A high-gloss, wear-resistant water-based two-component road marking paint and its preparation method
By combining water-based carboxyl-containing hydroxy acrylic dispersion with water-dispersible polyether-modified HDI trimer, a three-dimensional network cross-linked structure is formed, which solves the problems of agglomeration and bubbles in water-based two-component road marking paint, improves the density and wear resistance of the coating film, and enhances adhesion and construction quality.
Patent Information
- Application Number
- CN202611555575.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing water-based two-component road marking paints tend to agglomerate and clump in aqueous media, exhibiting poor compatibility, low cross-linking density, and difficulty in removing air bubbles, leading to brittle and peeling coatings and insufficient abrasion resistance.
A water-based carboxyl-containing hydroxy acrylic dispersion and water-dispersible polyether-modified HDI trimer are used as components A and B. A three-dimensional network cross-linked structure is formed through the nucleophilic addition reaction of hydroxyl groups and isocyanate groups. With the use of film-forming aids, wetting agents, defoamers and leveling agents, dispersibility and bubble removal are improved, and the density and adhesion of the coating film are enhanced.
It improves the density and wear resistance of the coating film, reduces cracking, enhances the smoothness and adhesion of the coating during application, and shortens the time before traffic can resume.
Smart Images

Figure CN123107516A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of coating manufacturing technology, specifically to a high-gloss, wear-resistant, water-based two-component road marking coating and its preparation method. Background Technology
[0002] Current road marking paints are gradually moving towards water-based formulations. Conventional single-component water-based paints, limited by their thermoplastic film-forming mechanism, lack a chemical cross-linking network between molecular chains, resulting in a loose internal film structure. This often leads to insufficient adhesion and abrasion resistance for heavy-traffic roads. To improve physical and mechanical properties, the industry has experimented with compounding hydroxyl-containing resins with isocyanate curing agents to form two-component reactive water-based road marking paints. However, conventional isocyanate curing agents have strong hydrophobicity, making homogeneous dispersion difficult in deionized water media, easily leading to agglomeration and poor compatibility after mixing the two components. Uneven local cross-linking density reduces the final film density, making the paint film prone to brittle cracking and peeling under vehicle loads.
[0003] Conventional water-based two-component systems face the challenge of difficult-to-eliminate air bubbles during formulation and application. Mechanical stirring introduces a large amount of air into the mixture, and the internal stress of coating systems that have not undergone polymer structure modification and lack a reasonable induction period cannot be relaxed in time, causing air bubbles to remain inside the cured film. Microscopic pinhole defects present after film formation reduce the overall wear resistance and surface smoothness of the coating. In addition, conventional systems lack an internal catalytic mechanism, resulting in a slow addition reaction rate at room temperature, which delays the opening of road markings to traffic. Existing formulations cannot simultaneously achieve a balance between resin dispersion stability, curing crosslinking density, and coating mechanical toughness in an aqueous environment. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a high-gloss, wear-resistant water-based two-component road marking paint and its preparation method. It solves the problems that conventional isocyanate curing agents tend to agglomerate and clump in aqueous media, resulting in poor system compatibility and low crosslinking density. Additionally, bubbles generated during the mixing stage are difficult to expel and form microscopic pinholes inside the paint film, ultimately leading to the paint film being prone to brittle cracking and peeling under vehicle loads and insufficient wear resistance.
[0005] To achieve the above objectives, the present invention provides the following technical solution: In a first aspect, the present invention provides a high-gloss, wear-resistant, water-based two-component road marking paint, employing the following technical solution: A high-gloss, wear-resistant, water-based two-component road marking paint, comprising separately packaged component A and component B; Component A comprises the following raw materials in parts by weight: 60.0 to 90.0 parts of aqueous carboxyl-containing hydroxy acrylic acid dispersion, 10.0 to 30.0 parts of deionized water, 2.0 to 6.0 parts of film-forming aid, 0.1 to 0.5 parts of wetting agent, 0.1 to 0.6 parts of defoamer, and 0.1 to 0.5 parts of leveling agent; Component B comprises the following components in parts by weight: 10.0 to 30.0 parts of water-dispersible polyether-modified HDI trimer.
[0006] By adopting the above technical solution, using an aqueous carboxyl-containing hydroxy acrylic dispersion as the main resin and a water-dispersible polyether-modified HDI trimer as the curing agent, a dense coating with excellent wear resistance and environmental safety is achieved. In the specific reaction and film-forming process, the hydroxy acrylic dispersion in component A, due to its carboxyl structure, can spontaneously disperse in deionized water when mixed with component B, which has been modified with polyether to introduce hydrophilic segments, thanks to its nonionic surface activity. This characteristic facilitates the formation of a homogeneous system after mixing the two components, thus improving the tendency of unmodified isocyanate to agglomerate in the aqueous phase. During water evaporation, the hydroxyl groups on the resin segments of component A undergo nucleophilic addition reactions with the isocyanate groups in component B, thereby generating urethane bonds. Since this crosslinking process can occur at room temperature or under heating conditions, a relatively dense three-dimensional network polymer structure is formed after curing, providing the coating with basic mechanical strength. In addition, the free carboxyl groups in component A have a certain internal catalytic effect on the formation of urethane bonds, which helps to improve the curing rate; the polar carboxyl groups can also form hydrogen bonds with the active sites on the surface of the road substrate, further improving the adhesion and wear resistance of the coating.
[0007] Preferably, the aqueous carboxyl-containing hydroxy acrylic acid dispersion has a solid content of 40 to 45%, a hydroxyl value of 80 to 120 mg KOH / g, and an acid value of 15 to 25 mg KOH / g; The aqueous carboxyl-containing hydroxy acrylic dispersion is made from a mixture of monomers comprising the following parts by weight: 30.0 to 35.2 parts of methyl methacrylate, 35.0 to 40.0 parts of butyl acrylate, 15.5 to 30.6 parts of hydroxyethyl methacrylate, and 2.0 to 4.2 parts of methacrylic acid.
[0008] By employing the above technical solutions, methyl methacrylate is mainly used to construct the rigidity and wear resistance base of the coating film, while butyl acrylate can provide a certain degree of flexibility to the macromolecular chains, thus mitigating the tendency of the coating film to crack under road loads. Hydroxyethyl methacrylate introduces hydroxyl crosslinking sites that can participate in the reaction. Controlling the hydroxyl value at 80 to 120 mg KOH / g is to retain sufficient crosslinking sites during the reaction with component B, thereby helping to build the crosslinked network after curing. Controlling the acid value at 15 to 25 mg KOH / g and the specific ratio of methacrylic acid are mainly to balance the electrostatic repulsion stability of the dispersion in the aqueous phase, while avoiding excessively high acid values that would reduce the water resistance of the coating film. The reasonable combination of monomer types and proportions helps to achieve a relative physical balance between the hardness and flexibility of the final paint film.
[0009] Preferably, the water-dispersible polyether-modified HDI trimer is prepared by reacting raw materials comprising the following parts by weight: 100.0 parts of hexamethylene diisocyanate trimer and 2.5 to 20.0 parts of monomethyl etherified polyethylene glycol with a number average molecular weight of 400 to 600. The water-dispersible polyether-modified HDI trimer has an -NCO mass fraction of 17.0 to 21.0%.
[0010] By employing the above technical solution, monomethyl etherified polyethylene glycol with a number-average molecular weight of 400 to 600 can introduce nonionic hydrophilic polyether segments into the hydrophobic HDI trimer molecular backbone through the reaction of terminal hydroxyl groups with some isocyanate groups of the hexamethylene diisocyanate trimer. The specific molecular weight range of the polyether and its dosage ratio can impart a certain hydrophilic-lipophilic balance property to component B without significantly reducing the water resistance of the coating film, making it easy to form a small dispersed particle size and maintain dispersion stability in aqueous systems. Controlling the mass fraction of isocyanate groups retained after the reaction to 17.0% to 21.0% aims to retain an appropriate amount of reactive groups to support the overall crosslinking degree after the two-component system is cured.
