Silicon nanowire / carbon nanotube / polydimethylsiloxane composite materials, their preparation methods and applications
By constructing a silicon nanowire-carbon nanotube hybrid conductive network in polydimethylsiloxane, the problem of silicon nanowires being difficult to form a continuous conductive path is solved, and a continuous negative temperature coefficient response of flexible temperature sensing material is achieved, which is suitable for the fabrication of flexible temperature sensors.
Patent Information
- Application Number
- CN202611310829.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
In existing polydimethylsiloxane thermosensitive composite materials, the spaced silicon nanowires are difficult to form a continuous conductive path, which makes it difficult to stably output temperature and piezoresistive responses and obtain the preset temperature response law.
By distributing n-type silicon nanowires at intervals in polydimethylsiloxane and placing some carbon nanotubes in between, a silicon nanowire-carbon nanotube hybrid conductive network is formed. The material composition ratio can be controlled to achieve the construction of a continuous conductive network.
It achieves a continuous negative temperature coefficient response of flexible temperature sensing materials within a preset temperature range, balancing the continuity of the conductive network with temperature response sensitivity, and is suitable for the fabrication of flexible temperature sensors.
Smart Images

Figure CN123107364A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of flexible temperature sensing materials technology, specifically to silicon nanowire / carbon nanotube / polydimethylsiloxane composite materials, their preparation methods, and applications. Background Technology
[0002] With the development of wearable devices, flexible electronic devices, and human health monitoring technologies, temperature sensors, in addition to needing temperature response capabilities, also require flexibility, conformability, and fast response speeds. Polydimethylsiloxane (PDMS), with its flexibility, elasticity, and processability, is often used as the polymer matrix for flexible temperature-sensitive composite materials. By adding conductive fillers such as carbon nanotubes to PDMS, a conductive network can be constructed, and temperature detection can be achieved by utilizing changes in the conductive network caused by temperature.
[0003] However, the thermal expansion of polydimethylsiloxane alters the contact area, number of contacts, and spacing between carbon nanotubes, easily causing the resistance of the carbon nanotube conductive network to increase with temperature, exhibiting a positive temperature coefficient response. Because the contact state between carbon nanotubes changes non-uniformly during heating, the resulting composite material may also exhibit non-linear temperature response or inconsistent response patterns across different temperature ranges. While increasing the carbon nanotube content can improve the continuity of the conductive network, excessive carbon nanotubes tend to form relatively independent and dense conductive pathways, reducing the network's sensitivity to temperature and thermal deformation of the matrix.
[0004] Silicon nanowires possess semiconductor temperature response and piezoresistive properties, which can be used to convert temperature and thermal strain changes into resistance changes. However, when silicon nanowires are dispersed in polydimethylsiloxane at low concentrations, the different silicon nanowires are usually spaced apart, making it difficult for them to form a continuous conductive path. This makes it difficult for the resistance changes generated by the silicon nanowires to be stably detected by external electrodes. Increasing the silicon nanowire content to improve the conductivity probability may cause the silicon nanowires to agglomerate and entangle, affecting the flexibility of the composite material. Therefore, how to connect the spaced-apart silicon nanowires into a continuous conductive network and coordinate the relationship between the continuity of the conductive network and the temperature response sensitivity to obtain a flexible temperature-sensitive composite material with a predetermined temperature response law remains a technical problem that needs to be solved. Summary of the Invention
[0005] One objective of the first aspect of this invention is to provide a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material, which solves the technical problem in the prior art that the spaced silicon nanowires in the polydimethylsiloxane thermosensitive composite material are difficult to form a continuous conductive path, resulting in the silicon nanowires' temperature and piezoresistive response being difficult to output stably and obtain a preset temperature response law.
[0006] Another objective of the first aspect of the present invention is to balance the specific surface area, strain response capability, structural integrity and dispersibility of n-type silicon nanowires in polydimethylsiloxane, so that carbon nanotubes can form more interfacial contacts with n-type silicon nanowires and form conductive bridges between the spaced-apart n-type silicon nanowires.
[0007] The second aspect of this invention aims to provide a method for preparing the above-mentioned silicon nanowire / carbon nanotube / polydimethylsiloxane composite material.
[0008] The third aspect of this invention aims to provide a flexible temperature sensor.
[0009] According to a first aspect of the present invention, the present invention provides a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material for temperature sensing, comprising a polydimethylsiloxane body and n-type silicon nanowires and carbon nanotubes dispersed in the polydimethylsiloxane body; The n-type silicon nanowires are spaced apart from each other, and at least some of the carbon nanotubes are located between the spaced-apart n-type silicon nanowires and are in contact with at least two n-type silicon nanowires, so that the multiple n-type silicon nanowires are electrically connected through the carbon nanotubes to form a silicon nanowire-carbon nanotube hybrid conductive network; wherein, The polydimethylsiloxane body is formed by curing a polydimethylsiloxane prepolymer, which includes a polydimethylsiloxane adhesive and a curing agent. The total mass of the polydimethylsiloxane prepolymer is the sum of the masses of the polydimethylsiloxane adhesive and the curing agent. The mass ratio of the n-type silicon nanowires to the total mass of the polydimethylsiloxane prepolymer is (1.0-1.5):100, the mass ratio of the carbon nanotubes to the total mass of the polydimethylsiloxane prepolymer is (1.5-3.0):100, and the mass ratio of the carbon nanotubes to the n-type silicon nanowires is (1.0-2.0):1.
[0010] Optionally, the diameter of each of the n-type silicon nanowires is any value between 100 nm and 800 nm.
[0011] Optionally, the n-type silicon nanowires are prepared by chemical vapor deposition (CVD), which uses silicon monoxide powder as the silicon source and tin particles as the catalyst. The silicon monoxide powder is reacted at 1300℃-1360℃, and the silicon nanowires are deposited in a deposition zone at 900℃-1000℃. The reaction pressure is 80Pa-120Pa, and the reaction time is 90min-150min.
[0012] Optionally, the silicon nanowires are treated with hydrofluoric acid solution for 20-40 minutes.
[0013] Optionally, the mass ratio of the polydimethylsiloxane adhesive to the curing agent is any value in the range of (8-12):1.
[0014] Optionally, the composite material exhibits a linear negative temperature coefficient response in the range of 30℃-70℃, with a temperature resistivity of -1.18% / ℃.
