A diatomaceous earth sound-absorbing decorative panel and its preparation method

By introducing silica sol and polyvinyl alcohol into gypsum-based materials, combined with soluble salting-out agents and foam stabilizers, a closed-cell-micro-perforated structure is formed, which solves the contradiction between pore structure and mechanical strength in gypsum sound-absorbing boards, achieving a balance of lightweight, high strength, and excellent sound absorption and insulation performance, making it suitable for building decorative panels.

CN123106151APending Publication Date: 2026-11-17山东凯大新型材料科技有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611207739.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing gypsum sound-absorbing boards cannot simultaneously achieve uniformity in pore structure and synergistic effect of closed pores and micro-perforations. The trade-off between mechanical strength and acoustic performance has not been effectively resolved. Pore stability and pore wall thickness distribution are difficult to control, resulting in the material being prone to brittleness or unstable sound absorption and insulation effects in engineering applications.

Method used

Using raw materials such as α-hemihydrate gypsum, diatomaceous earth, silica sol, polyvinyl alcohol, alkyl polysaccharide glycoside, hydrolyzed gelatin, citric acid, and ammonium bicarbonate, a uniform closed-cell-microperforated composite structure is formed by precisely controlling the foaming-coagulation-curing process. The density of the pore walls is enhanced by the filling and cross-linking effect of nanoparticles, and secondary microperforated channels are formed by combining soluble salting-out agents. Foam stabilizers and coagulation control agents are used to ensure the stability and uniformity of the pore structure.

Benefits of technology

It achieves lightweight and high porosity while maintaining excellent flexural strength and sound absorption and insulation effects. Its acoustic performance is stable in different frequency bands, thus balancing the material's structural stability and acoustic performance, meeting the needs of the construction industry for high-performance functional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106151A_ABST
    Figure CN123106151A_ABST
Patent Text Reader

Abstract

This invention discloses a diatomaceous earth sound-absorbing decorative panel and its preparation method, relating to the field of building materials technology. The decorative panel is composed of α-hemihydrate gypsum, diatomaceous earth, silica sol, polyvinyl alcohol, alkyl polysaccharide glycosides, hydrolyzed gelatin, citric acid, ammonium bicarbonate, and sodium chloride crystals. Combined with lactic acid-triggered foaming and salting-out steps, a uniform porous structure is formed, which is then cured and dried to obtain the finished product. The preparation method includes raw material mixing, slurry preparation, foaming and molding, curing and drying, and dissolution steps. Silica sol and polyvinyl alcohol synergistically strengthen the pore walls, maintaining strength despite high porosity; sodium chloride dissolves to form micro-perforated channels between closed pore walls, constructing a "closed-pore-micro-perforated" composite structure that balances lightweight, sound absorption, and sound insulation; alkyl polysaccharide glycosides and hydrolyzed gelatin stabilize the foam, and citric acid controls coagulation, ensuring uniform pore distribution and preventing collapse, ultimately achieving lightweight, high strength, and excellent acoustic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building materials technology, and in particular to a diatomaceous earth sound-absorbing decorative panel and its preparation method. Background Technology

[0002] With the increasing demands for quality in modern buildings and indoor environments, sound-absorbing and sound-insulating functional materials have gradually become a hot topic in research and engineering applications. Porous structural materials are widely used in walls, ceilings, and decorative panels due to their excellent sound energy dissipation capabilities. Among them, gypsum-based sound-absorbing boards are widely used due to their advantages such as light weight, fire resistance, moderate cost, and ease of molding, and have gradually developed into various types, including composite porous materials, modified gypsum boards, and functional filler materials. In recent years, to further improve the coordination between acoustic and mechanical properties, researchers have attempted to introduce porous mineral fillers, colloidal reinforcing materials, or multiphase composite processes into gypsum-based systems to improve the uniformity and stability of the pore structure. However, existing gypsum sound-absorbing boards still suffer from problems such as high structural brittleness, irregular pores, and unstable sound absorption and insulation effects, making it difficult to meet the comprehensive requirements for lightweight, high-strength, and high-efficiency acoustic performance.

