Ultra-high performance concrete using diabase coarse aggregate and its preparation method
By adopting diabase coarse aggregate and optimizing the preparation process, the problems of aggregate selection and mix proportion in ultra-high performance concrete have been solved, realizing the preparation of high-strength, low-cost concrete, which is suitable for high-end projects such as bridges and wind power towers.
Patent Information
- Application Number
- CN202611155814.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-31
- Publication Date
- 2026-11-17
AI Technical Summary
In existing ultra-high performance concrete, the selection of coarse aggregates is limited and the mix design is unreasonable, resulting in high cost and unstable performance. In addition, traditional aggregates are difficult to process and have poor interfacial bonding performance, which affects the long-term durability of concrete.
Using diabase coarse aggregate as the core aggregate, combined with mixed sand, cementitious materials and polycarboxylate high-performance water-reducing agent, ultra-high performance concrete is prepared through segmented mixing, layered vibration and precise curing, optimizing the gradation design and water-cement ratio to form a densely packed structure.
It improves the strength, fluidity, and density of concrete, has stable and reliable performance, is suitable for industrial production, reduces costs, and is applicable to high-end engineering fields.
Smart Images

Figure CN123106102A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ultra-high performance concrete technology, and in particular to an ultra-high performance concrete using diabase coarse aggregate and its preparation method. Background Technology
[0002] Ultra-high performance concrete (UHPC) is a new type of cement-based composite material with ultra-high strength, high durability, and high toughness. Its compressive strength is typically ≥120MPa and its flexural strength is ≥15MPa. Compared with ordinary concrete and high-performance concrete, it has significant advantages in mechanical properties and durability. It is widely used in fields with extremely high requirements for concrete performance, such as heavy-duty transportation, high-rise buildings, bridge engineering, and marine engineering.
[0003] Coarse aggregate, as the core skeleton of ultra-high performance concrete, directly affects the strength, durability, and workability of the concrete. Currently, the coarse aggregates used in existing ultra-high performance concrete are mainly quartz sand and basalt. Although these meet the basic performance requirements, they have significant limitations: First, the distribution of quartz sand and basalt resources is uneven, and mining is difficult in some areas, resulting in high raw material costs and restricting the large-scale application of ultra-high performance concrete. Second, quartz sand has high hardness but is brittle, and basalt is difficult to process and has poor particle shape. The interfacial bonding performance between these two materials and cementitious materials needs improvement, as interfacial cracking is prone to occur, affecting the long-term durability of the concrete. Third, existing mix design is mostly based on empirical formulas and does not fully incorporate the characteristics of coarse aggregate for optimization, making it difficult to balance the workability and mechanical properties of the concrete, resulting in unstable performance and cost waste.
[0004] Diabase is a basic shallow intrusive rock, mainly composed of pyroxene and basic plagioclase. It possesses excellent physical properties and good durability, and its resources are widely distributed and relatively inexpensive to mine, making it an ideal building aggregate. However, currently, diabase coarse aggregate is mainly used in asphalt pavement concrete and other processes requiring wear resistance. How to fully utilize the advantages of diabase coarse aggregate and solve the problems of limited selection of coarse aggregate, unreasonable mix proportions, high costs, and unstable performance in existing ultra-high performance concrete has become an urgent technical problem to be solved in this field. Summary of the Invention
[0005] The purpose of this invention is to provide an ultra-high performance concrete using diabase coarse aggregate and its preparation method, so as to solve the technical problems mentioned in the background art.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: An ultra-high performance concrete using diabase coarse aggregate comprises the following raw materials in parts by weight: 200-300 parts of diabase coarse aggregate, 700-850 parts of cementitious material, 600-750 parts of mixed sand, 12-18 parts of admixture, and 100-120 parts of water.
[0007] Furthermore, the particle size of the diabase coarse aggregate is 5-8 mm.
[0008] Furthermore, the particle size of the mixed sand is 0.15-5 mm.
[0009] Furthermore, the cementing material includes P O 52.5 Cement, silica fume, microspheres, fly ash.