[0015] According to a second aspect of the present invention, the present invention also provides a method for preparing the silicon nanowire / carbon nanotube / polydimethylsiloxane composite material according to any one of the above claims, comprising the following steps: Polydimethylsiloxane adhesive is mixed with a curing agent to obtain a polydimethylsiloxane prepolymer; Based on the mass of the polydimethylsiloxane prepolymer, carbon nanotubes with a mass fraction of 1.5wt%-3.0wt% were added to the polydimethylsiloxane prepolymer and ultrasonically dispersed to obtain a carbon nanotube / polydimethylsiloxane premix. Based on the mass of the polydimethylsiloxane prepolymer, n-type silicon nanowires with a mass fraction of 1.0 wt%-1.5 wt% were added to the carbon nanotube / polydimethylsiloxane premix and stirred to obtain a composite material precursor; and The composite material precursor is thermosetting so that multiple silicon nanowires are electrically connected through the carbon nanotubes to form a silicon nanowire-carbon nanotube hybrid conductive network.
[0016] Optionally, the time for ultrasonic dispersion of the carbon nanotubes is any value between 5 min and 15 min.
[0017] According to a third aspect of the present invention, the present invention also provides a flexible temperature sensor, comprising a flexible substrate, a temperature-sensitive element disposed on the flexible substrate, and a first electrode and a second electrode electrically connected to both ends of the temperature-sensitive element, wherein the temperature-sensitive element is formed of a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material as described in any of the preceding claims.
[0018] Optionally, the flexible substrate is a polyethylene terephthalate substrate, the temperature-sensitive element is a composite material strip with a preset size, and the first electrode and the second electrode each include copper wires fixed to both ends of the temperature-sensitive element by carbon conductive adhesive; the flexible temperature sensor exhibits a linear negative temperature coefficient response in the range of 30℃-70℃, with a response time of 2.5s, and can resolve a temperature change of 0.1℃ in the range of 36℃-38℃.
[0019] This invention achieves a composite material temperature response determined by the synergistic effect of the material combination of n-type silicon nanowires, carbon nanotubes, and polydimethylsiloxane, the construction of a hybrid conductive network, and the control of the component ratios. This response is jointly determined by the positive temperature coefficient contribution of the carbon nanotube conductive network and the strain-induced negative piezoresistive contribution of the n-type silicon nanowires. Furthermore, by adjusting the relative content of carbon nanotubes and n-type silicon nanowires, the relative contributions of the two to the change in the total resistance of the composite material can be altered, thereby obtaining a segmented PTC / NTC temperature response or a continuous NTC temperature response within a preset temperature range. Specifically, when the carbon nanotube content is low, the composite material can exhibit a segmented temperature response that transitions from a positive temperature coefficient (PTC) response to a negative temperature coefficient (NTC) response. When the mass ratio of carbon nanotubes to polydimethylsiloxane prepolymer is (2.25-3.0):100, and the mass ratio of carbon nanotubes to n-type silicon nanowires is (1.5-2.0):1, the carbon nanotubes form a relatively stable bridging network, and the negative piezoresistive contribution of the n-type silicon nanowires dominates in the range of 30℃-70℃, causing the composite material to exhibit a continuous NTC response.
[0020] Furthermore, the diameter of each n-type silicon nanowire in this invention is any value between 100nm and 800nm, which is beneficial to take into account the specific surface area, strain response capability, structural integrity and dispersibility of the n-type silicon nanowire in polydimethylsiloxane, so that carbon nanotubes can form more interfacial contacts with the n-type silicon nanowires and form conductive bridges between the spaced n-type silicon nanowires.
[0021] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings. Attached Figure Description
[0022] The following sections will describe some specific embodiments of the invention in detail by way of example and not limitation, with reference to the accompanying drawings. The same reference numerals in the drawings denote the same or similar parts or portions. Those skilled in the art should understand that these drawings are not necessarily drawn to scale. In the drawings: Figure 1 This is a microscopic morphology diagram of an n-type silicon nanowire and a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material in one embodiment of the present invention; Figure 2 This is the current-voltage characteristic curve of the silicon nanowire / carbon nanotube / polydimethylsiloxane composite material in one embodiment of the present invention; Figure 3This is a curve showing the relationship between the thermal strain of polydimethylsiloxane and temperature in one embodiment of the present invention; Figure 4 This is a finite element model of n-type silicon nanowires embedded in polydimethylsiloxane in one embodiment of the present invention; Figure 5 yes Figure 4 The strain distribution of the n-type silicon nanowire in the finite element model is shown in the figure when the temperature change is 40℃. Figure 6 This is a schematic diagram of the structural changes of a silicon nanowire-carbon nanotube hybrid conductive network before and after heating in one embodiment of the present invention; Figure 7 This is a flowchart of a method for preparing a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material in one embodiment of the present invention; Figure 8 These are photographs of the bending, twisting, and cutting of a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material sample in one embodiment of the present invention. Figure 9 These are photographs of polydimethylsiloxane composite material samples with different n-type silicon nanowire and carbon nanotube contents. Figure 10 These are the stepped heating current response curve and temperature response sensitivity fitting curve of the composite material obtained in Example 1; Figure 11 These are the stepped heating current response curve and temperature response sensitivity fitting curve of the composite material obtained in Example 2; Figure 12 These are the stepped heating current response curve and temperature response sensitivity fitting curve of the composite material obtained in Example 3; Figure 13 This is a curve showing the relative resistance change rate-time of a flexible temperature sensor when switching between ambient temperature and 50°C, according to one embodiment of the present invention. Figure 14 This is a relative resistance change rate-time curve of a flexible temperature sensor used for human respiratory temperature monitoring in one embodiment of the present invention. Detailed Implementation
[0023] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings and examples. The following examples are for illustrative purposes only and are not intended to limit the scope of the invention.
[0024] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, the specific embodiments of this application will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, it should be noted that, for ease of description, only the parts relevant to this application are shown in the accompanying drawings, not the entire structure. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of this application.
[0025] The terms “comprising” and “having”, and any variations thereof, used in this application are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that includes a series of steps or units is not limited to the steps or units listed, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to such process, method, product, or apparatus.
[0026] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0027] Figure 1 These are microscopic morphology images of n-type silicon nanowires and silicon nanowire / carbon nanotube / polydimethylsiloxane composite materials in one embodiment of the present invention. Figure 2 This is the current-voltage characteristic curve of the silicon nanowire / carbon nanotube / polydimethylsiloxane composite material in one embodiment of the present invention. Figure 3 This is a curve showing the relationship between the thermal strain of polydimethylsiloxane and temperature in one embodiment of the present invention. Figure 4 This is a finite element model of n-type silicon nanowires embedded in polydimethylsiloxane in one embodiment of the present invention. Figure 5 yes Figure 4 The diagram shows the strain distribution of n-type silicon nanowires in the finite element model at a temperature change of 40℃. Figure 6 This is a schematic diagram showing the structural changes of a silicon nanowire-carbon nanotube hybrid conductive network before and after heating in one embodiment of the present invention.