[0003] However, existing technologies still have significant shortcomings. First, it is often difficult to achieve both uniformity in pore structure and synergistic effects between closed pores and micro-perforations. For example, in patent CN104379849B, the "gypsum board for sound-absorbing ceiling" uses a large number of perforations, but the holes are through-hole open structures. Although it can obtain a high NRC value in the mid-to-high frequency range, the sound transmission of the open holes is too strong, resulting in poor sound insulation performance and low-frequency sound absorption. The insufficient strength of the hole walls and the closed pore portion cause sound waves to easily leak from the holes, reducing the overall sound transmission loss. Second, the trade-off between mechanical strength and acoustic performance has not been effectively resolved. Taking patent CN101563220A as an example, this patent discloses "low-dust gypsum wall panel with high void volume". Its void volume is extremely high (about 80-92%), which can greatly improve the sound absorption effect and reduce the weight of the panel. However, the corresponding mechanical flexural or compressive strength often cannot meet the requirements of engineering applications, and it is prone to brittleness or breakage during processing / assembly. Third, the influence of foam stability, pore wall thickness distribution, and coagulation / curing conditions on pore closure or perforation structure formation is not systematically controlled in existing technologies. In existing literature, most sound-absorbing panels exhibit unstable foam cells, excessive interconnected pores, and a broad pore size distribution during the foaming process. Simultaneously, during curing or drying, pore wall shrinkage or collapse often leads to the destruction of closed-cell structures, thereby reducing mechanical properties and sound insulation performance. While literature CN110698160A attempts to improve strength by adjusting porosity through filler, it does not simultaneously achieve a good balance between high porosity and high sound insulation performance; its structure does not form a closed-cell + micro-perforated combined structure, and low-frequency sound insulation remains insufficient.

[0004] Based on the above situation, there is an urgent need in this field for a decorative panel that can simultaneously achieve lightweight, high porosity, good mechanical properties, and excellent sound absorption and insulation effects. Specifically, the following core issues need to be addressed: First, how to achieve controllability of the pore structure throughout the foaming-condensation-curing process, enabling the material to form a uniform closed-cell-micro-perforated composite system; second, how to maintain high porosity while avoiding a decrease in mechanical strength, ensuring sufficient flexural strength for engineering applications; and third, how to ensure stable acoustic performance across different frequency bands, avoiding the problem of large frequency fluctuations in the sound absorption and insulation effects of existing materials. Only by overcoming these bottlenecks can a new type of sound-absorbing and sound-insulating decorative panel with both structural stability and excellent acoustic performance be developed to meet the urgent demand for high-performance functional materials in the construction industry. Summary of the Invention

[0005] To achieve the above-mentioned objectives and address the aforementioned technical problems, the present invention provides a diatomaceous earth sound-absorbing decorative panel, wherein the decorative panel is composed of raw materials within the following weight range: The composition includes 70-90 parts α-hemihydrate gypsum, 5-25 parts diatomaceous earth, 1-10 parts silica sol, 0.5-5 parts polyvinyl alcohol, 0.1-1.0 parts alkyl polysaccharide, 0.05-0.5 parts hydrolyzed gelatin, 0.05-0.5 parts citric acid, 0.5-3 parts ammonium bicarbonate, 1-5 parts sodium chloride crystals, and the remainder being deionized water. The polyvinyl alcohol and hydrolyzed gelatin are measured on a solids basis.

[0006] Preferably, the sodium chloride crystals have a particle size of 80–120 μm.

[0007] Preferably, the diatomaceous earth is calcined and purified diatomaceous earth with a particle size of 400 mesh and a SiO2 content greater than 85%.

[0008] Preferably, the polyvinyl alcohol is polyvinyl alcohol with a degree of hydrolysis of 88%, which is added after being prepared into a 5wt% aqueous solution.