[0010] Furthermore, the cementitious material is composed of P O 52.5 is made of cement, silica fume, microspheres and fly ash in a mass ratio of 7:1:1:1.
[0011] Furthermore, the admixture is a polycarboxylate high-performance water-reducing agent.
[0012] Furthermore, the water-to-binder ratio is less than 0.19.
[0013] A method for preparing ultra-high performance concrete using diabase coarse aggregate. S1 Raw Material Pretreatment: Dry the diabase coarse aggregate and mixed sand to a moisture content of ≤0.5%; remove impurities from the cementitious material by passing it through an 80-mesh sieve; mix the admixture with water and stir evenly to prepare an admixture aqueous solution; S2 segmented mixing: First, put the pretreated diabase coarse aggregate and mixed sand into the mixer and mix at low speed for 30-60 seconds until they are evenly mixed; then add the cementitious material and continue to mix at low speed for 60-90 seconds; finally, slowly add the admixture aqueous solution and mix at high speed for 120-180 seconds to obtain the concrete mixture. S3 Layered Vibration: Pour the concrete mixture into the mold, pour it in layers and vibrate it, with a vibration time of 10-15 seconds; S4 molding and curing: After vibration, smooth the surface of the mold and place it in the curing room for 24-48 hours before demolding; continue curing for 28 days after demolding to obtain the final product.
[0014] Furthermore, in S2, the low-speed stirring speed is 150-200 r / min, and the high-speed stirring speed is 300-350 r / min.
[0015] The advantages of this invention compared to the prior art are as follows: 1. This invention uses diabase coarse aggregate as the core aggregate of ultra-high performance concrete, making full use of the advantages of diabase such as high hardness, low crushing value, low water absorption and good durability. It adopts mixed sand to replace traditional single aggregate, and combines cement, silica fume and microsphere mineral admixtures in a synergistic system to further improve fluidity and density while ensuring ultra-high strength.
[0016] 2. This invention adopts a low water-cement ratio design, combined with overall system gradation optimization, to achieve the densest particle packing, fewer internal defects in concrete, strong interfacial bonding, stable and reliable performance, compressive strength >120MPa, flexural strength >15MPa, freeze-thaw resistance grade >F300, and impermeability grade >P12.
[0017] 3. This invention employs segmented stirring, layered vibration, and precise curing to solve the problems of poor homogeneity and large quality fluctuations in traditional preparation methods, making it suitable for industrial and large-scale production.
[0018] 4. The raw materials of this invention are widely available. Compared with traditional UHPC, it achieves controllable cost while significantly improving performance. It is green, low-carbon, and economical, and can be widely used in high-end engineering fields such as bridges, wind power hybrid towers, PC components, and heavy-duty structures. Attached Figure Description
[0019] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and preferred embodiments. However, it should be noted that many details listed in the specification are merely to provide the reader with a thorough understanding of one or more aspects of the invention, and these aspects of the invention can be achieved even without these specific details.
[0021] An ultra-high performance concrete using diabase coarse aggregate and its preparation method, comprising the following raw materials in parts by weight: 200-300 parts of diabase coarse aggregate, 700-850 parts of cementitious material, 600-750 parts of mixed sand, 12-18 parts of admixture, and 100-120 parts of water, with a water-cement ratio not exceeding 0.19.
[0022] The diabase coarse aggregate has a particle size of 5-8 mm, continuous gradation, a crushing value of 8%, a water absorption rate of 0.2%, a Mohs hardness of 6.5, and a density of 2.9 g / cm³. 3 The content of needle-like and flaky particles is 3%.
[0023] The mixed sand has a particle size of 0.15-5mm, a fineness modulus of 2.8, and a mud content of 0.3%. It is a non-alkali reactive fine aggregate that forms a gradient compact packing structure with the diabase coarse aggregate.
[0024] The mixed sand is made by mixing natural sand and manufactured sand at a mass ratio of 3:7; the natural sand is river sand; the manufactured sand is diabase manufactured sand, which is made from the same parent rock as the diabase coarse aggregate and is continuously graded by crushing.