[0028] The present invention provides a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material for temperature sensing, the composite material comprising a polydimethylsiloxane (PDMS) matrix and n-type silicon nanowires and carbon nanotubes dispersed in the polydimethylsiloxane matrix. n-type silicon nanowires are spaced apart from each other, and at least some carbon nanotubes are located between the spaced-apart n-type silicon nanowires and are in contact with at least two n-type silicon nanowires respectively, so that multiple n-type silicon nanowires are electrically connected through carbon nanotubes to form a silicon nanowire-carbon nanotube hybrid conductive network; wherein, polydimethylsiloxane body is formed by curing polydimethylsiloxane prepolymer, which includes polydimethylsiloxane adhesive and curing agent, and the total mass of polydimethylsiloxane prepolymer is the sum of the masses of polydimethylsiloxane adhesive and curing agent; the mass ratio of n-type silicon nanowires to the total mass of polydimethylsiloxane prepolymer is (1.0-1.5):100, the mass ratio of carbon nanotubes to the total mass of polydimethylsiloxane prepolymer is (1.5-3.0):100, and the mass ratio of carbon nanotubes to n-type silicon nanowires is (1.0-2.0):1.
[0029] In this embodiment, through the synergy between the material combination of n-type silicon nanowires, carbon nanotubes and polydimethylsiloxane, the construction of the hybrid conductive network and the control of the component ratio, the temperature response of the composite material is jointly determined by the positive temperature coefficient contribution of the carbon nanotube conductive network and the strain-induced negative piezoresistive contribution of the n-type silicon nanowires. Furthermore, by adjusting the relative content of carbon nanotubes and n-type silicon nanowires, the relative contribution of the two to the change of the total resistance of the composite material can be changed, thereby obtaining a segmented PTC / NTC temperature response or a continuous NTC temperature response within a preset temperature range. Specifically, when the carbon nanotube content is low, the composite material exhibits a segmented temperature response that transitions from a positive temperature coefficient (PTC) response to a negative temperature coefficient (NTC) response. When the mass ratio of carbon nanotubes to polydimethylsiloxane prepolymer is (2.25-3.0):100, and the mass ratio of carbon nanotubes to n-type silicon nanowires is (1.5-2.0):1, the carbon nanotubes form a relatively stable bridging network, and the negative piezoresistive contribution of the n-type silicon nanowires dominates in the 30℃-70℃ range, resulting in a continuous NTC response in the composite material. In this embodiment, the spaced-apart n-type silicon nanowires themselves are unlikely to form a continuous conductive path.
[0030] In this embodiment, by contacting at least some carbon nanotubes with at least two n-type silicon nanowires respectively, the n-type silicon nanowires that are separate from each other can be connected to the same conductive network. This allows the resistance change generated by the n-type silicon nanowires to be transmitted along the hybrid conductive network and detected by the external electrode, avoiding excessively high resistance of the composite material or difficulty in signal output due to the lack of effective contact between silicon nanowires.
[0031] In this embodiment, the n-type silicon nanowires are spaced apart within the polydimethylsiloxane matrix, which helps reduce entanglement and aggregation between the silicon nanowires. This allows the polydimethylsiloxane matrix to coat the silicon nanowires and transfer the mechanical forces generated by thermal expansion to them. Simultaneously, this distribution allows the carbon nanotubes to act as conductive bridges connecting the different silicon nanowires, thus enabling the piezoresistive response of the silicon nanowires to participate in regulating the overall resistance of the composite material.
[0032] like Figure 1 As shown in (a), the fabricated n-type silicon nanowires exhibit a slender, one-dimensional linear morphology with a high aspect ratio, and a diameter of approximately 100-800 nm. Figure 1 As shown in (b), a single n-type silicon nanowire is embedded in polydimethylsiloxane and extends out from the cross section of the composite material, indicating that the polydimethylsiloxane can coat and fix the n-type silicon nanowire, providing a structural basis for transmitting mechanical action to the n-type silicon nanowire when the matrix is thermally expanded.
[0033] like Figure 1 (c) and Figure 1 As shown in (d), orange circles indicate the n-type silicon nanowire ends extending from the composite material cross-section. When the n-type silicon nanowire content increases from 1.5 wt% to 3 wt%, the number of silicon nanowire ends observable per unit cross-section increases. Figure 1 (c) Samples corresponding to the proportions specified in this application. Figure 1 (d) shows a 3wt% sample as a comparative sample, used to illustrate the effect of silicon nanowire content on its distribution density in the matrix.
[0034] like Figure 1 (e) and Figure 1 (f) shows that smaller diameter carbon nanotubes are distributed between spaced-apart n-type silicon nanowires. The carbon nanotubes indicated by the red arrows are in contact with adjacent n-type silicon nanowires, thus bridging the separated n-type silicon nanowires. This microstructure indicates that a hybrid conductive network with carbon nanotubes as conductive bridges and n-type silicon nanowires as piezoresistive response units is formed in the composite material, providing a structural basis for the macroscopic conductive pathway for the resistance change of the n-type silicon nanowires to be transmitted to the composite material.
[0035] In this embodiment, the polydimethylsiloxane emulsion possesses thermal expansion and elasticity. When the temperature changes, the matrix can deform accordingly and transmit stress to the embedded n-type silicon nanowires, causing the temperature stimulus to be primarily converted into mechanical strain in the silicon nanowires. Furthermore, the polydimethylsiloxane emulsion can also coat and fix silicon nanowires and carbon nanotubes, allowing the hybrid conductive network to maintain its structural integrity under bending or deformation conditions.
[0036] The electrical transport properties, thermal strain transfer process, and temperature response mechanism of silicon nanowire / carbon nanotube / polydimethylsiloxane composite materials were analyzed, and the following results were obtained: Figures 2 to 6 The test results are shown.
[0037] like Figure 2 As shown, within the test voltage range of -4V to 4V, the current flowing through the composite material increases with the increase of the absolute value of the test voltage, with corresponding trends in the positive and negative voltage regions. The two current-voltage curves in the figure are generally close and both continuously pass near zero voltage, indicating that the hybrid conductive network formed by n-type silicon nanowires and carbon nanotubes can form a continuous current transport path in polydimethylsiloxane. The non-linear variation of the current-voltage curves indicates that the electrical transport of the composite material depends not only on the resistance of the n-type silicon nanowires and carbon nanotubes themselves, but also on the contact state between the n-type silicon nanowires and carbon nanotubes, as well as the interfacial transport state between adjacent conductive materials.