[0011] Preferably, the film-forming aid is dipropylene glycol methyl ether; The wetting agent is a polyether-modified siloxane wetting agent; The defoamer is an organosilicone defoamer; The leveling agent is a polyether-modified polydimethylsiloxane leveling agent.
[0012] By adopting the above technical solution, dipropylene glycol methyl ether, with its suitable evaporation rate and resin compatibility, helps promote the melt-plastic deformation and continuous film formation of polymer particles in the later stages of water evaporation. The polyether-modified siloxane wetting agent mainly reduces the surface tension of the system, thereby improving the penetration and coating ability of the marking paint on rough road substrates. The silicone defoamer in the formulation, combined with shear dispersion and the application process, can promote the rupture of most microbubbles, reducing microscopic defects inside the cured coating; the polyether-modified polydimethylsiloxane leveling agent is responsible for improving the surface tension gradient of the wet film and reducing brush marks on the surface. The various additives produce a synergistic effect, which is beneficial to improving the application tolerance and appearance smoothness of the coating system.
[0013] Secondly, the present invention provides a method for preparing a high-gloss, wear-resistant, water-based two-component road marking paint, employing the following technical solution: A method for preparing a high-gloss, wear-resistant, water-based two-component road marking paint includes the following steps: A water-based carboxyl-containing hydroxy acrylic dispersion was mixed with deionized water and stirred. Film-forming aid, wetting agent, defoamer, and leveling agent were added dropwise in sequence under stirring and dispersed at high speed. The mixture was then filtered to obtain component A. Water-dispersible polyether-modified HDI trimer is provided as component B; Mix component A and component B according to the specified ratio, stir evenly, and let stand to mature to obtain a high-gloss, wear-resistant, water-based two-component road marking paint.
[0014] By adopting the above technical solution, the process flow is rationally designed, and the physical and chemical processes between each step are interconnected, which helps to prepare coatings with excellent comprehensive performance. In actual operation, by pre-mixing the water-based main resin and deionized water, the rheological state of the system can be initially adjusted, providing a homogeneous medium environment for the subsequent addition of additives. The four additives for film formation, wetting, defoaming, and leveling are added slowly and sequentially under mechanical stirring. Combined with the shear stress applied by high-speed dispersion, this facilitates the dispersion of microscopic molecular clusters of the additives in the aqueous phase. The hydrodynamic shearing action promotes the uniform adsorption of additive molecules on the surface of polymer particles and in the dispersion medium. The subsequent filtration step is mainly used to intercept undispersed large particulate impurities to maintain the physical homogeneity of component A during long-term storage. Before application, the two components are mixed in proportion, and a corresponding static curing stage is set as the induction period. During this period, component B spontaneously emulsifies in the aqueous phase using its own hydrophilic segments, and the two components interpenetrate at the microscopic scale. The dissolved air bubbles inside the system can be partially expelled, and at the same time, the hydroxyl groups and isocyanate groups undergo a preliminary nucleophilic addition reaction, which promotes a moderate increase in the viscosity of the system and establishes a thixotropic structure, laying a physical foundation for the subsequent coating film formation and smoothness.
[0015] Preferably, in the mixing and stirring of the aqueous carboxyl-containing hydroxy acrylic acid dispersion with deionized water, the mixing and stirring speed is 300-700 r / min, and the mixing and stirring time is 5-15 min; In high-speed dispersion, the stirring speed is 800-1200 r / min, and the high-speed dispersion time is 10-30 min. In the filtration process, the filter screen used for filtration is 200 mesh.
[0016] By adopting the above technical solution, the gradient rotation speed and time design takes into account both the requirements of material mixing and fine dispersion. The low-to-medium speed range is mainly used to achieve macroscopic homogenization of the base liquid while reducing material splashing; the high speed range imparts higher shear force to the fluid to promote the dispersion of additive particles. A reasonable dispersion time setting can generally reduce the risk of resin demulsification or gelation caused by excessive shearing and heat generation. A 200-mesh filter can trap particles larger than 75 micrometers, basically meeting the fineness requirements of road marking paint spraying operations and reducing the probability of clogging the application nozzles.
[0017] Preferably, before mixing and stirring the aqueous carboxyl-containing hydroxyacrylic acid dispersion with deionized water, the aqueous carboxyl-containing hydroxyacrylic acid dispersion is prepared in advance. The steps for preparing the aqueous carboxyl-containing hydroxyacrylic acid dispersion include: Nitrogen gas was introduced into 25.0 parts of dipropylene glycol methyl ether solvent and the temperature was raised to 85-90°C. A monomer mixture containing methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, and methacrylic acid was mixed and dissolved with 1.2 to 2.0 parts of azobisisobutyronitrile initiator and added dropwise at a uniform rate for 3-4 hours. The heat preservation time is 1 hour, then 0.2 parts of azobisisobutyronitrile initiator are added, and the heat preservation time is continued for 2 hours. Cool to 60°C and slowly add 1.6 to 3.9 parts of N,N-dimethylethanolamine, achieving a neutralization degree of 80 to 90%. Phase inversion dispersion was carried out by slowly adding 103.0 to 111.0 parts of deionized water at a shear rate of 800 r / min to obtain an aqueous hydroxy acrylic acid dispersion containing carboxyl groups.
[0018] By employing the above technical solution, the dispersion is prepared through a combination of free radical solution polymerization and phase inversion. During the early stages of polymerization and the monomer addition process, nitrogen is continuously introduced to purge oxygen from the reactor, aiming to reduce the inhibitory effect of oxygen on free radical polymerization. Uniformly adding the monomer mixture keeps the instantaneous monomer concentration in the system at a low level, which helps to mitigate the exothermic reaction and promotes a uniform polymer molecular weight distribution. After the main reaction is completed, the system is kept at a constant temperature, and a small amount of initiator is added to further polymerize the remaining monomers, aiming to further improve the monomer conversion rate and reduce the volatile organic compound residue in the resin product.
[0019] Subsequently, N,N-dimethylethanolamine was introduced as a weak base neutralizing agent, which neutralized the free carboxyl groups on the polymer chain to form a hydrophilic quaternary ammonium salt structure. The set degree of neutralization maintained the balance between the hydrophilicity and water resistance of the polymer chain. After neutralization, deionized water was added dropwise to the system under continuous shear. As the amount of water increased, the system gradually underwent a reversal from a water-in-oil state to an oil-in-water state, eventually forming a uniformly dispersed aqueous polymer dispersion.
[0020] Preferably, before providing the water-dispersible polyether-modified HDI trimer as component B, the water-dispersible polyether-modified HDI trimer is prepared in advance. The steps for preparing the water-dispersible polyether-modified HDI trimer include: In a dry nitrogen-protected reactor, the hexamethylene diisocyanate trimer was heated to 70–80°C, and monomethyl etherified polyethylene glycol was slowly added dropwise. 0.02 to 0.04 parts of dibutyltin dilaurate were added as a catalyst, and the reaction was maintained at 70–80°C for 2–3 hours. The mixture was then cooled and discharged to obtain a water-dispersible polyether-modified HDI trimer.
[0021] By employing the above technical solution, the dry nitrogen environment isolates external moisture, helping to reduce losses caused by side reactions of highly reactive isocyanate groups upon contact with moisture. Since the reaction is catalyzed by dibutyltin dilaurate, the activation energy of the addition reaction between the terminal hydroxyl groups of monomethyl etherified polyethylene glycol and the isocyanate groups can be effectively reduced. Controlling the synthesis temperature within the range of 70 to 80°C takes into account both the reaction conversion rate and, to a certain extent, suppresses the spontaneous formation of byproducts such as urea diketone or isocyanurate from isocyanates at high temperatures. This ensures the relatively precise structure of the introduced hydrophilic polyether segments, maintaining the dispersibility and reactivity of the crosslinking agent.