[0009] Preferably, the hydrolyzed gelatin is prepared as a 40wt% solution and added.

[0010] Preferably, the silica sol is an aqueous sol with a SiO2 solid content of 20–40 wt% and a SiO2 particle size of 10–30 nm.

[0011] The present invention also provides a method for preparing the diatomaceous earth sound-absorbing decorative panel according to the above, comprising the following steps: (1) Mix α-hemihydrate gypsum, diatomaceous earth and sodium chloride crystals; (2) Deionized water, silica sol and polyvinyl alcohol solution were added to the mixture in sequence to obtain the basic slurry; (3) Add alkyl polysaccharide, hydrolyzed gelatin solution and citric acid to the base slurry, and further add ammonium bicarbonate to obtain foamed slurry; (4) Pour the foamed slurry into the mold, spray in the lactic acid aqueous solution to trigger foaming, and obtain the slab after initial setting and final setting; (5) After demolding the slab, cure and dry it to obtain the board material; (6) The board is soaked in deionized water to dissolve sodium chloride, and then dried with hot air to obtain the diatomaceous earth sound-absorbing decorative board.

[0012] Preferably, the amount of deionized water added in step (2) is 0.4 to 0.6 times the total mass of the α-hemihydrate gypsum, diatomaceous earth, and SiO2 solids in the silica sol. Preferably, in step (4), the concentration of the lactic acid aqueous solution is 6-10 wt%, and the spray volume is 1.0-1.5 wt% of the total mass of the foamed slurry.

[0013] Preferably, the initial setting time in step (4) is 2 to 5 minutes, and the final setting time is 6 to 12 minutes.

[0014] Preferably, the curing conditions in step (5) are 40-50℃, relative humidity 50-60%, and time 12-36h; Preferably, in step (6), the sodium chloride dissolution conditions are soaking in deionized water at 20-30°C for 5-10 minutes, followed by hot air drying at 60-80°C for 4-6 hours.

[0015] The beneficial effects of the technical solution provided by this invention are as follows: This invention achieves effective control over the setting rate and framework strength of the slurry by introducing silica sol and polyvinyl alcohol into a gypsum-diatomaceous earth system. The nanoparticles of the silica sol fill and cross-link between gypsum crystals, enhancing pore wall density and structural stability; while polyvinyl alcohol plays a role in flexibility enhancement and film formation during slurry hardening. The resulting material maintains excellent flexural strength even under high porosity conditions, avoiding the strength deficiency problem found in traditional foamed gypsum.

[0016] This invention uses sodium chloride crystals as a soluble salting-out agent. After post-treatment and dissolution, secondary micro-perforated channels are formed between the closed-pore walls, thus constructing a "closed-pore-micro-perforated" composite structure. This structure ensures both lightweight overall surface density and provides channels for sound energy dissipation. Sound waves undergo multiple reflections and frictional losses within the pores, significantly improving the sound absorption coefficient. Simultaneously, the uniform closed-pore wall layer acts as a barrier to sound wave transmission, thereby achieving high transmission loss.

[0017] This invention utilizes the synergistic foam-stabilizing effect of alkyl polysaccharide glycosides and hydrolyzed gelatin, combined with the retarding and regulating effect of citric acid, to maintain a uniform distribution of bubble nuclei throughout the entire process of acid triggering, gas release, and coagulation hardening, thus preventing pore connectivity and bubble wall rupture. The result is a significantly increased and uniformly distributed porosity, ensuring a balance between acoustic and mechanical properties. In contrast, when foam stabilizers, coagulation regulators, or salting-out agents are lacking, pore wall collapse, excessive interconnected pores, or uneven pore size distribution often occur, leading to decreased flexural strength and significant deterioration of both sound absorption and sound insulation performance.