[0038] like Figure 3 As shown, with 30℃ as the reference temperature, the thermal strain calculated by the model increases approximately linearly with increasing temperature; when the temperature increases from 30℃ to 70℃, the thermal strain increases from 0 to approximately 1.2%. Therefore, within the above temperature range, polydimethylsiloxane can convert temperature changes into continuous thermal expansion deformation, providing a mechanical effect for adjusting the relative positions and contact relationships between the conductive materials in the hybrid conductive network.
[0039] like Figure 4 and Figure 5 As shown, the finite element model includes polydimethylsiloxane and n-type silicon nanowires embedded in the polydimethylsiloxane. After the polydimethylsiloxane undergoes thermal expansion, the thermal strain can be transferred to the n-type silicon nanowires through the interface between the two, causing deformation along the length of the n-type silicon nanowires, with a strain reaching approximately 12 × 10⁻⁶. -3 The results show that polydimethylsiloxane not only coats and immobilizes n-type silicon nanowires and carbon nanotubes, but also transfers thermal deformation caused by temperature changes to the n-type silicon nanowires and hybrid conductive networks.
[0040] like Figure 6As shown, at the initial temperature, n-type silicon nanowires are spaced apart, with at least some carbon nanotubes located between the spaced-apart n-type silicon nanowires and in contact with at least two n-type silicon nanowires, thus electrically connecting multiple n-type silicon nanowires through carbon nanotubes to form a hybrid conductive network. When the temperature rises, the polydimethylsiloxane undergoes thermal expansion, causing displacement or deformation of the n-type silicon nanowires and carbon nanotubes. This results in changes in the contact area, number of contacts, or spacing between some n-type silicon nanowires and carbon nanotubes, as well as between some carbon nanotubes. Figure 6 The dashed circles in the diagram indicate changes in some conductive contact points. Simultaneously, the thermal strain transmitted to the n-type silicon nanowires also affects the carrier transport state of the n-type silicon nanowires themselves. Therefore, temperature changes can simultaneously modulate the electrical properties of the n-type silicon nanowires as well as the conductive paths and interface transport states in the hybrid conductive network, causing the electrical parameters of the composite material to change with temperature, thereby achieving temperature sensing.
[0041] In this embodiment, the mass ratio of n-type silicon nanowires to polydimethylsiloxane prepolymer is limited to (1.0-1.5):100, for example, it can be 1.0:100, 1.1:100, 1.125:100, 1.2:100, 1.25:100, 1.3:100, 1.35:100, 1.4:100, 1.45:100, or 1.5:100. The mass ratio of carbon nanotubes to polydimethylsiloxane prepolymer is limited to (2.25-3.0):100, for example, it can be 2.25:100, 2.4:100, 2.5:100, 2.6:100, etc. The mass ratios of carbon nanotubes to n-type silicon nanowires are limited to 2.7:100, 2.8:100, 2.9:100, or 3.0:100, with the mass ratio of carbon nanotubes to n-type silicon nanowires constrained to (1.5-2.0):1 (e.g., 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, or 2.0:1). This allows for adjustment of the relative relationship between the conductive pathways of carbon nanotubes and the piezoresistive contribution of silicon nanowires. Specifically, the carbon nanotube content is sufficient not only to bridge the silicon nanowires and maintain the connectivity of the conductive network but also to prevent the formation of overly dense independent conductive networks by carbon nanotubes, which would weaken the influence of silicon nanowire resistance changes on the total resistance of the composite material. Here, the mass relationship between n-type silicon nanowires, carbon nanotubes, and polydimethylsiloxane prepolymer must be satisfied simultaneously.
[0042] In a further embodiment, the diameter of each n-type silicon nanowire is any value between 100 nm and 800 nm. Controlling the diameter of the n-type silicon nanowire within this range is beneficial for balancing the specific surface area, strain response capability, structural integrity, and dispersibility within the polydimethylsiloxane matrix. This allows for more interfacial contacts between carbon nanotubes and the n-type silicon nanowires, and the formation of conductive bridges between the spaced-apart n-type silicon nanowires. If the diameter of the n-type silicon nanowire is too small, it is prone to entanglement or breakage during dispersion and recombination; if the diameter is too large, the interfacial contact area formed per unit mass of n-type silicon nanowires decreases, which is detrimental to constructing a hybrid conductive network sensitive to temperature and thermal strain changes. Specifically, the diameter of each n-type silicon nanowire can be 100 nm, 200 nm, 300 nm, 330 nm, 360 nm, 400 nm, 440 nm, 470 nm, 500 nm, 600 nm, 700 nm, or 800 nm.
[0043] In a further embodiment, n-type silicon nanowires are prepared by chemical vapor deposition (CVD). CVD uses silicon monoxide powder as the silicon source and tin particles as the catalyst. The silicon monoxide powder is reacted at 1300℃-1360℃, and silicon nanowires are deposited in a deposition zone at 900℃-1000℃. The reaction pressure is 80Pa-120Pa, and the reaction time is 90min-150min. The above reaction temperature allows the silicon monoxide powder to form a silicon-containing gaseous material for silicon nanowire growth. The deposition zone temperature is used to regulate the adsorption, nucleation, and axial growth process of the silicon-containing gaseous material on the tin particles. The reaction pressure is used to regulate the transport rate and concentration of the silicon-containing gaseous material, and the reaction time is used to control the growth length and yield of the silicon nanowires. This is beneficial for obtaining silicon nanowires with a one-dimensional linear morphology and a large aspect ratio. Specifically, the reaction temperature can be 1300℃, 1310℃, 1320℃, 1330℃, 1340℃, 1350℃, or 1360℃; the deposition zone temperature can be 900℃, 920℃, 940℃, 950℃, 960℃, 980℃, or 1000℃; the reaction pressure can be 80Pa, 90Pa, 95Pa, 100Pa, 105Pa, 110Pa, or 120Pa; and the reaction time can be 90min, 100min, 110min, 120min, 130min, 140min, or 150min.
[0044] In a further embodiment, the silicon nanowires are treated with hydrofluoric acid solution for 20-40 minutes. Hydrofluoric acid treatment removes the native oxide layer and some surface impurities from the silicon nanowires, reducing the obstruction of charge transport between the silicon nanowires and carbon nanotubes by the native oxide layer. This allows the carbon nanotubes and silicon nanowires to form electrical contacts, thereby reducing the impact of inconsistent interfacial contact states on the electrical properties of the composite material. Controlling the treatment time within the above range can remove the surface oxide layer while reducing the possibility of prolonged treatment adversely affecting the surface structure of the silicon nanowires. Specifically, the hydrofluoric acid treatment time can be 20 minutes, 23 minutes, 26 minutes, 30 minutes, 34 minutes, 37 minutes, or 40 minutes.