[0022] Preferably, in the mixing of component A and component B, the mass ratio of component A to component B is 72.3–127.6:10.0–30.0; During the mixing process, the stirring speed is 300-500 r / min at room temperature, and the mixing time is 3-10 min. During the static aging process, the aging time is 10–20 minutes.
[0023] By adopting the above technical solution, a specific mixing ratio range is set to define the effective molar ratio of resin hydroxyl groups to curing agent isocyanate groups, which is beneficial for establishing a relatively dense curing crosslinking network. Low to medium speed stirring combined with short stirring time relies mainly on the surface activity of the modified HDI trimer for gentle dispersion, reducing the risk of excessive mechanical stirring introducing large amounts of air into the system or accelerating the reaction due to frictional heat. The subsequent settling time provides the system with some time to relax internal stress, allowing air bubbles trapped in the mixture to rise and dissipate, thereby improving the density of the paint film during coating and reducing pinholes.
[0024] Preferably, after obtaining the high-gloss, wear-resistant, water-based two-component road marking paint, the high-gloss, wear-resistant, water-based two-component road marking paint is directly sprayed or brushed onto the surface of the substrate and cross-linked and cured into a film at room temperature or under heating conditions.
[0025] By adopting the above technical solution, the curing and crosslinking conditions are highly adaptable. After the coating is sprayed or brushed onto the road surface, as the moisture evaporates, the reaction sites between the polymer chains gradually move closer, triggering a network crosslinking reaction at room temperature and promoting surface drying. During the curing process, polar groups generate chemical anchoring and hydrogen bonding on the surface of the asphalt or concrete substrate, which helps to form a wear-resistant coating that is tightly bonded to the road substrate.
[0026] This invention provides a high-gloss, wear-resistant water-based two-component road marking paint and its preparation method. It has the following beneficial effects: 1. This invention utilizes an aqueous carboxyl-containing hydroxy acrylic dispersion combined with a water-dispersible polyether-modified HDI trimer. The hydroxyl groups in the resin undergo a nucleophilic addition reaction with the isocyanate groups in the curing agent to generate urethane bonds and construct a three-dimensional network cross-linked structure, which imparts mechanical strength and wear resistance to the coating. At the same time, the free carboxyl groups carried by the dispersion play an internal catalytic role in the cross-linking process and can form hydrogen bonds with the surface of the road substrate, increasing the adhesion of the coating film.
[0027] 2. This invention adjusts the rigidity and flexibility of the polymer macromolecular chain by controlling the ratio of methyl methacrylate to butyl acrylate in an aqueous carboxyl-containing hydroxy acrylic dispersion, thereby mitigating the phenomenon of brittle cracking of the coating under load. In conjunction with the monomethyl etherification of hexamethylene diisocyanate trimer with polyethylene glycol, nonionic hydrophilic segments are introduced into the molecular backbone to improve the dispersion state of isocyanate in deionized water medium, reduce agglomeration and clumping problems, and improve the compatibility and film density of the two components after mixing.
[0028] 3. This invention employs mixing and stirring at different speeds and high-speed dispersion during the preparation stage, combined with the sequential addition of film-forming aids, wetting agents, defoamers, and leveling agents. The fluid dynamics shearing action promotes the dispersion and adsorption of the aids in the aqueous medium. A static curing step is set after the two components are mixed to provide the system with internal stress relaxation time, allowing air bubbles entrained in the mixture to float and be expelled, reducing microscopic defects inside the paint film and improving the smoothness of the coating film. Attached Figure Description
[0029] Figure 1 This is a schematic diagram of the infrared spectrum of the curing agent of the present invention; Figure 2 This is a schematic diagram of the differential scanning calorimetry temperature rise curve of the present invention; Figure 3 This is a schematic diagram showing the evolution of the viscosity of the coating after mixing over time according to the present invention. Figure 4 This is a schematic diagram illustrating the evolution trend of cumulative wear of the coating in this invention. Detailed Implementation
[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0031] Preparation Example 1: This preparation example provides a method for preparing an aqueous carboxyl-containing hydroxy acrylic dispersion, including the following steps: In a four-necked flask equipped with a stirrer, condenser, thermometer, and dropping funnel, 25.0 parts of dipropylene glycol methyl ether solvent were added, and the mixture was purged with nitrogen and heated to 85°C. A monomer mixture (containing 30.0 parts methyl methacrylate, 35.0 parts butyl acrylate, 15.5 parts hydroxyethyl methacrylate, and 2.0 parts methacrylic acid) was mixed with 1.2 parts of azobisisobutyronitrile initiator and dissolved thoroughly. At 85°C, the mixture was added dropwise to the reaction flask at a uniform rate over a period of 3 hours. After the addition was complete, the mixture was kept at this temperature for 1 hour; then, 0.2 parts of azobisisobutyronitrile initiator were added, and the mixture was kept at this temperature for another 2 hours. The system was then cooled to 60°C, and 1.6 parts of N,N-dimethylethanolamine were slowly added, maintaining a neutralization degree of 80%. After stirring for 30 minutes, 103.0 parts of deionized water were slowly added dropwise at a shear rate of 800 r / min to carry out phase inversion dispersion, and finally a transparent to slightly bluish aqueous hydroxy acrylic dispersion containing carboxyl groups was obtained with a solid content of 40%, a hydroxyl value of 80 mg KOH / g, and an acid value of 15 mg KOH / g.
[0032] Preparation Example 2: This preparation example provides a method for preparing an aqueous carboxyl-containing hydroxy acrylic dispersion, including the following steps: In a four-necked flask equipped with a stirrer, condenser, thermometer, and dropping funnel, 25.0 parts of dipropylene glycol methyl ether solvent were added, and the mixture was purged with nitrogen and heated to 85°C. A monomer mixture (containing 35.0 parts methyl methacrylate, 40.0 parts butyl acrylate, 23.6 parts hydroxyethyl methacrylate, and 3.1 parts methacrylic acid) was mixed with 1.5 parts of azobisisobutyronitrile (AIBN) initiator and dissolved thoroughly. At 85°C, the mixture was added dropwise to the reaction flask at a uniform rate over 3.5 hours. After the addition was complete, the mixture was kept at this temperature for 1 hour; then 0.2 parts of AIBN initiator were added, and the mixture was kept at this temperature for another 2 hours. The system was then cooled to 60°C, and 2.7 parts of N,N-dimethylethanolamine were slowly added, maintaining a neutralization degree of 85%. After stirring for 30 minutes, 111.0 parts of deionized water were slowly added dropwise at a shear rate of 800 r / min to carry out phase inversion dispersion, and finally a transparent to slightly bluish aqueous hydroxy acrylic dispersion containing carboxyl groups was obtained with a solid content of 42%, a hydroxyl value of 100 mg KOH / g, and an acid value of 20 mg KOH / g.
[0033] Preparation Example 3: This preparation example provides a method for preparing an aqueous carboxyl-containing hydroxy acrylic dispersion, including the following steps: In a four-necked flask equipped with a stirrer, condenser, thermometer, and dropping funnel, 25.0 parts of dipropylene glycol methyl ether solvent were added, and the mixture was purged with nitrogen and heated to 90°C. A monomer mixture (containing 35.2 parts methyl methacrylate, 40.0 parts butyl acrylate, 30.6 parts hydroxyethyl methacrylate, and 4.2 parts methacrylic acid) was mixed with 2.0 parts of azobisisobutyronitrile initiator and dissolved thoroughly. At 90°C, the mixture was added dropwise to the reaction flask at a uniform rate over a period of 4 hours. After the addition was complete, the mixture was kept at this temperature for 1 hour; then 0.2 parts of azobisisobutyronitrile initiator were added, and the mixture was kept at this temperature for another 2 hours. The system was then cooled to 60°C, and 3.9 parts of N,N-dimethylethanolamine were slowly added, maintaining a neutralization degree of 90%. After stirring for 30 minutes, 103.3 parts of deionized water were slowly added dropwise at a shear rate of 800 r / min to carry out phase inversion dispersion, and finally a transparent to slightly bluish aqueous hydroxy acrylic dispersion containing carboxyl groups was obtained with a solid content of 45%, a hydroxyl value of 120 mg KOH / g, and an acid value of 25 mg KOH / g.
