polished first, then cleaned, dried with nitrogen, and then dried with hot air.

[0032] Example 1: This embodiment provides a fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence, comprising the following raw material components in molar amounts: 23 parts ZrF4, 20 parts ZnF2, 14 parts BaF2, 12 parts SrF2, 6 parts CaF2, 15 parts AlF3, 8.9 parts YF3, 0.1 parts AgCl, 1 part ErF3; The preparation method specifically includes the following steps: S1. Weigh the above raw materials precisely according to the molar ratio to obtain a total of 15g of mixed powder; add 3g of H4HF2 to the mixed powder and stir thoroughly until the powder is uniformly mixed; pour the mixture into a clean platinum crucible and heat at 900℃ for 0.5h to complete fluorination and dehydration; S2. Preheat the copper plate to 320℃; transfer the platinum crucible that has undergone fluorination and dehydration into a high-temperature melting furnace, continuously introduce a mixed protective gas of nitrogen and oxygen, and melt at 900℃ for 2 hours to obtain molten glass; the volume fractions of nitrogen and oxygen are 95% and 5%, respectively. S3. Quickly pour the molten glass onto the surface of the preheated copper plate, then transfer it to an annealing furnace, heat it to 330℃ and hold it at that temperature for 3 hours; slowly cool it to room temperature to obtain the annealed glass; S4. Polish both sides of the annealed glass to a thickness of 3mm to facilitate subsequent heat treatment and optical testing; S5. The polished glass is placed in a 100% N2 atmosphere and heated to 380℃ and kept at that temperature for 4 hours, so that the silver species inside the glass form silver nanoparticles in situ, resulting in fluoride glass with silver nanoparticle-enhanced rare earth ion luminescence.

[0033] Example 2: This embodiment provides a fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence, comprising the following raw material components in molar amounts: 23 parts ZrF4, 20 parts ZnF2, 14 parts BaF2, 12 parts SrF2, 6 parts CaF2, 15 parts AlF3, 8.8 parts YF3, 0.2 parts AgCl, 1 part ErF3; The preparation method specifically includes the following steps: S1. Weigh the above raw materials precisely according to the molar ratio to obtain a total of 30g of mixed powder; add 6g of H4HF2 to the mixed powder and stir thoroughly until the powder is uniformly mixed; pour the mixture into a clean platinum crucible and heat at 850℃ for 0.5h to complete fluorination and dehydration; S2. Preheat the copper plate to 315℃; transfer the platinum crucible that has undergone fluorination and dehydration into a high-temperature melting furnace, continuously introduce a mixed protective gas of nitrogen and oxygen, and melt at 850℃ for 2 hours to obtain molten glass; the volume fractions of nitrogen and oxygen are 95% and 5%, respectively. S3. Quickly pour the molten glass onto the surface of the preheated copper plate, then transfer it to an annealing furnace, heat it to 325℃ and hold it at that temperature for 3 hours; slowly cool it to room temperature to obtain the annealed glass; S4. Polish both sides of the annealed glass to a thickness of 3mm to facilitate subsequent heat treatment and optical testing; S5. The polished glass is placed in a 100% N2 atmosphere and heated to 360℃ and kept at that temperature for 4 hours, so that the silver species inside the glass form silver nanoparticles in situ, resulting in fluoride glass with silver nanoparticle-enhanced rare earth ion luminescence.

[0034] Example 3: This embodiment provides a fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence, comprising the following raw material components in molar amounts: 23 parts ZrF4, 20 parts ZnF2, 14 parts BaF2, 12 parts SrF2, 6 parts CaF2, 15 parts AlF3, 8.7 parts YF3, 0.3 parts AgCl, 1 part ErF3; The preparation method specifically includes the following steps: S1. Weigh the above raw materials precisely according to the molar ratio to obtain a total of 30g of mixed powder; add 8g of H4HF2 to the mixed powder and stir thoroughly until the powder is evenly mixed; pour the mixture into a clean platinum crucible and heat at 800℃ for 0.5h to complete fluorination and dehydration; S2. Preheat the copper plate to 310℃; transfer the platinum crucible that has undergone fluorination and dehydration into a high-temperature melting furnace, continuously introduce a mixed protective gas of nitrogen and oxygen, and melt at 800℃ for 2 hours to obtain molten glass; the volume fractions of nitrogen and oxygen are 95% and 5%, respectively. S3. Quickly pour the molten glass onto the surface of the preheated copper plate, then transfer it to an annealing furnace, heat it to 315℃ and hold it at that temperature for 3 hours; slowly cool it to room temperature to obtain the annealed glass; S4. Polish both sides of the annealed glass to a thickness of 3mm to facilitate subsequent heat treatment and optical testing; S5. The polished glass is placed in a 100% N2 atmosphere and heated to 350℃ and kept at that temperature for 4 hours, so that the silver species inside the glass form silver nanoparticles in situ, resulting in fluoride glass with silver nanoparticle-enhanced rare earth ion luminescence.