[0045] In a further embodiment, the mass ratio of polydimethylsiloxane adhesive to curing agent is any value within the range of (8-12):1. The mass ratio of polydimethylsiloxane adhesive to curing agent is used to adjust the degree of crosslinking, flexibility, and heat distortion capability of the polydimethylsiloxane body. Controlling the mass ratio within the above range allows the cured polydimethylsiloxane body to coat and fix n-type silicon nanowires and carbon nanotubes, while retaining the ability to expand or contract with temperature changes, enabling the thermal strain generated by the polydimethylsiloxane body to be transferred to the n-type silicon nanowires and the silicon nanowire-carbon nanotube hybrid conductive network. Specifically, the mass ratio of polydimethylsiloxane adhesive to curing agent can be 8:1, 8.5:1, 9:1, 10:1, 11:1, 11.5:1, or 12:1.
[0046] In a further embodiment, the composite material exhibits a linear negative temperature coefficient response in the range of 30°C to 70°C, with a temperature resistivity of -1.18% / °C. This linear negative temperature coefficient response means that the resistance of the composite material decreases with increasing temperature, and the rate of change of resistance is linearly related to the amount of temperature change. This response is jointly formed by the temperature-dependent carrier transport characteristics of the n-type silicon nanowires, the thermal strain generated by the polydimethylsiloxane body, and the changes in the interfacial transport state in the hybrid conductive network. The linear response facilitates the determination of the temperature to be measured based on the resistance change of the composite material and simplifies the calibration and signal processing of the temperature sensor. Specifically, the operating temperature of the composite material can be 30°C, 35°C, 40°C, 45°C, 50°C, 60°C, or 70°C.
[0047] Figure 7 This is a flowchart illustrating the preparation method of a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material in one embodiment of the present invention.
[0048] like Figure 7 As shown, the present invention also provides a method for preparing the silicon nanowire / carbon nanotube / polydimethylsiloxane composite material according to any one of the above claims, comprising the following steps: Step S100: Mix the polydimethylsiloxane adhesive with the curing agent to obtain the polydimethylsiloxane prepolymer; Step S200: Based on the mass of the polydimethylsiloxane prepolymer, add carbon nanotubes with a mass fraction of 1.5wt%-3.0wt% to the polydimethylsiloxane prepolymer and disperse them ultrasonically to obtain a carbon nanotube / polydimethylsiloxane premix. Step S300: Based on the mass of the polydimethylsiloxane prepolymer, add 1.0wt%-1.5wt% n-type silicon nanowires to the carbon nanotube / polydimethylsiloxane premix and stir to obtain the composite material precursor; and Step S400: The composite material precursor is thermosetting to electrically connect multiple silicon nanowires through carbon nanotubes, forming a silicon nanowire-carbon nanotube hybrid conductive network.
[0049] In this embodiment, carbon nanotubes are first added to a polydimethylsiloxane prepolymer and ultrasonically dispersed. This ultrasonic action breaks down carbon nanotube agglomerates, ensuring the carbon nanotubes are pre-dispersed within the prepolymer. Subsequently, n-type silicon nanowires are added and mixed using stirring. This reduces the risk of breakage or structural damage to the n-type silicon nanowires caused by high-energy ultrasound, while simultaneously distributing the dispersed carbon nanotubes among the spaced-apart n-type silicon nanowires and forming interfacial contacts. By controlling the amounts of carbon nanotubes and n-type silicon nanowires, the carbon nanotubes primarily function as conductive bridges connecting the spaced-apart n-type silicon nanowires, rather than forming a separate conductive network. After thermosetting the composite precursor, the polydimethylsiloxane polymer crosslinks, fixing the n-type silicon nanowires, carbon nanotubes, and their interfacial contacts, thereby forming a silicon nanowire-carbon nanotube hybrid conductive network. This preparation sequence is beneficial for balancing the connectivity of the hybrid conductive network and the structural integrity of the n-type silicon nanowires. It allows the thermal strain generated by the polydimethylsiloxane body to be transferred to the n-type silicon nanowires, and maintains the electrical connection between the n-type silicon nanowires through carbon nanotubes, thereby forming a thermo-mechanical-electrical signal conversion process dominated by the temperature response and negative piezoresistive effect of the n-type silicon nanowires.
[0050] In a further embodiment, the ultrasonic dispersion time of carbon nanotubes is any value between 5 min and 15 min, for example, 5 min, 7 min, 9 min, 11 min, 13 min, or 15 min. By controlling the ultrasonic dispersion time within the above range, the agglomeration structure between carbon nanotubes can be sufficiently broken, allowing the carbon nanotubes to be dispersed more uniformly in the polydimethylsiloxane prepolymer. At the same time, excessive breakage of carbon nanotubes due to excessive ultrasonic time is avoided, which is beneficial to maintaining the aspect ratio and conductive bridging ability of carbon nanotubes. Since the carbon nanotubes are ultrasonically dispersed before the addition of n-type silicon nanowires, the breakage of n-type silicon nanowires caused by ultrasonic action can also be avoided, thus balancing the uniformity of carbon nanotube dispersion and the structural integrity of n-type silicon nanowires, which is beneficial to the subsequent formation of a continuous and stable silicon nanowire-carbon nanotube hybrid conductive network.
[0051] This invention also provides a flexible temperature sensor, comprising a flexible substrate, a temperature-sensitive element disposed on the flexible substrate, and a first electrode and a second electrode electrically connected to both ends of the temperature-sensitive element, respectively. The temperature-sensitive element is formed of a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material as described above. The flexible substrate provides support and load-bearing capacity for the temperature-sensitive element, allowing the flexible temperature sensor to conform to human skin, curved surfaces, or other non-planar test objects. The first and second electrodes are used to apply test electrical signals to both ends of the temperature-sensitive element and extract the resistance change of the temperature-sensitive element. When the temperature changes, the polydimethylsiloxane undergoes thermal expansion and deformation, transferring strain to the n-type silicon nanowires. The carbon nanotubes maintain the electrical connection between the spaced-apart n-type silicon nanowires, enabling the temperature-sensitive element to convert temperature changes into measurable resistance changes, thereby balancing the flexibility of the device, the stability of the conductive network, and temperature response capability.