[0034] Preparation Example 4: This preparation example provides a method for preparing a water-dispersible polyether-modified HDI trimer, including the following steps: In a dry, nitrogen-protected reactor, 100.0 parts of hexamethylene diisocyanate trimer (NCO mass fraction 21.8%) were added, and the temperature was raised to 70°C. 2.5 parts of monomethyl etherified polyethylene glycol with a number-average molecular weight of 400 were slowly added dropwise. 0.02 parts of dibutyltin dilaurate were added as a catalyst, and the reaction was maintained at 70°C for 2 hours. The -NCO content was determined by di-n-butylamine back titration at regular intervals. When the -NCO mass fraction decreased to 21.0% and remained stable, the mixture was cooled and discharged to obtain a water-dispersible polyether-modified HDI trimer with nonionic surfactant properties.
[0035] Preparation Example 5: This preparation example provides a method for preparing a water-dispersible polyether-modified HDI trimer, including the following steps: In a dry nitrogen-protected reactor, 100.0 parts of hexamethylene diisocyanate trimer (NCO mass fraction of 21.8%) were added, and the temperature was raised to 75°C. 10.2 parts of monomethyl etherified polyethylene glycol with a number-average molecular weight of 500 were slowly added dropwise. 0.03 parts of dibutyltin dilaurate were added as a catalyst, and the reaction was maintained at 75°C for 2.5 h. The -NCO content was determined by di-n-butylamine back titration at regular intervals. When the -NCO mass fraction decreased to 19.0% and remained stable, the mixture was cooled and discharged to obtain a water-dispersible polyether-modified HDI trimer with nonionic surfactant properties.
[0036] Preparation Example 6: This preparation example provides a method for preparing a water-dispersible polyether-modified HDI trimer, including the following steps: In a dry nitrogen-protected reactor, 100.0 parts of hexamethylene diisocyanate trimer (NCO mass fraction of 21.8%) were added, and the temperature was raised to 80℃. 20.0 parts of monomethyl etherified polyethylene glycol with a number-average molecular weight of 600 were slowly added dropwise. 0.04 parts of dibutyltin dilaurate were added as a catalyst, and the reaction was maintained at 80℃ for 3 hours. The -NCO content was determined by di-n-butylamine back titration at regular intervals. When the -NCO mass fraction decreased to 17.0% and remained stable, the mixture was cooled and discharged to obtain a water-dispersible polyether-modified HDI trimer with nonionic surfactant properties.
[0037] Example 1: This embodiment provides a method for preparing a high-gloss, wear-resistant, water-based two-component road marking paint, including the following steps: (1) Preparation of component A: In a dispersion vessel equipped with a stirring device, 75.0 parts of the aqueous carboxyl-containing hydroxy acrylic dispersion prepared in Preparation Example 2 and 20.0 parts of deionized water were added sequentially. The stirring was started and the speed was set to 500 r / min for 10 min. Then, under stirring, 4.0 parts of dipropylene glycol methyl ether film-forming aid, 0.3 parts of polyether modified siloxane wetting agent, 0.4 parts of organosilicon defoamer and 0.3 parts of polyether modified polydimethylsiloxane leveling agent were added dropwise. After the addition was completed, the stirring speed was increased to 1000 r / min and high-speed dispersion was continued for 20 min. Then, the material was filtered through a 200-mesh filter to obtain a uniform and stable component A.
[0038] (2) Preparation of component B: The water-dispersible polyether modified HDI trimer prepared in Preparation Example 5 was directly used as curing agent component B.
[0039] (3) Formulation and film formation of the two-component coating: Before construction, the above-mentioned component A and component B are mixed at a mass ratio of 100.0:20.0. Stir at 400 r / min for 5 min at room temperature to make it uniformly mixed; let it stand for 15 min to eliminate air bubbles in the system, and a high-gloss, wear-resistant water-based two-component road marking coating is obtained. This coating can be directly sprayed or brushed onto the surface of the substrate and crosslinked and cured into a film at room temperature or under heating conditions.
[0040] Example 2: This embodiment provides a method for preparing a high-gloss, wear-resistant, water-based two-component road marking paint, including the following steps: (1) Preparation of component A: In a dispersion vessel equipped with a stirring device, 60.0 parts of the aqueous carboxyl-containing hydroxy acrylic dispersion prepared in Preparation Example 1 and 10.0 parts of deionized water were added in sequence. The stirring was started and the speed was set to 300 r / min for 5 min. Then, under stirring, 2.0 parts of dipropylene glycol methyl ether film-forming aid, 0.1 parts of polyether modified siloxane wetting agent, 0.1 parts of organosilicon defoamer and 0.1 parts of polyether modified polydimethylsiloxane leveling agent were slowly added dropwise. After the addition was completed, the stirring speed was increased to 800 r / min and high-speed dispersion was continued for 10 min. Then, the material was filtered through a 200-mesh filter to obtain a uniform and stable component A.
[0041] (2) Preparation of component B: The water-dispersible polyether modified HDI trimer prepared in Preparation Example 4 was directly used as curing agent component B.
[0042] (3) Formulation and film formation of the two-component coating: Before construction, the above-mentioned component A and component B are mixed at a mass ratio of 72.3:10.0. Stir at 300 r / min for 3 min at room temperature to make it uniformly mixed; let it stand for 10 min to eliminate air bubbles in the system, and a high-gloss, wear-resistant water-based two-component road marking coating is obtained. This coating can be directly sprayed or brushed onto the surface of the substrate and crosslinked and cured into a film at room temperature or under heating conditions.
[0043] Example 3: This embodiment provides a method for preparing a high-gloss, wear-resistant, water-based two-component road marking paint, including the following steps: (1) Preparation of component A: In a dispersion vessel equipped with a stirring device, 90.0 parts of the aqueous carboxyl-containing hydroxy acrylic dispersion prepared in Preparation Example 3 and 30.0 parts of deionized water were added sequentially. The stirring was started and the speed was set to 700 r / min for 15 min. Then, under stirring, 6.0 parts of dipropylene glycol methyl ether film-forming aid, 0.5 parts of polyether modified siloxane wetting agent, 0.6 parts of organosilicon defoamer and 0.5 parts of polyether modified polydimethylsiloxane leveling agent were added dropwise sequentially. After the addition was completed, the stirring speed was increased to 1200 r / min and high-speed dispersion was continued for 30 min. Then, the material was filtered through a 200-mesh filter to obtain a uniform and stable component A.
[0044] (2) Preparation of component B: The water-dispersible polyether modified HDI trimer prepared in Preparation Example 6 was directly used as curing agent component B.
[0045] (3) Formulation and film formation of the two-component coating: Before construction, the above-mentioned component A and component B are mixed at a mass ratio of 127.6:30.0. Stir at 500 r / min for 10 min at room temperature to make it uniformly mixed; let it stand for 20 min to eliminate air bubbles in the system, and a high-gloss, wear-resistant water-based two-component road marking coating is obtained. This coating can be directly sprayed or brushed onto the surface of the substrate and crosslinked and cured into a film at room temperature or under heating conditions.
[0046] Comparative Example 1: Compared with Example 1, the difference is that in step (2), an equal amount of unmodified hexamethylene diisocyanate trimer is used instead of the water-dispersible polyether modified HDI trimer prepared in Example 5, while the rest are the same.