[0025] The cementing material includes P O 52.5 Cement, silica fume, microspheres and fly ash are made in a mass ratio of 7:1:1:1, wherein the silica fume has a SiO2 content of ≥90%, and the microspheres are used to improve fluidity and interfacial bonding strength.
[0026] The additive is a polycarboxylate high-performance water-reducing agent with a water reduction rate of 38%.
[0027] like Figure 1 As shown, a method for preparing ultra-high performance concrete using diabase coarse aggregate includes the following steps: S1 Raw Material Pretreatment: The diabase coarse aggregate and mixed sand are dried to a moisture content ≤0.5%; P O 52.5 Cement, silica fume, microspheres, and fly ash are mixed evenly in a mass ratio of 7:1:1:1 to obtain a cementitious material, which is then passed through an 80-mesh sieve to remove impurities; the admixture is mixed with water and stirred evenly to prepare an admixture aqueous solution; S2 segmented mixing: First, add the pretreated diabase coarse aggregate and mixed sand into the mixer and mix at a low speed of 150-200 r / min for 30-60 seconds until uniformly mixed; then add the cementitious material and continue mixing at a low speed of 150-200 r / min for 60-90 seconds to evenly cover the aggregate surface with the cementitious material; finally, slowly add the admixture aqueous solution and mix at a high speed of 300-350 r / min for 120-180 seconds to obtain a uniform, lump-free concrete mixture with good fluidity; S3 Layered Vibration: Pour the concrete mixture into the mold, pour and vibrate in layers, with each layer not exceeding 200mm in thickness and a vibration time of 10-15s; S4 Molding and Curing: After vibration, smooth the surface of the mold and place it in a standard curing room with a temperature of 20±2℃ and a relative humidity of ≥95% for 24-48 hours before demolding. Continue curing for 28 days after demolding, keeping the surface of the specimen moist during the curing period and avoiding direct sunlight and wind.
[0028] Example 1 An ultra-high performance concrete using diabase coarse aggregate and its preparation method, comprising the following raw materials in parts by weight: 250 parts of diabase coarse aggregate, 800 parts of cementitious material, 700 parts of mixed sand, 15 parts of admixture, and 110 parts of water, with a water-cement ratio of 0.14.
[0029] A method for preparing ultra-high performance concrete using diabase coarse aggregate includes the following steps: S1 Raw Material Pretreatment: The diabase coarse aggregate and mixed sand are dried to a moisture content ≤0.5%; P O 52.5 Cement, silica fume, microspheres, and fly ash are mixed evenly in a mass ratio of 7:1:1:1 to obtain a cementitious material, which is then passed through an 80-mesh sieve to remove impurities; the admixture is mixed with water and stirred evenly to prepare an admixture aqueous solution; S2 segmented mixing: First, the pretreated diabase coarse aggregate and mixed sand are put into the mixer and mixed at a low speed of 200 r / min for 45 seconds to mix evenly; then the cementitious material is added and the mixture is continued to be mixed at a low speed of 150 r / min for 70 seconds to make the cementitious material evenly cover the surface of the aggregate; finally, the admixture aqueous solution is slowly added and the mixture is mixed at a high speed of 320 r / min for 150 seconds to obtain a uniform, lump-free concrete mixture with good fluidity. S3 Layered Vibration: Pour the concrete mixture into the mold, pour and vibrate in layers, with each layer not exceeding 200mm in thickness and a vibration time of 15s; S4 Molding and Curing: After vibration, smooth the surface of the mold and place it in a standard curing room with a temperature of 20±2℃ and a relative humidity of ≥95% for 48 hours before demolding. Continue curing for 28 days after demolding, keeping the surface of the specimen moist during the curing period and avoiding direct sunlight and wind.
[0030] Example 2 An ultra-high performance concrete using diabase coarse aggregate and its preparation method, comprising the following raw materials in parts by weight: 300 parts of diabase coarse aggregate, 850 parts of cementitious material, 750 parts of mixed sand, 18 parts of admixture, and 100 parts of water, with a water-cement ratio of 0.12.