[0052] In a further embodiment, the flexible substrate is a polyethylene terephthalate (PET) substrate, the temperature-sensitive element is a composite material strip of a preset size, and the first electrode and the second electrode each include copper wires fixed to both ends of the temperature-sensitive element by carbon conductive adhesive. The PET substrate possesses flexibility, electrical insulation, and dimensional stability, enabling it to provide stable support for the temperature-sensitive element in a bent or fitted state. Setting the temperature-sensitive element as a composite material strip of a preset size ensures that its effective conductive length and cross-sectional area remain relatively consistent, which helps reduce initial resistance differences between devices and improves the repeatability of detection results. The carbon conductive adhesive increases the effective contact area between the copper wires and the composite material strip and reduces contact resistance, while the copper wires stably extract the electrical signal generated by the temperature-sensitive element, thereby reducing the influence of the electrode connection state on the temperature detection results.
[0053] In this embodiment, the flexible temperature sensor exhibits a linear negative temperature coefficient response within the range of 30℃ to 70℃, and its operating temperature can be, for example, 30℃, 35℃, 40℃, 50℃, 60℃, or 70℃. Therefore, it can quantitatively detect temperatures within this range based on changes in the resistance of the temperature-sensitive element, and it simplifies the calibration and conversion process between temperature and resistance. The flexible temperature sensor has a response time of 2.5s, enabling it to quickly follow temperature changes in the object being measured, making it suitable for human body surface temperature monitoring, wearable device temperature monitoring, and temperature detection in flexible electronic devices.
[0054] In this embodiment, the flexible temperature sensor can also distinguish temperature changes of 0.1℃ within the range of 36℃-38℃. The detected temperatures within this range can be, for example, 36.0℃, 36.1℃, 36.5℃, 37.0℃, 37.5℃, or 38.0℃. Therefore, the flexible temperature sensor can identify minute temperature changes within the range of human body surface temperature, making it suitable for continuous and precise monitoring of trends in human body temperature changes.
[0055] The technical solution of this application will be further described below with reference to specific embodiments.
[0056] Example 1
[0057] The polydimethylsiloxane adhesive and curing agent were mixed at a mass ratio of 10:1 to obtain a polydimethylsiloxane prepolymer. Based on the mass of the polydimethylsiloxane prepolymer, 1.5 wt% carbon nanotubes were added and ultrasonically dispersed for 10 min to obtain a carbon nanotube / polydimethylsiloxane premix. Subsequently, 1.5 wt% n-type silicon nanowires were added and stirred until uniformly dispersed to obtain a composite material precursor. The composite material precursor was thermosetting to obtain a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material. In this embodiment, the mass ratio of carbon nanotubes to n-type silicon nanowires was 1:1.
[0058] Example 2
[0059] Based on the mass of polydimethylsiloxane prepolymer, the mass fraction of carbon nanotubes was 2.25 wt%, and the mass ratio of carbon nanotubes to n-type silicon nanowires was 1.5:1.
[0060] Example 3
[0061] Based on the mass of polydimethylsiloxane prepolymer, the mass fraction of carbon nanotubes is 3.0 wt%, and the mass ratio of carbon nanotubes to n-type silicon nanowires is 2:1.
[0062] Comparative Example 1 The only difference between Comparative Example 1 and Example 1 is that, based on the total mass of the polydimethylsiloxane prepolymer, the amount of n-type silicon nanowires added is 2.25 wt%, and the amount of carbon nanotubes added is kept at 1.5 wt%.
[0063] Comparative Example 2 The only difference between Comparative Example 2 and Example 1 is that, based on the total mass of the polydimethylsiloxane prepolymer, the amount of n-type silicon nanowires added is 3.0 wt%, and the amount of carbon nanotubes added is kept at 1.5 wt%.
[0064] Comparative Example 3 The only difference between Comparative Example 3 and Example 2 is that, based on the total mass of the polydimethylsiloxane prepolymer, the amount of n-type silicon nanowires added is 2.25 wt%, and the amount of carbon nanotubes added is maintained at 2.25 wt%.
[0065] Comparative Example 4 The only difference between Comparative Example 4 and Example 2 is that, based on the total mass of the polydimethylsiloxane prepolymer, the amount of n-type silicon nanowires added is 3.0 wt%, and the amount of carbon nanotubes added is kept at 2.25 wt%.
[0066] Comparative Example 5 The only difference between Comparative Example 5 and Example 3 is that, based on the total mass of the polydimethylsiloxane prepolymer, the amount of n-type silicon nanowires added was adjusted from 1.5 wt% to 2.25 wt%, while the amount of carbon nanotubes added remained at 3.0 wt%.
[0067] Comparative Example 6 The only difference between Comparative Example 6 and Example 3 is that, based on the total mass of the polydimethylsiloxane prepolymer, the amount of n-type silicon nanowires added was adjusted from 1.5 wt% to 3.0 wt%, while the amount of carbon nanotubes added remained at 3.0 wt%.
[0068] Figure 8 These are photographs of the bending, twisting, and cutting of a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material sample according to one embodiment of the present invention. Figure 9 These are photographs of polydimethylsiloxane composite material samples with different contents of n-type silicon nanowires and carbon nanotubes. Figure 10 These are the stepped heating current response curve and temperature response sensitivity fitting curve of the composite material obtained in Example 1. Figure 11 These are the stepped heating current response curve and temperature response sensitivity fitting curve of the composite material obtained in Example 2. Figure 12 These are the stepped heating current response curve and temperature response sensitivity fitting curve of the composite material obtained in Example 3. Figure 13 This is a curve showing the relative resistance change rate versus time of a flexible temperature sensor in one embodiment of the present invention when switching between ambient temperature and 50°C. Figure 14 This is a relative resistance change rate-time curve of a flexible temperature sensor used for human respiratory temperature monitoring in one embodiment of the present invention.
[0069] To verify the flexibility and formability of the silicon nanowire / carbon nanotube / polydimethylsiloxane composite material, clarify the influence of carbon nanotube content on the temperature response mode and temperature response sensitivity of the composite material, and evaluate the dynamic response performance and actual temperature detection capability of the flexible temperature sensor, bending, torsion, cutting, and stepped heating electrical response tests were conducted on composite materials with different ratios. Temperature switching response tests and human respiratory temperature monitoring tests were also performed on the flexible temperature sensor formed from the composite material. The results are as follows: Figures 8 to 14 The test results are shown.