[0047] Comparative Example 2: The difference from Example 1 is that the preparation formula of component A lacks the dormant AZC catalyst, while the rest are the same.
[0048] Comparative Example 3: Compared with Example 1, the difference is that the neutralization system in the preparation process of component A adopts a monoamine system (lacking the fast-drying ammonia water compound component), while the rest are the same.
[0049] Comparative Example 4: Compared with Example 1, the difference is that the neutralization system in the preparation process of component A uses a monoamine system (lacking the AMP-95 multifunctional amine with steric hindrance effect), while the rest are the same.
[0050] Comparative Example 5: Compared with Example 1, the difference is that in the preparation of component B, no chemical reaction modification process was used. Instead, the unmodified hexamethylene diisocyanate trimer was directly mixed with an equal amount of monomethyl etherified polyethylene glycol in a conventional physical blend as curing agent component B. All other aspects are the same.
[0051] Comparative Example 6: The difference from Example 1 is that incorrect thermodynamic parameters were used in the preparation of component B (water-dispersible polyether modified HDI trimer), which abnormally increased the modification reaction temperature from 75°C to 110°C. All other parameters are the same.
[0052] Test Example 1: Unmodified hexamethylene diisocyanate trimer, component B prepared in Example 1, component B prepared in Comparative Example 5, and component B prepared in Comparative Example 6 were selected as targets for infrared spectroscopy scanning.
[0053] Each of the above test samples was uniformly coated onto the clean, dried potassium bromide salt window surface. The same amount of coating was used, and the liquid film thickness of each test sample was controlled to be consistent using a spacer with a fixed thickness. After removing air bubbles from the liquid film, another potassium bromide salt window was used to cover and clamp the sample to form a uniform liquid film, thus obtaining a test sample for infrared transmission mode.
[0054] Fourier transform infrared spectroscopy was used to scan and test each sample at 25℃, with the spectral scanning range set to 4000 cm⁻¹. -1 Up to 500cm -1 The instrument resolution was adjusted to 4cm. -1 Each individual sample underwent a total of 32 scans to reduce the impact of background noise.
[0055] After acquiring the raw spectral data, baseline correction was performed. The peak positions and corresponding transmittance values of isocyanate groups, urethane NH stretching vibrations, and ether bonds within their respective characteristic wavenumber ranges were extracted and recorded. The transmittance data of each sample were semi-quantitatively compared under the same sample preparation conditions and test parameters.
[0056] Table 1. Wavenumber and transmittance test data of infrared absorption peaks of characteristic groups of each component B
[0057] Note: The “-” in the table indicates that the characteristic absorption peak of the corresponding group could not be detected under the current test conditions, therefore there is no corresponding transmittance data.
[0058] Figure 1 The Fourier transform infrared spectra of each test object are superimposed spectra after baseline correction and longitudinal shift processing. In the figure, the black solid line represents the unmodified HDI trimer, the dark gray solid line represents component B of Example 1, the gray dashed line represents component B of Comparative Example 5, and the dark gray dotted dashed line represents component B of Comparative Example 6.
[0059] According to the data in Table 1, the unmodified HDI trimer was at 2271.4 cm⁻¹. -1 An isocyanate group absorption peak was present nearby, but no characteristic absorption peaks attributable to the NH stretching vibration of urethane and the COC stretching vibration of polyether were detected under the test conditions.
[0060] Conclusion: Component B of Example 1 was at 1108.5 cm. -1 The characteristic peak of monomethyl etherified polyethylene glycol ether bond appears at 3324.1 cm⁻¹. -1 Absorption signals attributable to the NH stretching vibration of urethane were detected in the region. Considering that the stretching vibration of the hydroxyl groups at the polyether terminus will produce overlapping absorptions in similar wavenumber regions, this peak is not used as the sole criterion for determining the formation of urethane. Under the same sample preparation and testing conditions, the transmittance at the measured isocyanate group characteristic peak increased from 12.3% to 34.6%, indicating a decrease in the corresponding characteristic absorption. Combined with the appearance of ether bond characteristic absorption and the formation of urethane NH-related absorption signals, the test results support the reaction between the active groups at the polyether terminus and the isocyanate groups in the HDI trimer, indicating that the nonionic polyether segments are introduced into the curing agent structure through chemical bonding, providing a structural basis for the subsequent dispersion of the resin in the aqueous system.
[0061] Comparative Example 5 employed a physical blending process, superimposing the ether bond signal of polyethylene glycol into the spectral data. However, no characteristic absorption changes corresponding to those in Example 1 and attributed to the newly generated urethane NH were observed. The transmittance of the isocyanate characteristic peak in this sample was similar to that of the unmodified control group, indicating that the isocyanate groups were not substantially consumed under these test conditions. No clear evidence of a chemical reaction between monomethyl etherified polyethylene glycol and HDI trimer was observed, suggesting that the polyether component mainly existed in a physically blended state. Due to the lack of stable covalent bonds between the polyether segments and the HDI trimer, there was a certain degree of migration or phase separation tendency during subsequent aqueous dispersion and film formation.
[0062] Comparative Example 6, using a higher modification reaction temperature, showed an increase in the transmittance of its isocyanate characteristic peak to 86.4%, with a significant decrease in the corresponding characteristic absorption, indicating that the free isocyanate groups in the system were consumed to some extent. Considering the general trend of side reactions occurring in isocyanate systems at higher temperatures, it is speculated that the higher reaction temperature, in addition to promoting the target reaction, further triggers the reaction between the already formed urethane structure and the remaining isocyanate groups, accompanied by the formation of side reaction structures such as urea carbamate. This additional consumption of free isocyanate groups reduces the effective active sites for crosslinking during subsequent curing, leading to a decrease in the overall degree of crosslinking in the system and adversely affecting the subsequent formation of a dense three-dimensional crosslinked network.
[0063] Test Example 2: Two-component resin matrices corresponding to Examples 1 to 3 and Comparative Examples 1, 2, and 5, without the addition of pigments and acetone-insoluble inorganic fillers, were uniformly coated onto a flat polytetrafluoroethylene (PTFE) plate, with the wet film thickness controlled to be approximately 200 μm. The coated samples were then cured for 7 days under constant temperature and humidity conditions of 25°C and 50% relative humidity. After curing, the coating was carefully peeled off from the substrate to obtain free coating samples.
[0064] Regular fragments weighing approximately 0.5 g were cut from each of the above-mentioned free coating films, and their initial mass was accurately weighed using an analytical balance with an accuracy of 0.1 mg. The weighed coating fragments were then wrapped in a pre-weighed 300-mesh stainless steel mesh, sealed tightly, and completely immersed in an Erlenmeyer flask containing sufficient acetone solvent. The flask was left to soak at room temperature for 48 hours, with gentle shaking periodically during this time. After soaking, the mesh package was removed and dried in a 60°C vacuum drying oven until constant weight. The remaining mass after extraction was weighed. The gelation rate of the system was obtained by calculating the percentage of the insoluble polymer component after extraction relative to the initial polymer sample mass.
[0065] A trace sample of 5-8 mg was taken from the same batch of free coating film, spread evenly in a standard aluminum crucible, and pressed and sealed. Differential scanning calorimetry (DSC) was used for thermal analysis at a dynamic high-purity nitrogen atmosphere flow rate of 50 mL / min. The first heating program was set to heat from -20℃ to 150℃ at a heating rate of 10℃ / min. The heat flow curve during the first heating process was recorded. The glass transition temperature of the coating film after 7 days of curing was determined by the midpoint of the baseline step change. Simultaneously, the presence of residual curing exothermic signals was observed during the heating process. After the first heating, the sample was cooled to -20℃ at the same rate and then heated again to 150℃ at 10℃ / min. The glass transition temperature obtained from the second heating was used to characterize the thermal properties of the material after eliminating the effects of thermal history and post-curing, and was not used as the primary evaluation criterion for the original degree of curing after 7 days at 25℃.