[0018] Under optimized conditions, the samples exhibit a regular polyhedral closed-pore morphology with smooth, uniform pore walls and a small number of micro-perforations, which facilitates the formation of a dual mechanism of "sound energy dissipation + sound insulation barrier." Samples deviating from these key conditions generally show defects such as rough pore walls, collapse, or excessive interconnected pores. This demonstrates that the formulation and process of this invention, through precise control of the pore structure, achieves a unified effect of lightweight, high strength, and excellent sound absorption and insulation performance—effects that are difficult to achieve simultaneously with existing technologies. Attached Figure Description

[0019] Figure 1 This is a process flow diagram of the present invention. Figure 2 This is a SEM image of Embodiment 1 of the present invention; Figure 3 This is a SEM image of Comparative Example 2 of the present invention; Figure 4 This is a SEM image of Comparative Example 3 of the present invention; Figure 5 This is a SEM image of Comparative Example 4 of the present invention; Figure 6 This is a SEM image of Comparative Example 6 of the present invention; Figure 7 This is a SEM image of Comparative Example 7 of the present invention; Figure 8 The present invention includes a sound absorption testing system and a physical diagram. Figure 9 This is a picture of the sound insulation testing system and physical object of the present invention. Detailed Implementation

[0020] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. Of course, the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0021] Example 1 I. Finished Products Finished product dimensions: 300mm×300mm×25mm Mold: Rigid flat mold (300×300×25mm), with an inner wall covered with 0.1mm PET release film. II. Formula (parts by weight) α-Hemihydrate gypsum: 85 parts Calcined and purified diatomaceous earth (400 mesh, SiO2>85%): 18 parts Silica sol (aqueous sol, SiO2 solid content 30wt%, particle size 20nm): 7 parts Polyvinyl alcohol (PVA, 88% hydrolyzed, on a solids basis): 1.2 parts Alkyl polysaccharide APG0810: 0.30 parts Hydrolyzed gelatin (on a solids basis; added to prepare a 40 wt% solution): 0.08 parts Citric acid: 0.08 parts Ammonium bicarbonate: 0.75 parts Sodium chloride crystals (particle size 80–120 μm): 3.0 parts Deionized water: Added at a ratio of water / cementing material = 0.50. Cementing material = α-hemihydrate gypsum (solid) + diatomaceous earth (solid) + SiO2 solid in silica sol Triggering fluid (added via spray) Lactic acid aqueous solution: 8wt% Spray volume: 1.2 wt% of the total mass of the foamed slurry. III. Equipment Planetary mixer (0–1000 rpm), atomizing spray gun (nozzle 0.8 mm, liquid supply 0.10–0.15 g / s, air pressure 0.20 MPa), constant temperature and humidity chamber, hot air drying oven, timer, rheometer, mesh screen, ultrapure water system.

[0022] IV. Process Steps S0 Raw material pretreatment Sift diatomaceous earth through a 400-mesh sieve (65μm), bake at 110℃ for 2 hours, cool and seal; dry and store ammonium bicarbonate; dry NaCl particles with a diameter of 80–120μm; mix silica sol, PVA, and hydrolyzed gelatin; cover the mold with 0.1mm PET and store at 23℃ for later use.

[0023] S1 Slurry Preparation α-Hemihydrate gypsum, diatomaceous earth, and NaCl were dry-mixed at 300 rpm for 3 minutes, and the mixture was scraped against the wall once. Add the following ingredients sequentially at 300 rpm: deionized water, silica sol, and PVA; then increase the rpm to 800 rpm and mix for 1 minute. Add APG0810, hydrolyzed gelatin, and citric acid in sequence; mix at 800 rpm for 1 minute. S2 In-situ foaming + simultaneous coagulation and shaping After the slurry is poured into the mold, it is gently stirred at 600 rpm for 20 seconds to remove large air bubbles and form fine bubble nuclei; The lactic acid solution is evenly sprayed into the atomizing spray gun within 15 seconds; at the same time, it is stirred at a low speed of 300 rpm for 10 seconds to ensure even distribution.