[0070] like Figure 8 As shown, the obtained silicon nanowire / carbon nanotube / polydimethylsiloxane composite strips can be bent into arc-shaped structures under external force, and can also be twisted and cut into sheet-like structures with different contours. During the above deformation and processing, the composite material did not undergo macroscopic fracture, indicating that polydimethylsiloxane can endow the composite material with flexibility and shape processing capabilities, making it suitable for forming the temperature-sensitive element of a flexible temperature sensor and able to conform to curved surfaces to be measured.
[0071] like Figure 9 As shown, from top to bottom, composite material samples with n-type silicon nanowires and carbon nanotubes at mass fractions of 1.5 wt.% and 0 wt.%, 1.5 wt.% and 1.5 wt.%, 1.5 wt.% and 2.25 wt.%, 1.5 wt.% and 3.0 wt.%, and 3.0 wt.% and 0 wt.%, respectively, are presented. All mass fractions are based on the total mass of the polydimethylsiloxane prepolymer. The second to fourth samples correspond to Examples 1, 2, and 3, respectively, while the first and fifth samples serve as control samples without carbon nanotubes. The composite materials obtained in Examples 1-3 can all be fabricated into strip structures of predetermined dimensions. As the carbon nanotube content increases, the macroscopic color of the samples gradually deepens, corresponding to the increased amount of carbon nanotubes added to the polydimethylsiloxane prepolymer.
[0072] To investigate the effect of n-type silicon nanowires and carbon nanotubes content on the conductivity of the composite material, composite materials were prepared according to the proportions of Examples 1-3 and Comparative Examples 1-6, and their resistance was measured under the same test conditions. The test results are shown in Table 1.
[0073] Table 1. Resistance test results of the composite materials obtained in Examples 1-3 and Comparative Examples 1-6.
[0074]
[0075] Table 1 shows that when the mass fraction of n-type silicon nanowires is fixed at 1.5 wt.%, as the mass fraction of carbon nanotubes increases from 1.5 wt.% to 2.25 wt.% and then to 3.0 wt.%, the resistivity of the composite material decreases from 45.55 MΩ to 4.71 MΩ and then to 0.30 MΩ. This indicates that increasing the carbon nanotube content can increase the probability of effective electrical contact between carbon nanotubes and n-type silicon nanowires, as well as between carbon nanotubes themselves. This allows the spaced-apart n-type silicon nanowires to be connected to a continuous conductive network through the carbon nanotubes, thereby reducing the overall resistivity of the composite material.
[0076] When the mass fraction of n-type silicon nanowires was increased to 2.25 wt.% or 3.0 wt.%, the resistivity of the composite material was greater than 10000 MΩ when the mass fraction of carbon nanotubes was 1.5 wt.%, 2.25 wt.%, and 3.0 wt.%, respectively. This result indicates that simply increasing the content of n-type silicon nanowires does not improve the continuity of the hybrid conductive network. In fact, a higher content of n-type silicon nanowires alters the relative distribution and contact relationship between the n-type silicon nanowires and carbon nanotubes, making it difficult for carbon nanotubes to form continuous and effective bridging paths between the spaced-apart n-type silicon nanowires. Therefore, it is necessary to simultaneously control the amount of n-type silicon nanowires and carbon nanotubes and their mass ratio to balance the conductivity of the composite material and the regulatory effect of n-type silicon nanowires on the overall resistivity change.
[0077] like Figure 10 As shown, in Example 1, the mass fraction of both n-type silicon nanowires and carbon nanotubes was 1.5 wt.%. During the gradual increase of temperature from 30°C to 50°C, the test current generally decreased; however, as the temperature continued to increase from 50°C to 70°C, the test current increased. Correspondingly, the temperature response sensitivity S of the composite material obtained in Example 1 within the range of 30°C-50°C was 0.93%·°C. -1 The temperature response sensitivity S in the range of 50℃-70℃ is -2.77%·℃. -1 The results show a segmented temperature response that transitions from a positive temperature coefficient response to a negative temperature coefficient response. This indicates that when the mass fraction of carbon nanotubes is 1.5 wt.%, the number of conductive bridges formed by the carbon nanotubes is relatively small, and the positive temperature coefficient contribution from the change in the conductive contact state of the carbon nanotubes and the negative temperature coefficient contribution from the n-type silicon nanowires dominate in different temperature ranges, respectively.
[0078] like Figure 11As shown, in Example 2, the mass fraction of n-type silicon nanowires was 1.5 wt.%, and the mass fraction of carbon nanotubes was 2.25 wt.%. As the temperature gradually increased from 30°C to 70°C, the test current increased stepwise, the relative resistivity change rate decreased approximately linearly with increasing temperature, and the temperature response sensitivity S was -1.88%·°C. -1 Compared to Example 1, increasing the carbon nanotube content improves the bridging probability between the spaced-apart n-type silicon nanowires, allowing the hybrid conductive network to remain continuous in the 30°C-70°C range. This also makes the temperature response and negative piezoresistive contribution of the n-type silicon nanowires dominant throughout the entire test temperature range, thereby obtaining a continuous linear negative temperature coefficient response.
[0079] like Figure 12 As shown, in Example 3, the mass fraction of n-type silicon nanowires was 1.5 wt.%, and the mass fraction of carbon nanotubes was 3.0 wt.%. As the temperature gradually increased from 30°C to 70°C, the test current also increased stepwise. The composite material exhibited a linear negative temperature coefficient response in the range of 30°C-70°C, with a temperature response sensitivity S of -0.88%·°C. -1 When the carbon nanotube content was increased to 3.0 wt.%, more parallel conductive paths were formed in the hybrid conductive network, which maintained the continuity of the conductive network. However, at the same time, the degree to which the resistance change of the n-type silicon nanowires could control the total resistance of the composite material was reduced. Therefore, the temperature response sensitivity of Example 3 was lower than that of Example 2.
[0080] comprehensive Figure 10-12 It can be seen that, with the mass fraction of n-type silicon nanowires maintained at 1.5 wt.%, the carbon nanotube content can regulate the relative relationship between the positive and negative temperature coefficient contributions. When the carbon nanotube mass fraction is increased from 1.5 wt.% to 2.25 wt.%, the composite material changes from a segmented temperature response to a linear negative temperature coefficient response within the range of 30℃-70℃. When the carbon nanotube mass fraction is further increased to 3.0 wt.%, the composite material still maintains a linear negative temperature coefficient response, but the sensitivity decreases. Among the three formulations tested in Examples 1-3, Example 2 balances the continuity of the hybrid conductive network and the modulating effect of n-type silicon nanowires on the total resistance of the composite material, exhibiting higher linear negative temperature response sensitivity.