[0066] Table 2. Test data on gelation rate and glass transition temperature of coatings for each system.
[0067] Figure 2 This is a differential scanning calorimetry (DSC) curve of the first temperature rise of the cross-linked and cured coatings of each system of the present invention. The solid black line represents the test curve of Example 1, the solid dark gray line represents the test curve of Example 2, the dashed gray line represents the test curve of Comparative Example 1, and the dotted dark gray line represents the test curve of Comparative Example 2.
[0068] According to the data in Table 2, the gelation rate of the coatings in Examples 1 to 3 remained above 91%, corresponding to glass transition temperatures in the range of 59°C to 65°C. These test results show that the system formed a high proportion of solvent-insoluble network structures, significantly restricting polymer chain movement and exhibiting a high degree of network crosslinking characteristics. In two-component waterborne polyurethane curing systems, the crosslinking network structure and effective crosslinking degree are often factors affecting the wear resistance and solvent resistance of the macroscopic coating. Based on the technical approach of this study, the partial hydrophilic modification of hexamethylene diisocyanate trimer using monomethyl etherified polyethylene glycol helps improve the dispersion uniformity and interfacial compatibility of the curing agent in waterborne carboxyl-containing hydroxyl acrylic dispersions. A good dispersion state increases the effective contact probability between isocyanate groups and resin hydroxyl groups. Combined with the effect of specific crosslinking promoting components, this is beneficial for improving the effective network formation degree of the system, thereby reducing the probability of side reactions of free isocyanate groups. During the film-forming stage as moisture gradually evaporates, the reactive groups retained from the hydrophilic modification continue to undergo urethane crosslinking with the resin hydroxyl groups, gradually constructing a network framework that restricts chain segment movement. This process is macroscopically manifested as a high gelation rate and glass transition temperature. Figure 2 No obvious residual exothermic signal was observed in the corresponding high-temperature section, indicating that the system reaction was relatively complete.
[0069] In comparison, the gel rates of Comparative Example 1 and Comparative Example 5 decreased to 76.22% and 71.53%, respectively, and their glass transition temperatures were also at a low level of 41.5℃ and 38.8℃. This decline in test data reflects the relatively insufficient proportion of solvent-insoluble networks formed by the two groups of samples. Tracing their formulation composition, Comparative Example 1 directly used an unmodified curing agent, which, due to its low hydrophilicity, resulted in poor dispersion and interfacial compatibility in the aqueous resin system, hindering uniform contact between reactive groups. Although Comparative Example 5 physically added polyethylene glycol, the free polyether was prone to migration or redistribution in the aqueous system, making it difficult to provide stable hydrophilic protection for the curing agent interface.
[0070] In the initial stages of actual construction, the aforementioned dispersion and compatibility issues can increase the risk of competitive side reactions between isocyanate groups and water molecules, with some reactive groups transforming into urea structures and escaping with carbon dioxide. The consumption of effective crosslinking nodes leads to the elution of more components not connected to the main network during acetone extraction, and the decrease in the degree of crosslinking also reduces the degree of restriction on chain segment movement, which is consistent with the characteristics of a lower gelation rate and glass transition temperature.
[0071] Further observation of Comparative Example 2, which did not contain the specific cross-linking promoting component, revealed a gelation rate of 82.71% and a glass transition temperature of 47.9℃. These lower values indicate that the system's efficiency in constructing an effective network structure was reduced under room temperature curing conditions. Combined with... Figure 2 The heating curves of Comparative Example 2 and Comparative Example 1 show a certain degree of exothermic broad peak in the high-temperature region after the glass transition. This complementary experimental phenomenon suggests that some unreacted active groups in the system undergo secondary curing and crosslinking after heating. As the moisture inside the coating gradually evaporates over time and the viscosity of the system continues to increase, the diffusion ability of polymer segments and active groups is gradually restricted. This hindered diffusion limits the effective collision of the remaining reactive groups in the later stages, leading to a gradual slowdown in the crosslinking rate. This restriction in later network formation not only increases the proportion of extractable free components but also confirms that the system is difficult to achieve the ideal degree of curing under conditions lacking crosslinking-promoting components. This will have a certain adverse effect on the mechanical strength and wear resistance of the final coating.
[0072] Test Example 3: Two-component waterborne coatings prepared in Examples 1 to 3, and Comparative Examples 1, 2, and 5 were mixed in a constant temperature and humidity laboratory at 25°C and 50% relative humidity. The curing agent component was added to the main agent according to the specified ratio, and the mixture was continuously stirred at 800 rpm for 3 minutes using a laboratory multi-functional mixer equipped with a dispersion disc of the same size to ensure uniform mixing and obtain the liquid coating to be tested. All tests used the same dispersion disc size, loading amount, and stirring position.
[0073] Immediately after mixing, the coating was poured into a 250mL standard test beaker. The moment mixing ended was taken as the starting point for the pot life. The initial apparent viscosity was measured using a rotational viscometer under the same temperature, rotor, and rotation speed conditions. Subsequently, the viscosity of the sample in the beaker was measured every 15 minutes until the coating viscosity reached twice the initial viscosity or obvious gel stringing occurred. When two adjacent viscosity measurement points exceeded twice the initial viscosity, linear interpolation was performed based on the viscosity and time data of the two adjacent measurement points to determine the time corresponding to the viscosity reaching twice the initial value. The sample state was continuously observed between two viscosity measurements; if obvious gel stringing occurred earlier, its actual occurrence time was recorded. The earlier of reaching twice the initial viscosity or the occurrence of obvious gel stringing was taken as the pot life of the coating. The sample beaker was covered during the test to prevent excessive moisture evaporation.
[0074] Using a bar coater, a wet film of approximately 200 μm thickness was prepared on a clean tinplate test plate by applying freshly mixed liquid coating. The sample was placed horizontally in the same constant temperature and humidity environment, and the dryness of the coating surface was checked at fixed time intervals using the finger touch method. Near the end of the surface drying period, the check interval was controlled to 1 minute. The surface drying time was recorded as the time from the completion of coating to the first time the coating was reached when a finger touched the coating surface with a basically consistent light touch without leaving fingerprints or feeling sticky.
[0075] Based on the surface dryness test, continue to observe the sample. Press the coating surface with your thumb using basically consistent pressure and rotate it 90°. If the coating surface is undamaged, without obvious indentations, and the underlying layer does not slip relative to the surface, the coating is considered to have reached the fully dry state. Record the time when the above criteria are first met as the fully dry time.
[0076] Table 3. Test data on the application performance and film-forming drying time of two-component coatings for each system.
[0077] Figure 3 This is a graph showing the continuous change in viscosity over time after mixing the two-component coatings of each system in this invention. The solid black line represents the viscosity evolution curve of Example 1, the solid dark gray line represents the viscosity evolution curve of Example 2, the dashed gray line represents the viscosity evolution curve of Comparative Example 1, and the dotted dark gray line represents the viscosity evolution curve of Comparative Example 2.
[0078] According to the data in Table 3, the initial viscosity of the mixtures in Examples 1 to 3 remained at a low level of 148.9 to 162.3 mPa·s, with a pot life of 128 to 142 min, and the surface drying and hard drying times controlled within 31 min and 3.7 h, respectively. In the actual application of road marking paints, the pot life and film drying speed of the mixed paint are usually mutually restrictive. Sufficient operating time is needed on-site to prevent equipment blockage, while a fast film drying speed is also required after spraying to facilitate the rapid restoration of road use. The systems in the examples can balance a long operating window with rapid curing characteristics. This result is consistent with the improved dispersion uniformity and interfacial compatibility of the curing agent modified with monomethyl etherified polyethylene glycol in the waterborne resin system. This stable dispersion state is beneficial for maintaining a low initial apparent viscosity and a stable application condition.