[0035] Comparative Example 1: This embodiment provides a rare-earth ion luminescent fluoride glass, which comprises the following raw material components in molar amounts: 23 parts ZrF4, 20 parts ZnF2, 14 parts BaF2, 12 parts SrF2, 6 parts CaF2, 15 parts AlF3, 9 parts YF3, 1 part ErF3; The preparation method is the same as in Example 1.

[0036] Figure 2 Examples 1-3 of this invention are comparative examples 1 and 2 with undoped silver chloride. 3+ Mid-infrared emission spectrum comparison curves; the solid lines in the figure represent the silver-doped fluoride glasses prepared in Examples 1-3, and the dashed lines represent the fluoride glasses prepared in Comparative Example 1. The test results clearly show that the emission peaks of all four curves are located near 2700 nm (i.e., the 2.7 μm mid-infrared characteristic emission band); the samples of Examples 1-3 rely on the localized surface plasmon resonance enhancement effect of silver nanoparticles precipitated in situ inside the glass, and their peak emission relative intensity is significantly higher than that of the undoped comparative sample. This proves that the present invention, through AgCl doping and heat treatment to introduce silver nanostructures, can effectively enhance Er... 3+ The luminescence efficiency in the mid-infrared band at 2.7μm solves the technical problem of weak infrared luminescence in traditional rare-earth-doped fluoride glasses.

[0037] It should be understood that the various forms of processes shown above can be used to reorder, add, or delete steps. For example, the steps described in this invention disclosure can be executed in parallel, sequentially, or in different orders, as long as the desired result of the technical solution disclosed in this invention can be achieved, and this is not limited herein.

[0038] The specific embodiments described above do not constitute a limitation on the scope of protection of this invention. Those skilled in the art should understand that various modifications, combinations, sub-combinations, and substitutions can be made according to design requirements and other factors. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this invention should be included within the scope of protection of this invention.

Claims

1. A fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence, characterized in that: On a molar basis, it includes the following raw material components: 21-25 parts ZrF4, 18-22 parts ZnF2, 12-16 parts BaF2, 10-15 parts SrF2, 4-8 parts CaF2, 13-17 parts AlF3, (9-x) parts YF3, x parts AgCl, 0.5-1.5 parts ErF3, with a total molar fraction of 100; where 0 < x ≤ 1.

2. The fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence according to claim 1, characterized in that: The range of x is 0.1 ≤ x ≤ 0.

3.

3. The fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence according to claim 1, characterized in that: The raw material components are 23 parts ZrF4, 20 parts ZnF2, 14 parts BaF2, 12 parts SrF2, 6 parts CaF2, 15 parts AlF3, (9-x) parts YF3, x parts AgCl, and 1 part ErF3; x takes the value of 0.1, 0.2, or 0.

3.

4. A method for preparing a fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence, used to prepare the fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence as described in claim 1, characterized in that: Specifically, the steps include the following: S1. Weigh each raw material precisely according to the molar ratio to obtain a mixed powder, add a dehydrating agent, and mix evenly; heat at 800~950℃ for 0.5~1h to complete fluorination and dehydration; S2. Preheat the copper plate to 300~350℃ in advance; under the protective atmosphere of nitrogen and oxygen, melt the mixture of fluorination and dehydration in step S1 at 800~950℃ for 1.5~2.5h to obtain molten glass liquid; S3. Quickly pour the molten glass onto the surface of the preheated copper plate, then transfer it to an annealing furnace, heat it to 300~330℃ and hold it at that temperature for 2.5~3.5 hours; then cool it to room temperature. S4. Polish until the glass thickness is 2~3mm; S5. Under a nitrogen atmosphere, the polished glass is heated to 350~380℃ and kept at that temperature for 3~5 hours, then naturally cooled to room temperature to obtain fluoride glass with silver nanoparticle-enhanced rare earth ion luminescence.

5. The method for preparing a fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence according to claim 4, characterized in that: The dehydration aid accounts for 20-30% of the total mass of the mixed powder; the dehydration aid is ammonium bifluoride.

6. The method for preparing a fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence according to claim 4, characterized in that: In step S2, the copper plate is preheated to 310~320℃; the volume fractions of nitrogen and oxygen in the mixed protective gas are 95% and 5%, respectively; and it is melted at 800~900℃ for 2 hours.

7. The method for preparing a fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence according to claim 4, characterized in that: In step S3, the temperature is raised to 315~330℃ and kept at that temperature for 3 hours.

8. The method for preparing a fluoride glass with silver nanoparticle-enhanced rare-earth ion luminescence according to claim 4, characterized in that: Before preparation, the copper plate is polished, then cleaned, dried with nitrogen, and then dried with hot air.