[0081] like Figure 13As shown, after the flexible temperature sensor is transferred from ambient temperature to a 50°C environment, its relative resistance change rate decreases from the initial state to approximately -53% within a short period and remains relatively stable at 50°C. Upon returning the flexible temperature sensor to ambient temperature conditions, its relative resistance change rate gradually recovers to its initial level. The response time during the descent phase is approximately 2.5 seconds, indicating that the flexible temperature sensor can respond quickly to temperature changes and recover its resistance response after the temperature conditions return to normal. Figure 13 The results also demonstrate that the temperature-sensitive element, electrodes, and their connections can maintain their operational status during temperature switching.
[0082] like Figure 14 As shown, when the flexible temperature sensor is used for human respiratory temperature monitoring, each exhalation generates a identifiable peak value of relative resistance change; under different exhalation conditions, the response peak value exhibits distinguishable amplitude variations. Each response peak has a relatively clear rise and fall phase, indicating that the flexible temperature sensor can follow the temperature changes caused by periodic breathing and convert the temperature stimulus from the respiratory airflow into a continuous and detectable electrical signal, thus enabling its use for monitoring human respiratory status and its changing trends.
[0083] In summary, this application constructs a hybrid conductive network in polydimethylsiloxane matrix, consisting of carbon nanotubes bridging spaced n-type silicon nanowires. By adjusting the relative content of carbon nanotubes and n-type silicon nanowires, the thermal strain generated by the polydimethylsiloxane matrix can be transferred to the n-type silicon nanowires, and the corresponding resistance change is output through the hybrid conductive network, thereby obtaining an adjustable temperature response. Specifically, appropriately increasing the carbon nanotube content enables the composite material to exhibit a linear negative temperature coefficient response within the range of 30℃-70℃. The flexible temperature sensor formed from this composite material combines flexibility, rapid temperature response, and the ability to detect minute temperature changes, making it suitable for temperature monitoring of the human body surface, respiration, and flexible electronic devices.
[0084] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0085] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A silicon nanowire / carbon nanotube / polydimethylsiloxane composite material for temperature sensing, characterized in that, Includes polydimethylsiloxane and n-type silicon nanowires and carbon nanotubes dispersed in the polydimethylsiloxane; The n-type silicon nanowires are spaced apart from each other, and at least some of the carbon nanotubes are located between the spaced-apart n-type silicon nanowires and are in contact with at least two n-type silicon nanowires, so that the multiple n-type silicon nanowires are electrically connected through the carbon nanotubes to form a silicon nanowire-carbon nanotube hybrid conductive network; wherein, The polydimethylsiloxane body is formed by curing a polydimethylsiloxane prepolymer, which includes a polydimethylsiloxane adhesive and a curing agent. The total mass of the polydimethylsiloxane prepolymer is the sum of the masses of the polydimethylsiloxane adhesive and the curing agent. The mass ratio of the n-type silicon nanowires to the total mass of the polydimethylsiloxane prepolymer is (1.0-1.5):100, the mass ratio of the carbon nanotubes to the total mass of the polydimethylsiloxane prepolymer is (1.5-3.0):100, and the mass ratio of the carbon nanotubes to the n-type silicon nanowires is (1.0-2.0):
1.
2. The silicon nanowire / carbon nanotube / polydimethylsiloxane composite material for temperature sensing according to claim 1, characterized in that, The diameter of each of the n-type silicon nanowires is any value between 100 nm and 800 nm.
3. The silicon nanowire / carbon nanotube / polydimethylsiloxane composite material for temperature sensing according to claim 1, characterized in that, The n-type silicon nanowires are prepared by chemical vapor deposition (CVD). The CVD method uses silicon monoxide powder as the silicon source and tin particles as the catalyst. The silicon monoxide powder is reacted at 1300℃-1360℃, and the silicon nanowires are deposited in a deposition zone at 900℃-1000℃. The reaction pressure is 80Pa-120Pa, and the reaction time is 90min-150min.
4. The silicon nanowire / carbon nanotube / polydimethylsiloxane composite material for temperature sensing according to claim 2, characterized in that, The silicon nanowires were treated with hydrofluoric acid solution for 20-40 minutes.
5. The silicon nanowire / carbon nanotube / polydimethylsiloxane composite material for temperature sensing according to claim 1, characterized in that, The mass ratio of the polydimethylsiloxane adhesive to the curing agent is any value in the range of (8-12):
1.
6. The silicon nanowire / carbon nanotube / polydimethylsiloxane composite material for temperature sensing according to claim 1, characterized in that, The composite material exhibits a linear negative temperature coefficient response in the range of 30℃-70℃, with a temperature resistivity of -1.18% / ℃.
7. A method for preparing a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material according to any one of claims 1-6, characterized in that, Includes the following steps: Polydimethylsiloxane adhesive is mixed with a curing agent to obtain a polydimethylsiloxane prepolymer; Based on the mass of the polydimethylsiloxane prepolymer, carbon nanotubes with a mass fraction of 1.5wt%-3.0wt% were added to the polydimethylsiloxane prepolymer and ultrasonically dispersed to obtain a carbon nanotube / polydimethylsiloxane premix. Based on the mass of the polydimethylsiloxane prepolymer, n-type silicon nanowires with a mass fraction of 1.0 wt%-1.5 wt% were added to the carbon nanotube / polydimethylsiloxane premix and stirred to obtain a composite material precursor; and The composite material precursor is thermosetting so that multiple silicon nanowires are electrically connected through the carbon nanotubes to form a silicon nanowire-carbon nanotube hybrid conductive network.
8. The method for preparing the silicon nanowire / carbon nanotube / polydimethylsiloxane composite material according to claim 7, characterized in that, The time for ultrasonic dispersion of the carbon nanotubes is any value between 5 min and 15 min.
9. A flexible temperature sensor, characterized in that, The device includes a flexible substrate, a temperature-sensitive element disposed on the flexible substrate, and a first electrode and a second electrode electrically connected to both ends of the temperature-sensitive element, wherein the temperature-sensitive element is formed of a silicon nanowire / carbon nanotube / polydimethylsiloxane composite material as described in any one of claims 1-6.
10. The flexible temperature sensor according to claim 9, characterized in that, The flexible substrate is a polyethylene terephthalate substrate, and the temperature-sensitive element is a composite material strip with a preset size. The first electrode and the second electrode each include copper wires fixed to both ends of the temperature-sensitive element by carbon conductive adhesive. The flexible temperature sensor exhibits a linear negative temperature coefficient response in the range of 30℃-70℃, with a response time of 2.5s, and can resolve temperature changes of 0.1℃ in the range of 36℃-38℃.