[0024] Static foaming: After standing at normal pressure for 45 seconds, CO2 continues to be generated, and the foam cells tend to form polyhedra due to mutual compression.

[0025] Condensation lock-in: Starting from the self-spraying acid, initial condensation takes 3 minutes and final condensation takes 8 minutes; during this period, there is no disturbance or vacuuming, and the pressure is normal.

[0026] S3 Maintenance and Drying After demolding, the product is cured in a constant temperature and humidity chamber at 45℃ / 55%RH for 24 hours; then dried with hot air at 65℃ for 6 hours until constant weight is achieved; and left to stand at room temperature for ≥30 minutes.

[0027] S4 Soluble Particle Removal The board was soaked in deionized water at 25°C for 8 minutes to dissolve sodium chloride; then dried with hot air at 65°C for 4 hours to constant weight.

[0028] Example 2 Prepared using the same method as in Example 1, except that the amount of α-hemihydrate gypsum used was 70 parts.

[0029] Example 3 Prepared using the same method as in Example 1, except that the amount of diatomaceous earth used is 5 parts.

[0030] Example 4 Prepared using the same method as in Example 1, except that the amount of silica sol used was 1 part (SiO2 solid content 20wt%, particle size 10nm).

[0031] Example 5 Prepared using the same method as in Example 1, except that the amount of silica sol used was 10 parts (SiO2 solid content 40wt%, particle size 30nm).

[0032] Example 6 Prepared using the same method as in Example 1, except that the amount of alkyl polysaccharide APG0810 used was 1.0 part.

[0033] Example 7 Prepared using the same method as in Example 1, except that the amount of hydrolyzed gelatin used was 0.5 parts (added after preparing a 40wt% solution).

[0034] Example 8 Prepared using the same method as in Example 1, except that the amount of citric acid used is 0.5 parts.

[0035] Example 9 Prepared using the same method as in Example 1, except that the amount of sodium chloride crystals used was 5 parts (particle size maintained at 80–120 μm).

[0036] Example 10 Prepared using the same method as in Example 1, except that the curing conditions were 40°C, 50% relative humidity, and 12 hours.

[0037] Example 11 Prepared using the same method as in Example 1, except that the curing conditions were 50°C, 60% relative humidity, and 36 hours.

[0038] Example 12 Prepared using the same method as in Example 1, except that the concentration of the lactic acid aqueous solution is 6 wt% and the spray volume is 1.0 wt% of the total mass of the foamed slurry.

[0039] Comparative Example 1 Prepared using the same method as in Example 1, except that no diatomaceous earth was added.

[0040] Comparative Example 2 Prepared using the same method as in Example 1, except that alkyl polysaccharide APG0810 was not added.

[0041] Comparative Example 3 Prepared using the same method as in Example 1, except that sodium chloride crystals were not added.

[0042] Comparative Example 4 Prepared using the same method as in Example 1, except that the concentration of the sprayed lactic acid aqueous solution was 12 wt%.

[0043] Comparative Example 5 Prepared using the same method as in Example 1, except that the amount of lactic acid aqueous solution sprayed is 0.5 wt% of the total mass of the foamed slurry.

[0044] Comparative Example 6 Prepared using the same method as in Example 1, except that citric acid was not added.

[0045] Comparative Example 7 Prepared using the same method as in Example 1, except that the curing conditions were room temperature 25°C and natural drying.

[0046] Comparative Example 8 Prepared using the same method as in Example 1, except that the soaking time in the sodium chloride dissolution step is 2 minutes.

[0047] Experimental test: 1. Areal density areal density (kg / m³) 2 = Dry mass / area Sample size: 300×300 mm, dried to constant weight, weighed directly.