[0079] Combination Figure 3 The evolution of the rheological curves shows that the viscosity increase in the example is extremely gradual over a relatively long period during the initial mixing stage. In the liquid aqueous state, the high water content and relatively dispersed state of the reactants reduce the tendency for rapid formation of a highly cross-linked network, thus maintaining a relatively stable viscosity change within the operating window after mixing. Simultaneously, the presence of the cross-linking promoting component supports the accelerated formation of the subsequent network structure. When the liquid coating is applied to the substrate surface, the solid content of the system gradually increases with the rapid evaporation of water molecules. This significantly increases the effective contact opportunities between resin hydroxyl groups, isocyanate groups, and related cross-linking components, accelerating the network formation process and resulting in shorter surface drying and actual drying times.
[0080] Comparative Example 1, using unmodified hexamethylene diisocyanate trimer, exhibited an initial viscosity as high as 312.5 mPa·s and a significantly reduced pot life of 58 min. This phenomenon indicates that the unmodified trimer has relatively insufficient dispersion compatibility with aqueous resin systems, easily leading to localized aggregation or decreased interfacial compatibility, which in turn affects its high initial viscosity and... Figure 3The relatively rapid upward trend shown by the curve throughout corresponds to this. In actual coating, poor dispersion increases the probability of competitive side reactions between isocyanate groups and water, as well as localized non-uniform reactions, thereby consuming some effective reactive groups and causing the system viscosity to rise too quickly, significantly shortening the effective application window. These factors also reduce the proportion of isocyanate groups that can be effectively crosslinked with the resin hydroxyl groups, affecting the uniform and dense formation of the subsequent network structure. This is consistent with the test result of Comparative Example 1, where the drying time was extended to 6.1 hours, indicating that its film-forming drying efficiency was significantly lower than that of the example. Although Comparative Example 5 incorporated hydrophilic polyether through physical mixing, its initial viscosity decreased compared to Comparative Example 1, but its pot life and drying time still did not reach the ideal state. It is speculated that the reason is that the physically blended polyether segments lack chemical bond anchoring, resulting in migration or redistribution in the aqueous system, leading to relatively insufficient stability of its hydrophilic modification effect on the curing agent interface. This instability of the interface state is not conducive to maintaining uniform dispersion of the system in the long term, thus resulting in a shorter pot life and extended surface drying and drying times.
[0081] Comparative Example 2, without the specific crosslinking promoter, exhibited different performance evolution characteristics. It had a pot life of up to 184 minutes, with the corresponding viscosity curve remaining at extremely low levels for a considerable period, but the final surface drying time and complete drying time were extended to 82 minutes and 8.5 hours, respectively. Without the crosslinking promoter, the rate of effective network structure formation decreased, resulting in a relatively slow viscosity increase in the liquid phase, but also significantly prolonging the subsequent film drying time. Especially as the coating moisture gradually evaporated and the overall viscosity of the system increased, the migration and diffusion capabilities of polymer segments and active groups gradually decreased. In an environment with insufficient crosslinking promotion, the probability of collisions between effective reactive groups and the network formation process were further limited. In practical road construction applications, this prolonged surface undried state increases the risk of dust contamination or early external disturbances to the coating, which is detrimental to improving the rapid film formation efficiency and ensuring project quality after marking construction.
[0082] Test Example 4: Two-component water-based coatings prepared in Examples 1 to 3 and Comparative Examples 1, 2, and 5 were mixed in a constant temperature and humidity laboratory at 25°C and 50% relative humidity. The uniformly mixed liquid coatings were evenly applied to standard cement substrates and tinplate using a wire bar coater, controlling the wet film thickness to approximately 400 μm. After curing, the dry film thickness of each group of samples was measured to confirm that the coating thicknesses for abrasion comparison were within a similar range. Immediately after coating, coated glass microspheres with a refractive index of 1.50, a particle size range of 150–850 μm, and a silane coupling agent surface treatment were uniformly sprinkled onto the wet film surface of the cement substrate. The amount of microspheres sprinkled was uniformly controlled at 350 g / m² for each group. 2 Each group used the same specifications, the same amount of material, and the same spreading method, allowing the glass microspheres to embed naturally in the wet film without any artificial adjustment to the final embedding depth. All samples were then placed horizontally in a constant temperature and humidity environment for 7 days of curing.
[0083] After curing the coating on the cement substrate under the aforementioned constant temperature and humidity conditions for 7 days, its initial retroreflectance luminance coefficient was determined using a retroreflectometer. During measurement, the instrument was placed close to the coating surface, avoiding edges and areas with obvious defects. The observation angle was set to 1.05° and the incident angle to 88.76°. All test samples were subjected to the same measurement geometry. Five different locations were randomly selected from each sample for measurement. The arithmetic mean of the data was calculated to characterize the initial retroreflectance performance of the system after film formation.
[0084] A coating sample without glass microspheres, cured for 7 days on a tinplate under the same conditions, was cut into circular specimens with a diameter of 100 mm and a central hole diameter of 6.5 mm and fixed on the test platform of a rotary abrasion tester. A CS-17 abrasion wheel was used, and a total test load of 500 g was applied to each wheel for abrasion testing. Before each group of tests, the CS-17 abrasion wheels were pretreated or surface-trimmed using the same method, and the condition of the abrasion wheels, dust collection conditions, and the test environment were kept consistent to reduce the impact of changes in the condition of the abrasion wheels on the test results.
[0085] After the instrument has been running for 1000 revolutions, the sample is removed. Loose abrasion debris on the sample surface is removed using a consistent cleaning method used by all groups, while avoiding additional coating peeling caused by the cleaning process itself. The purging air pressure is controlled at 0.4 MPa, the nozzle distance from the sample is 10 cm, and the purging time is 10 s. The mass of the sample before and after wear is accurately weighed using an analytical balance, and the mass loss is calculated as the basis for evaluating the wear resistance performance of the coating.
[0086] Table 4. Test data of initial retroreflective brightness coefficient and wear rate of coatings for each system
[0087] Figure 4 This is a continuous evolution trend graph showing the cumulative wear amount of the coatings in each system of the present invention as a function of wear revolutions. The solid black line represents the test curve of Example 1, the solid dark gray line represents the test curve of Example 2, the dashed gray line represents the test curve of Comparative Example 1, and the dotted dark gray line represents the test curve of Comparative Example 2.
[0088] According to the data in Table 4, the initial retroreflective luminance coefficients of the coatings in Examples 1 to 3 were 338.2–351.9 mcd·m. -2 ·lx -1 The mass loss after 1000 revolutions was 19.8–23.1 mg, exhibiting a high initial retroreflective level and low wear. The initial retroreflective performance of road markings largely depends on the distribution of glass microspheres on the coating surface and their effective exposure ratio. Simultaneously, the wetting and coating state of the coating on the glass microspheres and the network structure after film formation affect the stable retention of the microspheres in the coating. The system in the examples, due to the introduction of a monomethyl etherified polyethylene glycol modified curing agent and specific crosslinking promoting components, is beneficial to improving the dispersion uniformity of the curing agent in the aqueous resin system and promoting the formation of an effective network structure during film formation. The aforementioned better dispersion and network formation state helps maintain the uniformity of the coating surface structure and facilitates the formation of suitable glass microsphere embedding and exposure states; at the same time, sufficient network formation is beneficial to improving the coating's resistance to mechanical wear. In the continuous friction test under rotating abrasive wheels, the sufficiently formed polymer network is beneficial to improving the overall structural stability of the coating, which is consistent with the low wear mass loss results of the examples. In actual road traffic environments, good wear resistance and high initial retroreflectivity can provide favorable conditions for the markings to maintain good reflectivity in the future. However, their long-term retroreflectivity retention performance still needs to be further evaluated by combining retroreflectivity after wear, wheel load, or long-term aging tests.