[0031] A method for preparing ultra-high performance concrete using diabase coarse aggregate includes the following steps: S1 Raw Material Pretreatment: The diabase coarse aggregate and mixed sand are dried to a moisture content ≤0.5%; P O 52.5 Cement, silica fume, microspheres, and fly ash are mixed evenly in a mass ratio of 7:1:1:1 to obtain a cementitious material, which is then passed through an 80-mesh sieve to remove impurities; the admixture is mixed with water and stirred evenly to prepare an admixture aqueous solution; S2 segmented mixing: First, add the pretreated diabase coarse aggregate and mixed sand into the mixer and mix at a low speed of 180 r / min for 30 seconds to mix evenly; then add the cementitious material and continue mixing at a low speed of 200 r / min for 60 seconds to evenly cover the surface of the aggregate with the cementitious material; finally, slowly add the admixture aqueous solution and mix at a high speed of 300 r / min for 120 seconds to obtain a uniform, lump-free, and highly fluid concrete mixture. S3 Layered Vibration: Pour the concrete mixture into the mold, pour and vibrate in layers, with each layer not exceeding 200mm in thickness and a vibration time of 12s; S4 Molding and Curing: After vibration, smooth the surface of the mold and place it in a standard curing room with a temperature of 20±2℃ and a relative humidity of ≥95% for 24 hours before demolding. Continue curing for 28 days after demolding. During the curing period, keep the surface of the specimen moist and avoid direct sunlight and wind.
[0032] Example 3 An ultra-high performance concrete using diabase coarse aggregate and its preparation method, comprising the following raw materials in parts by weight: 200 parts of diabase coarse aggregate, 700 parts of cementitious material, 600 parts of mixed sand, 12 parts of admixture, and 120 parts of water, with a water-cement ratio of 0.17.
[0033] A method for preparing ultra-high performance concrete using diabase coarse aggregate includes the following steps: S1 Raw Material Pretreatment: The diabase coarse aggregate and mixed sand are dried to a moisture content ≤0.5%; P O 52.5 Cement, silica fume, microspheres, and fly ash are mixed evenly in a mass ratio of 7:1:1:1 to obtain a cementitious material, which is then passed through an 80-mesh sieve to remove impurities; the admixture is mixed with water and stirred evenly to prepare an admixture aqueous solution; S2 segmented mixing: First, the pretreated diabase coarse aggregate and mixed sand are put into the mixer and mixed at a low speed of 150 r / min for 60 s to mix evenly; then the cementitious material is added and the mixture is continued to be mixed at a low speed of 180 r / min for 90 s to make the cementitious material evenly cover the surface of the aggregate; finally, the admixture aqueous solution is slowly added and the mixture is mixed at a high speed of 350 r / min for 180 s to obtain a uniform, lump-free concrete mixture with good fluidity. S3 Layered Vibration: Pour the concrete mixture into the mold, pour and vibrate in layers, with each layer not exceeding 200mm in thickness and a vibration time of 10s; S4 Molding and Curing: After vibration, smooth the surface of the mold and place it in a standard curing room with a temperature of 20±2℃ and a relative humidity of ≥95% for 36 hours before demolding. Continue curing for 28 days after demolding. During the curing period, keep the surface of the specimen moist and avoid direct sunlight and wind.
[0034] Comparative Example 1 The method is basically the same as in Example 1, except that the coarse aggregate of diabase is replaced with an equal amount of coarse aggregate of basalt.
[0035] Performance testing The ultra-high performance concrete prepared in Examples 1-3 and Comparative Example 1 was tested for 28-day compressive strength and 28-day flexural strength according to GB / T 50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete". The frost resistance was tested according to the rapid freezing method according to GB / T 50082-2024 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete". The impermeability was tested using the stepwise pressure method. The results are shown in Table 1.