[0048] 2. Porosity The porosity of the diatomaceous earth sound-absorbing decorative panel of the present invention is determined by the water saturation method. Specifically, the sample is dried and weighed, then immersed in deionized water until saturated, and the saturated weight is weighed. The porosity is calculated as follows: P=(W) 饱和 -W 干燥 )×100% / ρ 水 V Among them, W 饱和 W is the saturated mass of the sample. 干燥 ρ is the dry mass of the sample, V is the geometric volume of the sample, and ρwater is the density of water.

[0049] 3. Flexural strength Standard: GB / T 9775 (Gypsum Board) Three-point bending method; report span, loading rate and minimum failure load.

[0050] 4. Sound absorption performance test The sound absorption performance was tested using the multi-microphone impedance tube method, in accordance with GB / T 18696.2-2002 "Measurement of Acoustic Properties of Acoustic Absorbing Materials - Part 2: Transfer Function Method". The test frequency range was 125 Hz to 6300 Hz. 5. Sound insulation performance test The sound insulation performance was tested using a transfer function method impedance tube system, in accordance with GB / T 19889.7-2005 "Acoustics of Buildings and Building Components - Sound Insulation Measurement Part 7: Laboratory Measurement of Sound Absorption by Impedance Tube Method". The test frequency range was 125 Hz to 6300 Hz.

[0051] Table 1 Test Data

[0052] Overall, the results of the tested samples show that the samples with complete formulation and process window achieve a mutually supportive balance between pore structure, mechanical and acoustic properties: the high and uniform porosity combined with the dense and flat pore walls enables the material to achieve greater viscous dissipation and multiple resonances while maintaining a lightweight surface density, thus benefiting from both sound absorption coefficient and sound transmission loss; at the same time, the "filling-bridging-toughening" effect of nano-silica and film-forming polymers on the pore walls offsets the strength attenuation common in high porosity, so the flexural strength does not decrease significantly with the increase of pores. In contrast, samples lacking key processes or deviating from the process window (such as unstabilized bubbles, uncontrolled coagulation, insufficient salting out, or excessively strong acid triggering) generally exhibit large and uneven pores, increased interconnected pores, or wrinkled and collapsed pore walls. This results in insufficient low-frequency resonance and reduced internal friction paths acoustically, weakening the sound barrier effect. Mechanically, it leads to poorer interfacial bonding and skeleton continuity, resulting in lower strength. When the salting-out agent is missing or insufficiently dissolved, the closed pore walls cannot form effective secondary micro-necks, disrupting the micro-perforation-cavity synergy, lowering the peak value of the sound absorption curve, and narrowing the bandwidth. Process conditions also have a consistent impact: insufficient curing or secondary shrinkage caused by natural drying causes wrinkling and local cracking of the pore walls; excessive acid triggering leads to excessively rapid instantaneous foaming, uncontrolled pore size distribution, and insufficient skeleton rearrangement, all of which manifest as a double decline in acoustics and mechanics.

[0053] The microstructure of the typical embodiments and comparative samples was observed by scanning electron microscopy (SEM). The results showed that the pore structure of the sample obtained in Example 1 was a regular polyhedral closed-pore morphology with smooth and uniform pore walls. Micro-perforated channels were visible on some pore walls, forming a "closed-pore-micro-perforated" composite structure. This structure is closely related to the synergistic effect of the foam stabilizer, the coagulation control of citric acid, and the salting-out agent used in this invention, ensuring excellent mechanical properties and sound absorption and insulation performance. In contrast, the comparative samples all showed obvious defects: the pore walls in Comparative Example 2 (without foam stabilizer) were rough and the interpores were severely interconnected; the pores in Comparative Example 3 (without salting-out agent) were sparse and lacked micro-perforated necks; the pore size in Comparative Example 4 (excessively high acid concentration) varied significantly, and the pore walls were excessively thick in some areas; the pore walls in Comparative Example 6 (without citric acid coagulation control) were cracked and the number of irregular openings increased; and the pore walls in Comparative Example 7 (naturally dried at room temperature) were wrinkled and collapsed. The above comparison results clearly demonstrate that by introducing alkyl polysaccharide foam stabilizers, citric acid coagulants, and sodium chloride salting-out particles into the system, and under suitable acid triggering and curing conditions, the present invention can significantly improve the morphology control of foaming pores, enabling the material to obtain a uniform closed-cell-micro-perforated structure, thereby achieving excellent comprehensive sound absorption and sound insulation performance.