[0089] Comparative observation of the test results of Comparative Example 1 and Comparative Example 5 reveals that the initial system compatibility and curing characteristics indicate that the unmodified or only physically blended curing agents have insufficient dispersion adaptability in aqueous environments. This result corresponds to the higher abrasion amount and lower initial retroreflective brightness coefficient in this test, indicating that the final film-forming overall performance is lower than that of the example system. Uneven dispersion will cause inconsistent effective network formation in different areas, thereby reducing the uniformity of the overall coating structure and surface state, and adversely affecting the wetting and coating state of the glass microspheres by the resin. Under external force, a weaker network structure will reduce the coating's ability to resist continuous mechanical abrasion, and will also be detrimental to the stable retention of glass microspheres in the coating. These factors are consistent with the lower initial retroreflective brightness coefficient and higher abrasion mass loss results of Comparative Example 1 and Comparative Example 5.
[0090] As shown in Table 4, at the endpoint of the 1000 rpm abrasion test, the mass loss of Comparative Example 2 was 37.2 mg, significantly higher than the 19.8–23.1 mg of Examples 1 to 3. Combined with the relatively lower gelation rate and glass transition temperature of Comparative Example 2 in Test Example 2, it can be concluded that under the same curing conditions, its effective network formation degree was lower than that of the Example system. This result is consistent with the higher abrasion amount in this test. A lower effective network formation degree means that the polymer chain segments are relatively less constrained, thereby reducing the coating's ability to resist continuous mechanical abrasion. The lower initial retroreflective brightness coefficient of Comparative Example 2 indicates that the final formed microspheres and the optical state of the coating surface are weaker than those of the Examples. This difference is related to factors such as the effective exposure ratio of glass microspheres, the wetting and coating state, and the coating surface structure, but the specific reason cannot be uniquely determined based solely on this test. This relatively lower network formation degree reduces the coating's ability to resist continuous mechanical abrasion, consistent with the higher mass loss result of Comparative Example 2 at 1000 rpm. This also indicates that introducing a suitable crosslinking promoting component into the waterborne two-component coating system of the present invention is beneficial to improving the effective network formation degree and wear resistance of the final coating film.
Claims
1. A high-gloss, wear-resistant, water-based two-component road marking paint, characterized in that, It contains separately packaged components A and B; Component A comprises the following raw materials in parts by weight: 60.0 to 90.0 parts of aqueous carboxyl-containing hydroxy acrylic acid dispersion, 10.0 to 30.0 parts of deionized water, 2.0 to 6.0 parts of film-forming aid, 0.1 to 0.5 parts of wetting agent, 0.1 to 0.6 parts of defoamer, and 0.1 to 0.5 parts of leveling agent; Component B comprises the following components in parts by weight: 10.0 to 30.0 parts of water-dispersible polyether-modified HDI trimer.
2. The high-gloss, wear-resistant, water-based, two-component road marking paint according to claim 1, characterized in that, The aqueous carboxyl-containing hydroxy acrylic acid dispersion has a solid content of 40 to 45%, a hydroxyl value of 80 to 120 mg KOH / g, and an acid value of 15 to 25 mg KOH / g. The aqueous carboxyl-containing hydroxy acrylic dispersion is made from a mixture of monomers comprising the following parts by weight: 30.0 to 35.2 parts of methyl methacrylate, 35.0 to 40.0 parts of butyl acrylate, 15.5 to 30.6 parts of hydroxyethyl methacrylate, and 2.0 to 4.2 parts of methacrylic acid.
3. The high-gloss, wear-resistant, water-based two-component road marking paint according to claim 1, characterized in that, The water-dispersible polyether-modified HDI trimer is prepared by reacting the following raw materials in parts by weight: 100.0 parts of hexamethylene diisocyanate trimer and 2.5 to 20.0 parts of monomethyl etherified polyethylene glycol with a number average molecular weight of 400 to 600. The water-dispersible polyether-modified HDI trimer has an -NCO mass fraction of 17.0 to 21.0%.
4. The high-gloss, wear-resistant, water-based two-component road marking paint according to claim 1, characterized in that, The film-forming aid is dipropylene glycol methyl ether; The wetting agent is a polyether-modified siloxane wetting agent; The defoamer is an organosilicone defoamer; The leveling agent is a polyether-modified polydimethylsiloxane leveling agent.
5. A method for preparing a high-gloss, wear-resistant, water-based two-component road marking paint according to any one of claims 1-4, characterized in that, Includes the following steps: The aqueous carboxyl-containing hydroxy acrylic dispersion is mixed and stirred with deionized water. Under stirring, the film-forming aid, the wetting agent, the defoamer, and the leveling agent are added dropwise in sequence for high-speed dispersion. The mixture is then filtered to obtain component A. The water-dispersible polyether-modified HDI trimer is provided as component B; The components A and B are mixed in the specified ratio, stirred evenly, and allowed to stand for curing to obtain the high-gloss, wear-resistant, water-based two-component road marking paint.
6. The preparation method according to claim 5, characterized in that, In the process of mixing and stirring the aqueous carboxyl-containing hydroxy acrylic acid dispersion with the deionized water, the stirring speed is 300-700 r / min and the stirring time is 5-15 min. In high-speed dispersion, the stirring speed is 800-1200 r / min, and the high-speed dispersion time is 10-30 min. In the filtration process, the filter screen used for filtration is 200 mesh.
7. The preparation method according to claim 5, characterized in that, Before mixing and stirring the aqueous carboxyl-containing hydroxyacrylic acid dispersion with the deionized water, the aqueous carboxyl-containing hydroxyacrylic acid dispersion is prepared in advance. The steps for preparing the aqueous carboxyl-containing hydroxyacrylic acid dispersion include: Nitrogen gas was introduced into 25.0 parts of dipropylene glycol methyl ether solvent and the temperature was raised to 85-90°C. The monomer mixture (containing methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, and methacrylic acid) was mixed and dissolved evenly with 1.2 to 2.0 parts of azobisisobutyronitrile initiator. The mixture was then added dropwise at a uniform rate for 3-4 hours. The heat preservation time is 1 hour, then 0.2 parts of azobisisobutyronitrile initiator are added, and the heat preservation time is continued for 2 hours. Cool to 60°C and slowly add 1.6 to 3.9 parts of N,N-dimethylethanolamine, achieving a neutralization degree of 80 to 90%. Phase inversion dispersion was carried out by slowly adding 103.0 to 111.0 parts of deionized water at a shear rate of 800 r / min to obtain the aqueous carboxyl-containing hydroxy acrylic dispersion.
8. The preparation method according to claim 5, characterized in that, Before providing the water-dispersible polyether-modified HDI trimer as component B, the water-dispersible polyether-modified HDI trimer is prepared in advance. The steps for preparing the water-dispersible polyether-modified HDI trimer include: In a dry nitrogen-protected reactor, the hexamethylene diisocyanate trimer is heated to 70–80°C, and monomethyl etherified polyethylene glycol is slowly added dropwise. 0.02 to 0.04 parts of dibutyltin dilaurate are added as a catalyst, and the reaction is maintained at 70–80°C for 2–3 hours. The mixture is then cooled and discharged to obtain the water-dispersible polyether-modified HDI trimer.
9. The preparation method according to claim 5, characterized in that, In the mixing of component A and component B in a specified ratio, the mass ratio of component A to component B is 72.3–127.6:10.0–30.
0. During the mixing process, the stirring speed is 300-500 r / min at room temperature, and the mixing time is 3-10 min. During the static aging process, the aging time is 10–20 minutes.
10. The preparation method according to claim 5, characterized in that, After obtaining the high-gloss, wear-resistant, water-based two-component road marking paint, the high-gloss, wear-resistant, water-based two-component road marking paint is directly sprayed or brushed onto the surface of the substrate and crosslinked and cured into a film at room temperature or under heating conditions.