[0036] Table 1 Performance Test Results As shown in Table 1, in terms of mechanical properties, the 28-day compressive strength of Example 1 was 126 MPa and the flexural strength was 16.8 MPa; the 28-day compressive strength of Example 2 was 132 MPa and the flexural strength was 17.3 MPa; and the 28-day compressive strength of Example 3 was 123 MPa and the flexural strength was 16.4 MPa. Among the three examples, Example 2 exhibited the best mechanical properties, with its compressive and flexural strengths increasing by 6.5% and 9.5% respectively compared to Comparative Example 1's 124 MPa and 15.8 MPa. The compressive and flexural strengths of Example 1 increased by 1.6% and 6.3% respectively compared to Comparative Example 1; and the flexural strength of Example 3 increased by 3.8% compared to Comparative Example 1. These results indicate that the synergistic effect of diabase coarse aggregate and the cement-silica fume-microsphere ternary cementitious system can significantly improve the mechanical properties of ultra-high performance concrete.
[0037] Regarding durability, Example 1 had a frost resistance rating of F350 and a permeability resistance rating > P12, Example 2 had a frost resistance rating of F400 and a permeability resistance rating > P12, and Example 3 had a frost resistance rating of F350 and a permeability resistance rating > P12. The frost resistance and permeability resistance of the three examples were higher than those of Comparative Example 1. This indicates that the extremely low water absorption of diabase, combined with the low water-cement ratio design, can significantly improve the freeze-thaw resistance of ultra-high performance concrete and enhance its permeability resistance.
[0038] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A type of ultra-high performance concrete using diabase coarse aggregate, characterized in that, The raw materials include the following parts by weight: 200-300 parts of diabase coarse aggregate, 700-850 parts of cementitious material, 600-750 parts of mixed sand, 12-18 parts of admixture, and 100-120 parts of water.
2. The ultra-high performance concrete using diabase coarse aggregate according to claim 1, characterized in that: The coarse aggregate of the diabase has a particle size of 5-8 mm.
3. The ultra-high performance concrete using diabase coarse aggregate according to claim 1, characterized in that: The particle size of the mixed sand is 0.15-5 mm.
4. The ultra-high performance concrete using diabase coarse aggregate according to claim 1, characterized in that: The cementing material includes P O 52.5 Cement, silica fume, microspheres, fly ash.
5. The ultra-high performance concrete using diabase coarse aggregate according to claim 4, characterized in that: The cementitious material is made of P O 52.5 is made of cement, silica fume, microspheres and fly ash in a mass ratio of 7:1:1:
1.
6. The ultra-high performance concrete using diabase coarse aggregate according to claim 1, characterized in that: The additive is a polycarboxylate high-performance water-reducing agent.
7. The ultra-high performance concrete using diabase coarse aggregate according to claim 1, characterized in that: The water-to-binder ratio is less than 0.
19.
8. The method for preparing ultra-high performance concrete using diabase coarse aggregate according to any one of claims 1-7, characterized in that, Includes the following steps: S1 Raw Material Pretreatment: Dry the diabase coarse aggregate and mixed sand to a moisture content of ≤0.5%; remove impurities from the cementitious material by passing it through an 80-mesh sieve; mix the admixture with water and stir evenly to prepare an admixture aqueous solution; S2 segmented mixing: First, put the pretreated diabase coarse aggregate and mixed sand into the mixer and mix at low speed for 30-60 seconds until they are evenly mixed; then add the cementitious material and continue to mix at low speed for 60-90 seconds; finally, slowly add the admixture aqueous solution and mix at high speed for 120-180 seconds to obtain the concrete mixture. S3 Layered Vibration: Pour the concrete mixture into the mold, pour it in layers and vibrate it, with a vibration time of 10-15 seconds; S4 molding and curing: After vibration, smooth the surface of the mold and place it in the curing room for 24-48 hours before demolding; continue curing for 28 days after demolding to obtain the final product.
9. The method for preparing ultra-high performance concrete using diabase coarse aggregate according to claim 8, characterized in that: In S2, the low-speed stirring speed is 150-200 r / min, and the high-speed stirring speed is 300-350 r / min.