[0054] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A diatomaceous earth sound-absorbing decorative panel, characterized in that, The decorative panel is composed of raw materials within the following weight range: The composition includes 70-90 parts α-hemihydrate gypsum, 5-25 parts diatomaceous earth, 1-10 parts silica sol, 0.5-5 parts polyvinyl alcohol, 0.1-1.0 parts alkyl polysaccharide, 0.05-0.5 parts hydrolyzed gelatin, 0.05-0.5 parts citric acid, 0.5-3 parts ammonium bicarbonate, 1-5 parts sodium chloride crystals, and the remainder being deionized water. The polyvinyl alcohol and hydrolyzed gelatin are measured on a solids basis.

2. The diatomaceous earth sound-absorbing decorative panel according to claim 1, characterized in that, The sodium chloride crystals have a particle size of 80–120 μm.

3. The diatomaceous earth sound-absorbing decorative panel according to claim 1, characterized in that, The diatomaceous earth is calcined and purified diatomaceous earth with a particle size of 400 mesh and a SiO2 content greater than 85%.

4. The diatomaceous earth sound-absorbing decorative panel according to claim 1, characterized in that, The polyvinyl alcohol is polyvinyl alcohol with a degree of hydrolysis of 88%, which is added after being prepared into a 5wt% aqueous solution.

5. The diatomaceous earth sound-absorbing decorative panel according to claim 1, characterized in that, The hydrolyzed gelatin was prepared as a 40 wt% solution and added.

6. The diatomaceous earth sound-absorbing decorative panel according to claim 1, characterized in that, The silica sol is an aqueous sol with a SiO2 solid content of 20–40 wt% and a SiO2 particle size of 10–30 nm.

7. A method for preparing a diatomaceous earth sound-absorbing decorative panel according to any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Mix α-hemihydrate gypsum, diatomaceous earth and sodium chloride crystals; (2) Deionized water, silica sol and polyvinyl alcohol solution were added to the mixture in sequence to obtain the basic slurry; (3) Add alkyl polysaccharide, hydrolyzed gelatin solution and citric acid to the base slurry, and further add ammonium bicarbonate to obtain foamed slurry; (4) Pour the foamed slurry into the mold, spray in the lactic acid aqueous solution to trigger foaming, and obtain the slab after initial setting and final setting; (5) After demolding the slab, cure and dry it to obtain the board material; (6) The board is soaked in deionized water to dissolve sodium chloride, and then dried with hot air to obtain the diatomaceous earth sound-absorbing decorative board.

8. The preparation method according to claim 7, characterized in that, The amount of deionized water added in step (2) is 0.4 to 0.6 times the total mass of α-hemihydrate gypsum, diatomaceous earth and SiO2 solid in silica sol. The concentration of lactic acid aqueous solution in step (4) is 6 to 10 wt%, and the spray volume is 1.0 to 1.5 wt% of the total mass of foamed slurry.

9. The preparation method according to claim 8, characterized in that, The initial setting time in step (4) is 2 to 5 minutes, and the final setting time is 6 to 12 minutes.

10. The preparation method according to claim 9, characterized in that, The curing conditions described in step (5) are 40-50℃, relative humidity 50-60%, and time 12-36h; the sodium chloride dissolution conditions in step (6) are soaking in deionized water at 20-30℃ for 5-10min, followed by hot air drying at 60-80℃ for 4-6h.

Citation Information

Patent Citations

  • Low dust gypsum wallboard

    CN101563220A

  • Gypsum panels for acoustic monolithic ceilings

    CN104379849B

  • Gypsum board slurry and preparation method thereof

    CN110698160A